Method and device for refining aluminum alloy for precision casting

By using a smelting furnace with thermal insulation layer and heat collector in aluminum alloy manufacturing, combined with the refining technology of permanent magnet stirrer and high-pressure nozzle, the problem of insufficient conductivity, thermal conductivity and corrosion resistance in aluminum alloy manufacturing is solved. , improves casting density and performance while reducing the risk of workers being exposed to irritating odors.

CN118910453AInactive Publication Date: 2024-11-08ANHUI SOLID FOUNDRY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410794332.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the manufacturing process of traditional aluminum alloys, there are problems such as weak conductivity, thermal conductivity and corrosion resistance, and pores and oxidation debris are generated, which affects the performance of the castings and poses a hazard to workers.

Method used

Using a smelting furnace with insulation layer and heat collector, combined with the first and second permanent magnet stirrers, refining with powdered composite refining agent and inert gas, adding refining agent and spraying purification through high-pressure nozzles to reduce slag inclusion And increase casting density.

Benefits of technology

Improve the insulation effect and energy efficiency of the smelting furnace, refine raw material particles, optimize smelting effect, reduce slag inclusion in aluminum melt, improve the density and pinhole of the casting, enhance the casting performance, and reduce the workers' exposure to irritating odors risks in.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910453A_ABST
    Figure CN118910453A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of metal smelting, and particularly discloses an aluminum alloy refining method and device for precision castings. Step 2, smelting; step 3, slagging off; step 4, sampling and component adjustment; 5, converter treatment; step 6, refining; step 7, slagging off for the second time; step 8, casting; a high-pressure nozzle is arranged to add a powdery refining agent, a guide pipe is arranged to introduce inert gas, during refining, a second permanent magnet stirrer acts to stir a melt in a refining furnace to enhance the mixed reaction of the refining agent and the melt, the refining agent and the inert gas act at the same time, and the composite refining agent can reduce part of inclusions into aluminum; and a refining agent is added for compounding use while blowing purification is carried out, so that slag inclusion in the aluminum melt can be reduced, the density of the aluminum melt can be increased, and the pinhole degree grade of a casting can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal smelting, and in particular to a method and device for refining aluminum alloy for precision castings. Background Art

[0002] Cast aluminum alloys are widely used in aerospace, automobile, machinery, electronics and other fields due to their low density, high specific strength, good plasticity, good electrical and thermal conductivity, good corrosion resistance, rich resources and easy processing. However, cast aluminum alloys may cause a series of defects in castings during the smelting process, such as pinholes, pores, slag inclusions, etc. Therefore, how to improve the smelting quality has always been a problem that needs to be considered in the actual production of castings. The inclusions in the smelting of cast aluminum alloys are mainly hydrogen and aluminum oxide, which can be removed through appropriate refining processes. Therefore, the refining process of cast aluminum alloys in the smelting process is the key link. If the refining process is improper, the continuity and density of aluminum castings will be destroyed, which will inevitably reduce the performance of the castings. There are many methods for refining aluminum alloys, which can be generally divided into two categories: one is the adsorption method; the other is the non-adsorption method. The non-adsorption method is less used in actual casting production and focuses on laboratory research. The adsorption method includes two categories: medium filtration method and flotation method. The flotation method is the most widely used because it is simple to operate and will not cause the harm of flux slag inclusion.

[0003] Refining agents are mostly used in the traditional aluminum alloy manufacturing process, which will result in the finished product having poor electrical conductivity, thermal conductivity and corrosion resistance. In addition, the alloy castings produced have high porosity, many pores will appear on the casting surface, and the proportion of oxidized impurities is also high, affecting the performance of the alloy castings. The products of the refining process have a pungent odor, which is extremely harmful to the health of workers. Summary of the invention

[0004] The present invention provides a method and device for refining aluminum alloy for precision castings to solve the problems raised in the above background technology.

[0005] To achieve the above object, the present invention provides the following technical solution: A method for refining aluminum alloy for precision castings, comprising:

[0006] Step 1: batching and charging the furnace. The batched raw materials are batched according to the composition of the aluminum alloy to be produced, and the batched raw materials are placed in the melting furnace;

[0007] Step 2: Melting: Turn on the heating system of the melting furnace to heat the raw materials to a working temperature of 630-700°C, so that the ingredients are in a liquid melt;

[0008] Step 3: Slag removal, remove the large amount of oxide slag floating on the surface of the melt;

[0009] Step 4: Sampling and adjusting composition. Sampling is performed for analysis before the furnace. When the composition does not meet the standard requirements, the melt is supplemented or diluted according to the sampling analysis results.

