High-strength and high-conductivity Cu-Ag alloy ultrathin strip for wafer test probe and preparation method of high-strength and high-conductivity Cu-Ag alloy ultrathin strip

Through medium frequency induction smelting and solid solution-rolling-aging treatment processes, high-strength and high conductivity Cu-Ag alloy ultra-thin strips were prepared, which solved the problems of insufficient material brittleness and conductivity in the prior art, and realized the Massive production of high-performance probe materials suitable for wafer detection.

CN118910459AActive Publication Date: 2024-11-08贵研功能材料(云南)有限公司 +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410954353.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

The existing Cu-Ag alloy strips cannot meet the high strength and high conductivity requirements of wafer detection probes, and there are problems of material brittleness and toxic oxides during the preparation process.

Method used

Using the combined process of medium frequency induction smelting, solid solution-rolling-aging treatment, large deformation cold rolling and intermediate heat treatment, Cu-Ag alloy ultra-thin strip with an Ag content of 6~20 wt% was prepared, and the Ag phase was passed through Precipitation and Cu matrix work hardening to form high-strength and high conductivity materials.

Benefits of technology

Massive preparation of Cu-Ag alloy ultra-thin strips with high strength (1132-1180MPa) and high conductivity (69-70.4%IACS) is suitable for medium power wafer detection probes, and the process is simple without adding any other Strengthening elements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910459A_ABST
    Figure CN118910459A_ABST
Patent Text Reader

Abstract

The invention discloses a high-strength and high-conductivity Cu-Ag alloy ultrathin strip for a wafer test probe and a preparation method of the high-strength and high-conductivity Cu-Ag alloy ultrathin strip. The content of Ag in the Cu-Ag alloy ultrathin strip is 6-20 wt%, the balance is Cu and inevitable impurities, and the content of the impurities is smaller than 0.01 wt%. The composite material mainly comprises a Cu-based solid solution and an Ag-based solid solution, wherein an Ag-rich phase is distributed in the Cu-based solid solution in a fiber structure form; the average grain size is 470-600nm, and the texture is mainly {211} lt; 111gt, 111gt; a copper texture; and the thickness is 30-60 [mu] m. The preparation method comprises the steps of fusion casting, homogenization treatment, rough rolling, aging treatment, intermediate rolling, intermediate annealing, finish rolling and leveling annealing with tension. According to the preparation method of the Cu-Ag alloy ultrathin strip, other strengthening elements do not need to be added, the preparation technological process is simple, and the high-strength and high-conductivity Cu-Ag ultrathin strip can be produced in batches. The tensile strength of the Cu-Ag ultrathin strip ranges from 1132 MPa to 1180 MPa, the yield strength ranges from 1052 MPa to 1101 MPa, the conductivity is about 70% IACS, the hardness ranges from 274 HV0.2 to 303 HV0.2, and the Cu-Ag ultrathin strip can be used as a material for a medium-power wafer detection probe.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of alloy materials, and in particular relates to a high-strength and high-conductivity Cu-Ag alloy ultra-thin strip for a wafer test probe and a preparation method thereof. Background Art

[0002] Semiconductor test probes are mainly used in semiconductor design verification, wafer testing, finished product testing and other links. They are core components and consumables throughout the entire semiconductor production process. According to the different powers of the wafer to be tested, the probes need to have different current carrying capacities. The current carrying capacity is closely related to the conductivity of the probe material. The conductivity of the probe for testing medium power must be above 65%, and the tensile strength must be above 1000MPa. In order to meet the minimum spacing of the probe card, the probe size is micron-level. At present, commonly used probe materials include tungsten alloy, beryllium copper, Cu-Ag alloy, etc. Tungsten has the advantages of high strength, high conductivity and high temperature resistance, but it also has the problems of high brittleness, easy breakage, easy scratching of the wafer surface, etc., which are not conducive to use. Beryllium copper has high strength and corrosion resistance, but beryllium copper has low conductivity. At the same time, during the preparation process, toxic beryllium oxide will be produced, which is harmful to the human body. Cu-Ag alloy maintains high strength while also having high conductivity, which can meet the performance requirements of probes for medium-power wafer detection.

[0003] At present, the research on high-strength and high-conductivity Cu-Ag alloy mainly focuses on the preparation of wires. The Cu-Ag alloy strips prepared by the existing technology cannot meet the performance requirements of wafer detection probes. The present invention aims to provide an efficient and batch preparation method for high-strength and high-conductivity Cu-Ag alloy ultra-thin strips for wafer test probes without adding additional strengthening elements, using medium-frequency induction melting, solid solution-rolling-aging, large deformation cold rolling and intermediate heat treatment. Summary of the invention

[0004] The first object of the present invention is to provide a high-strength and high-conductivity Cu-Ag alloy ultra-thin strip. The second object of the present invention is to provide a method for preparing the Cu-Ag alloy ultra-thin strip.