[0010] Step 5: Converter, which guides the melt in the smelting furnace into the refining furnace;

[0011] Step 6: Refining: let the melt stand and adjust the temperature of the melt to 730-810°C, add the refining agent under stirring conditions, and introduce inert gas into the refining furnace at the same time. The refining time is 35-45 minutes;

[0012] Step 7: Secondary slag removal, removing the waste slag produced after refining in the refining furnace;

[0013] Step 8: Casting, extract the alloy solution for casting processing.

[0014] Preferably, after heating for a period of time in step 1, the ingredients are fully stirred after becoming liquid.

[0015] Preferably, the refining agent added in step six is ​​a powdery composite refining agent, and the ingredients of the refining agent are: sodium chloride, potassium chloride, magnesium chloride, sodium fluorosilicate, sodium fluoroaluminate, calcium fluoride, sodium carbonate, refractory clay and other small amounts of additives.

[0016] Preferably, the standing time in step six is ​​30 minutes.

[0017] Preferably, the inert gas in step six is ​​argon.

[0018] An aluminum alloy refining device for precision castings comprises a smelting furnace and a refining furnace, wherein a heat preservation layer is arranged inside the smelting furnace, a base is arranged on the lower side of the smelting furnace, a first permanent magnetic stirrer is arranged at the lower end of the smelting furnace in the middle of the base, a heat collecting device is installed at the bottom end of the smelting furnace, a lifter is arranged at the top of the smelting furnace, a driving motor is arranged on one side of the lifter and is installed at the top of the smelting furnace, the driving motor is connected to the lifter through a shaft sleeve, a lifting rod is arranged on the lifter, a filter plate is connected to the lower end of the lifting rod, sliding frames are arranged on both sides of the interior of the smelting furnace, and the filter plate is slidably connected to the sliding frame The bottom end of one side of the smelting furnace is connected to the refining furnace through a pipeline; a regulating valve is arranged in the middle of the pipeline, horizontal plates are arranged on both sides of the refining furnace, a jack is arranged at the lower end of the horizontal plate, two vertical plates are fixedly arranged on both sides of the lower end of the refining furnace, a second permanent magnetic agitator is fixedly arranged between the two vertical plates, a sealing sleeve is arranged at the top center of the refining furnace, a conduit is installed in the sealing sleeve, an injection structure is arranged at the bottom end of the conduit and inserted into the melt, the inner center of the conduit is an air vent, an air outlet is penetrated on the injection structure to connect the air vent, an outlet pipe is arranged on one side of the refining furnace, and an electromagnetic valve is arranged on the outlet pipe.

[0019] Preferably, the first permanent magnetic stirrer and the second permanent magnetic stirrer are configured the same, and the permanent magnetic stirrer includes a permanent magnetic inductor, which is fixed on the rotating shaft of the motor and is an even number of permanent magnets spaced apart in the circumferential direction, and adjacent permanent magnets have opposite polarities.

[0020] Preferably, the heat collecting device is a disc-type heat collecting tube, which further reduces the heat loss in the furnace cavity and improves the heat preservation and energy-saving effects of the smelting furnace.

[0021] Preferably, a high-pressure nozzle is provided at the upper end of the refining furnace, the high-pressure nozzle is connected to an inlet pipe, the inlet pipe is used to input the refining agent, and a solenoid valve is provided on the inlet pipe.

[0022] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention improves the thermal insulation effect of the smelting furnace by arranging a smelting furnace with a thermal insulation layer, and at the same time, a heat collecting device is arranged inside the smelting furnace to reduce the heat loss in the furnace chamber, save energy consumption, and arrange a first permanent magnetic stirrer to refine the raw material particles, increase the melting speed, and optimize the smelting effect; the present invention arranges a high-pressure nozzle to add a powdered refining agent, and arranges a conduit to introduce an inert gas. During refining, the second permanent magnetic stirrer stirs the melt in the refining furnace to strengthen the mixing reaction of the refining agent and the melt. The refining agent and the inert gas act simultaneously, and the composite refining agent can reduce a part of the inclusions to aluminum. The refining agent is added for composite use while being sprayed for purification, which can not only reduce the slag inclusions in the aluminum melt, but also increase the density of the aluminum melt and improve the pinhole degree grade of the casting. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a schematic diagram of the overall structure of the present invention.

[0024] In the figure: 1, smelting furnace; 2, insulation layer; 3, base; 4, first permanent magnetic stirrer; 5, heat collecting device; 6, sliding frame; 7, filter plate; 8, driving motor; 9, lifting rod; 10, lifter; 11, pipeline; 12, regulating valve; 13, refining furnace; 14, cross plate; 15, jack; 16, sealing sleeve; 17, conduit; 171, vent hole; 172, air outlet; 18, inlet pipe; 19, high-pressure nozzle; 20, outlet pipe; 21, second permanent magnetic stirrer. DETAILED DESCRIPTION

[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] In the description of the present invention, it should be noted that the terms "vertical", "up", "down", "horizontal", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.

[0027] In the description of the present invention, it is also necessary to explain that, unless otherwise clearly specified and limited, the terms "set", "install", "connect", and "connect" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0028] See also Figure 1 The present invention provides a technical solution: a method for refining aluminum alloy for precision castings, comprising:

[0029] Step 1: batching and charging the furnace, batching the raw materials according to the composition of the aluminum alloy to be produced, and placing the batched raw materials into the smelting furnace 1;

[0030] Step 2: Melting: Turn on the heating system of the melting furnace 1 to heat the raw materials to a working temperature of 630-700° C., so that the ingredients are in a liquid melt;

[0031] Step 3: Slag removal, remove the large amount of oxide slag floating on the surface of the melt;

[0032] Step 4: Sampling and adjusting composition. Sampling is performed for analysis before the furnace. When the composition does not meet the standard requirements, the melt is supplemented or diluted according to the sampling analysis results.

[0033] Step 5: Converter, introducing the melt smelted in the smelting furnace 1 into the refining furnace 13;

[0034] Step 6: refining, the melt is allowed to stand and the temperature of the melt is adjusted to 730-810° C., a refining agent is added under stirring, and an inert gas is introduced into the refining furnace 13 at the same time, and the refining time is 35-45 minutes;

[0035] Step 7: Secondary slag removal, removing the waste slag produced after refining in the refining furnace 13;

[0036] Step 8: Casting, extract the alloy solution for casting processing.

[0037] Furthermore, after heating for a period of time in step 1, the ingredients are fully stirred after becoming liquid.

[0038] Furthermore, the refining agent added in step six is ​​a powdered composite refining agent, and the components of the refining agent are: sodium chloride, potassium chloride, magnesium chloride, sodium fluorosilicate, sodium fluoroaluminate, calcium fluoride, sodium carbonate, refractory clay and other small amounts of additives. The role of chloride is due to its small surface tension and strong wetting effect on Al2O3. It is also the main component of the flux. The melting point of the NaCl-KCl system in the eutectic composition is about 660°C. It has a low melting point and low surface tension and is the basis of most fluxes. Fluoride is an important component of the flux, which is characterized by a relatively high melting point and low hygroscopicity. The decomposition products reduce the wettability of the interface between solid alumina and aluminum melt, making it easy to separate from aluminum and promote the drying of the slag. Carbonates decompose in the aluminum melt to release CO2. The bubbles remove hydrogen during the rising process and increase the temperature during the effective action time to improve the diffusion conditions of inclusions to the flux.

[0039] Furthermore, the standing time in step six is ​​30 minutes.

[0040] Furthermore, the inert gas in step six is ​​argon.