[0005] The first object of the present invention is achieved by providing a high-strength and high-conductivity Cu-Ag alloy ultra-thin strip, wherein the Ag content is 6-20wt%, the rest is Cu and unavoidable impurities, and the impurity content is less than 0.01wt%; The Cu-Ag alloy ultra-thin strip is mainly composed of a Cu-based solid solution and an Ag-based solid solution, and the Ag-rich phase is distributed in the Cu-based solid solution in the form of a fibrous structure; The Cu-Ag alloy ultra-thin strip has an average grain size of 470-600 nm and a texture mainly of {211} <111> Copper texture; The Cu-Ag alloy ultra-thin strip has a thickness of 30-60 μm; The Cu-Ag alloy ultra-thin strip has a tensile strength of 1132-1180 MPa, a yield strength of 1052-1101 MPa, an electrical conductivity of 69-70.4% IACS, and a hardness of 274-303 HV 0.2 .

[0006] The second object of the present invention is achieved by the method for preparing the high-strength and high-conductivity Cu-Ag alloy ultra-thin strip, comprising the steps of melting and casting, homogenization treatment, rough rolling, aging treatment, intermediate rolling, intermediate annealing, finishing rolling, and strip tension leveling annealing; Among them, in the aging treatment process, the aging temperature is 400~500℃ and the time is 5~15h; The intermediate rolling process adopts multi-pass rolling, with the deformation of a single pass not exceeding 10% and the total deformation of 90~95%; In the intermediate annealing process, the annealing temperature is 250~350℃ and the holding time is 0.5h~2h.

[0007] The preparation method of the Cu-Ag alloy ultra-thin strip of the present invention adopts solid solution-rolling-aging treatment. On the one hand, the Ag phase is induced to precipitate from the Cu matrix to improve the strength of the alloy. The large deformation rolling causes the Ag precipitation phase to form an Ag fiber structure to produce a strengthening effect. Combined with the work hardening of the Cu matrix, the high strength of the Cu-Ag alloy ultra-thin strip is achieved. On the other hand, after the solid solution, a certain deformation rolling can increase the deformation energy storage and improve the recrystallization driving force of the Cu-Ag alloy. After the aging treatment, the Cu-Ag alloy is more likely to recrystallize, achieving a refinement and homogenization effect, thereby improving the plasticity of the Cu-Ag alloy material, which is conducive to subsequent large deformation rolling. In addition, adding a suitable intermediate annealing process during the preparation process can adjust the dislocation density and solute atom content of the Cu-Ag alloy, reduce the scattering effect in the alloy, and achieve high conductivity.

[0008] The beneficial effects of the present invention are as follows: the preparation method of the Cu-Ag alloy ultra-thin strip of the present invention does not require the addition of other strengthening elements, the preparation process is simple, and high-strength and high-conductivity Cu-Ag ultra-thin strips can be mass-produced. The Cu-Ag ultra-thin strip provided by the present invention has a tensile strength of 1132-1180MPa, a yield strength of 1052-1101MPa, an electrical conductivity of about 70%IACS, and a hardness of 274-303HV 0.2 , can be used as a material for medium-power wafer inspection probes. BRIEF DESCRIPTION OF THE DRAWINGS

[0009] Figure 1The cast structure diagram of the Cu-Ag alloy of the present invention, wherein (a), (b), and (c) are cast structure diagrams of the Cu-Ag alloy of Examples 1-3, respectively, and (d) is the cast structure diagram of the alloy of Comparative Example 1; Figure 2 Figures (a), (b), (c), and (d) are the solid solution microstructure diagrams of the Cu-Ag alloy of Examples 1-3 and Comparative Example 1, respectively; and Figures (e), (e), (g), and (h) are the aging microstructure diagrams of the Cu-Ag alloy of Examples 1-3 and Comparative Example 1, respectively. DETAILED DESCRIPTION

[0010] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments, but the present invention is not limited in any way. Any changes or improvements made based on the teachings of the present invention fall within the protection scope of the present invention.

[0011] The invention discloses a high-strength and high-conductivity Cu-Ag alloy ultra-thin strip for wafer test probes, wherein the Ag content is 6-20wt%, the rest is Cu and inevitable impurities, and the impurity content is less than 0.01wt%; The Cu-Ag alloy ultra-thin strip is mainly composed of a Cu-based solid solution and an Ag-based solid solution, and the Ag-rich phase is distributed in the Cu-based solid solution in the form of a fibrous structure; The Cu-Ag alloy ultra-thin strip has an average grain size of 470-600 nm and a texture mainly of {211} <111> Copper texture; The Cu-Ag alloy ultra-thin strip has a thickness of 30-60 μm; The Cu-Ag alloy ultra-thin strip has a tensile strength of 1132-1180 MPa, a yield strength of 1052-1101 MPa, an electrical conductivity of 69-70.4% IACS, and a hardness of 274-303 HV 0.2 .