[0041] A precision casting aluminum alloy refining device comprises a smelting furnace 1 and a refining furnace 13, wherein the smelting furnace 1 is provided with a heat preservation layer 2 inside, a base 3 is provided on the lower side of the smelting furnace 1, a first permanent magnetic stirrer 4 is provided at the lower end of the smelting furnace 1 in the middle of the base 3, a heat collecting device 5 is installed at the bottom end of the smelting furnace 1, a lifter 10 is provided at the top of the smelting furnace 1, a driving motor 8 is provided on one side of the lifter 10 and is installed at the top of the smelting furnace 1, the driving motor 8 is connected to the lifter 10 through a shaft sleeve, a lifting rod 9 is provided on the lifter 10, a filter plate 7 is connected to the lower end of the lifting rod 9, the filter plate 7 moves up and down through the lifting rod 9, and the waste slag at the upper end of the liquid surface is coarsely filtered to reduce the labor intensity of the workers, and sliding racks 6 are provided on both sides of the interior of the smelting furnace 1, and the filter plate 7 Slidingly connected with the sliding frame 6, the bottom end of one side of the smelting furnace 1 is connected to the refining furnace 13 through the pipeline 11; a regulating valve 12 is arranged in the middle of the pipeline 11, and horizontal plates 14 are arranged on both sides of the refining furnace 13, and a jack 15 is arranged at the lower end of the horizontal plate 14. Two vertical plates are fixedly arranged on both sides of the lower end of the refining furnace 13, and a second permanent magnetic stirrer 21 is fixedly arranged between the two vertical plates. A sealing sleeve 16 is arranged at the top center of the refining furnace 13, and a conduit 17 is installed in the sealing sleeve 16. The bottom end of the conduit 17 is provided with an injection structure inserted into the melt, and the inner center of the conduit 17 is a vent 171, and an air outlet 172 is penetrated on the injection structure to connect the vent 171. An outlet pipe 20 is arranged on one side of the refining furnace 13, and an electromagnetic valve is arranged on the outlet pipe 20.

[0042] Furthermore, the first permanent magnetic agitator 4 and the second permanent magnetic agitator 21 are configured the same, and the permanent magnetic agitator includes a permanent magnetic inductor, which is fixed on the rotating shaft of the motor. It is an even number of permanent magnets distributed at intervals in the circumferential direction, and the polarities of adjacent permanent magnets are opposite. The permanent magnetic agitator stirs evenly and refines the grains to achieve the best smelting effect without direct contact to avoid pollution. The first permanent magnetic agitator 4 is used to increase the melting rate of the raw materials in the smelting furnace 1, and the second permanent magnetic agitator 21 is used to evenly mix the refining agent into the melt.

[0043] Furthermore, the heat collecting device 5 is a disc-type heat collecting tube, which further reduces the heat loss in the furnace cavity and improves the heat preservation and energy-saving effects of the smelting furnace 1.

[0044] Furthermore, a high-pressure nozzle 19 is provided at the upper end of the refining furnace 13 , and the high-pressure nozzle 19 is connected to an inlet pipe 18 , and the inlet pipe 18 is used to input the refining agent, and a solenoid valve is provided on the inlet pipe 18 .

[0045] Working principle: The present invention provides a method and device for refining aluminum alloy for precision castings. When used specifically, the aluminum alloy method for precision castings is used for processing in the device. First, the ingredients are added into the smelting furnace 1, and the first permanent magnetic stirrer 4 is turned on to heat the ingredients. After sufficient stirring, slag is removed. The slag removal can first start the drive motor 8 to perform coarse filtration through the filter plate 7, and then the slag is removed manually. After completion, the melt is introduced into the refining furnace 13, and the melt is composite-refined inside the refining furnace 13. After completion, the casting work can be carried out. In particular, the refining furnace 13 is fixed on the jack 15 by a cross plate 14, and the refining furnace 13 can be transferred and dumped by a forklift; the present invention provides a smelting furnace 1 with a thermal insulation layer 2. The heat preservation effect of the high smelting furnace 1 is improved. At the same time, a heat collecting device 5 is arranged inside the smelting furnace 1 to reduce the heat loss in the furnace cavity and save energy. A first permanent magnetic stirrer 4 is arranged to refine the raw material particles, increase the melting speed and optimize the smelting effect. The present invention provides a high-pressure nozzle 19 to add a powdered refining agent, and a conduit 17 is arranged to introduce an inert gas. During refining, the second permanent magnetic stirrer 21 stirs the melt in the refining furnace 13 to strengthen the mixing reaction of the refining agent and the melt. The refining agent and the inert gas act at the same time. The composite refining agent can reduce a part of the inclusions to aluminum. The refining agent is added for composite use while being sprayed for purification, which can not only reduce the slag inclusions in the aluminum melt, but also increase the density of the aluminum melt and improve the pinhole degree of the casting.

[0046] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for refining aluminum alloy for precision castings, characterized in that: include: Step 1: batching and charging the furnace, batching the raw materials according to the composition of the aluminum alloy to be produced, and placing the batched raw materials into the smelting furnace (1); Step 2: Melting: Turn on the heating system of the melting furnace (1) to heat the raw materials to a working temperature of 630-700° C., so that the ingredients are in a liquid melt; Step 3: Slag removal, remove the large amount of oxide slag floating on the surface of the melt; Step 4: Sampling and adjusting composition. Sampling is performed for analysis before the furnace. When the composition does not meet the standard requirements, the melt is supplemented or diluted according to the sampling analysis results. Step 5: Converter, introducing the melt smelted in the smelting furnace (1) into the refining furnace (13); Step 6: refining, the melt is allowed to stand and the temperature of the melt is adjusted to 730-810° C., a refining agent is added under stirring, and an inert gas is introduced into the refining furnace (13) for 35-45 minutes; Step 7: Secondary slag removal, removing the waste slag produced after refining in the refining furnace (13); Step 8: Casting, extract the alloy solution for casting processing.

2. The method for refining aluminum alloy for precision castings according to claim 1, characterized in that: After heating for a period of time in step 1, the ingredients are fully stirred after becoming liquid.

3. The method for refining aluminum alloy for precision castings according to claim 1, characterized in that: The refining agent added in step six is ​​a powdery composite refining agent, and the ingredients of the refining agent are: sodium chloride, potassium chloride, magnesium chloride, sodium fluorosilicate, sodium fluoroaluminate, calcium fluoride, sodium carbonate, refractory clay and other small amounts of additives.

4. The method for refining aluminum alloy for precision castings according to claim 1, characterized in that: The standing time in step 6 is 30 minutes.

5. The method for refining aluminum alloy for precision castings according to claim 1, characterized in that: The inert gas in step six is ​​argon.

6. An aluminum alloy refining device for precision castings, characterized in that: The invention comprises a smelting furnace (1) and a refining furnace (13), wherein a heat-insulating layer (2) is arranged inside the smelting furnace (1), a base (3) is arranged on the lower side of the smelting furnace (1), a first permanent magnetic stirrer (4) is arranged at the lower end of the smelting furnace (1) in the middle of the base (3), a heat collecting device (5) is installed at the bottom end of the smelting furnace (1), a lifter (10) is arranged at the top of the smelting furnace (1), a driving motor (8) is arranged on one side of the lifter (10) and is installed at the top of the smelting furnace (1), the driving motor (8) is connected to the lifter (10) through a shaft sleeve, a lifting rod (9) is arranged on the lifter (10), and a filter plate (7) is connected to the lower end of the lifting rod (9), sliding frames (6) are arranged on both sides of the interior of the smelting furnace (1), the filter plate (7) is slidably connected to the sliding frame (6), and the side of the smelting furnace (1) is provided with a lifting rod (9). The bottom end is connected to a refining furnace (13) through a pipeline (11); a regulating valve (12) is arranged in the middle of the pipeline (11); horizontal plates (14) are arranged oppositely on both sides of the refining furnace (13); a jack (15) is arranged at the lower end of the horizontal plate (14); two vertical plates are fixedly arranged on both sides of the lower end of the refining furnace (13); a second permanent magnetic stirrer (21) is fixedly arranged between the two vertical plates; a sealing sleeve (16) is arranged at the center of the top end of the refining furnace (13); a guide tube (17) is installed in the sealing sleeve (16); a jet structure is arranged at the bottom end of the guide tube (17) and inserted into the melt; the inner center of the guide tube (17) is a vent hole (171); an air outlet hole (172) is penetrated on the jet structure and connected to the vent hole (171); an outlet pipe (20) is arranged on one side of the refining furnace (13); and a solenoid valve is arranged on the outlet pipe (20).

7. The aluminum alloy refining device for precision castings according to claim 6, characterized in that: The first permanent magnetic stirrer (4) is configured the same as the second permanent magnetic stirrer (21), and comprises a permanent magnetic inductor, which is fixedly mounted on the rotating shaft of the motor and is an even number of permanent magnets spaced apart in a circumferential direction, and adjacent permanent magnets have opposite polarities.

8. The aluminum alloy refining device for precision castings according to claim 6, characterized in that: The heat collection device (5) is a disc-type heat collection tube.

9. The aluminum alloy refining device for precision castings according to claim 6, characterized in that: A high-pressure nozzle (19) is arranged at the upper end of the refining furnace (13), and the high-pressure nozzle (19) is connected to an inlet pipe (18). The inlet pipe (18) is used to input a refining agent, and a solenoid valve is arranged on the inlet pipe (18).