[0012] The present invention also provides a method for preparing the high-strength and high-conductivity Cu-Ag alloy ultra-thin strip for the wafer test probe, which is achieved by the following steps: 1) Melting and casting: using a vacuum medium frequency furnace to heat the Cu and Ag raw materials to 1200°C in a vacuum for alloying and melting, and casting to obtain a Cu-Ag ingot; 2) Homogenization treatment: placing the Cu-Ag ingot obtained in step 1) into a muffle furnace, and polishing the surface of the ingot to a bright finish after quenching; 3) Rough rolling: rolling the Cu-Ag ingot after homogenization treatment in step 2); 4) Aging treatment: The Cu-Ag block after rough rolling in step 3) is subjected to aging treatment, and the surface of the block is polished to be bright after air cooling; 5) Intermediate rolling: The Cu-Ag block after aging treatment in step 4) is subjected to multiple cold rolling to obtain a Cu-Ag sheet; 6) Intermediate annealing: perform intermediate annealing on the plate after intermediate rolling in step 5), air cool and then grind the plate surface to a bright finish; 7) Finish rolling: The annealed sheet in step 6) is subjected to finish rolling to obtain a 30-60 μm ultra-thin strip of Cu-Ag alloy; 8) Strip tension leveling annealing: The ultra-thin strip after the finish rolling in step 7) is subjected to strip tension leveling annealing.

[0013] In step 2), the homogenization temperature is 750-800°C and the temperature is kept for 4-6 hours.

[0014] In step 3), the total deformation of rough rolling is controlled to be 40-60%.

[0015] In step 4), the aging temperature is 400-500°C and the temperature is kept for 5-15 hours.

[0016] In step 5), the deformation of a single pass of multi-pass cold rolling is controlled to be no more than 10%, and the total deformation is controlled to be 90-95%.

[0017] In step 6), the intermediate annealing temperature is 250-350° C., and the holding time is 0.5 h-2 h.

[0018] In step 7), the deformation of a single pass of finishing rolling is controlled to be no more than 5%, and the total deformation is controlled to be 99.8-99.95%.

[0019] In step 8), the tension leveling annealing temperature is 200~300℃, and the temperature is kept for 0.5h~1h. The vacuum degree of leveling annealing is not less than 5×10 -3 Pa, tension is not less than 400MPa.

[0020] Example 1 1) Melting and casting: Cu and Ag with a purity of ≥99.99% are selected as raw materials, wherein the Ag content is 6wt% and the rest is Cu. The Cu and Ag raw materials are heated to 1200°C in a vacuum in a vacuum medium frequency furnace for alloying and smelting, and then cast to obtain a Cu-6Ag ingot; the alloy structure diagram obtained in this step is as follows: Figure 1 (a) shown.

[0021] 2) Homogenization treatment: The Cu-6Ag ingot obtained in step (1) is placed in a muffle furnace, heated to 780°C and kept for 4 hours, then quenched and the surface of the ingot is polished to a bright finish; the alloy structure obtained in this step is shown in FIG. Figure 2 (a) shown.

[0022] 3) Rough rolling: rolling the homogenized Cu-6Ag ingot obtained in step (2) using a two-roll reversible rolling mill, with the total deformation amount controlled to 40%, to obtain a Cu-6Ag block; 4) Aging treatment: The Cu-6Ag block after rough rolling in step 3) is subjected to aging treatment at a temperature of 500°C for 5 hours. After air cooling, the surface of the block is polished to a bright finish. The alloy structure diagram obtained in this step is shown in FIG. Figure 2 (e) shown.

[0023] 5) Intermediate rolling: The Cu-6Ag block after aging treatment in step 4) is subjected to multiple cold rolling by a two-roll reversible rolling mill, with the deformation of each pass controlled to 10% and the total deformation controlled to 92%, to obtain a Cu-6Ag plate; 6) Intermediate annealing: The plate after intermediate rolling in step 5) is subjected to intermediate annealing at a temperature of 350°C for 1 hour. After air cooling, the plate surface is polished to a bright finish. 7) Finish rolling: The plate after intermediate annealing in step 6) is finish rolled using a precision four-roller rolling mill. The single pass deformation of the finish rolling is controlled to be 5%, and the total deformation is controlled to be 99.9%, to obtain a 40 μm ultra-thin strip of Cu-6Ag alloy.

[0024] 8) Strip tension leveling annealing: A vacuum annealing furnace is used to perform strip tension leveling annealing on the ultra-thin strip after finishing in step 7). The vacuum strip tension leveling annealing temperature is 200°C, the temperature is kept for 1 hour, and the leveling annealing vacuum degree is 5×10 -3 Pa, tension is 400MPa.

[0025] Example 2 1) Melting and casting: Cu and Ag with a purity of ≥99.99% are selected as raw materials, wherein the Ag content is 10wt% and the rest is Cu. The Cu and Ag raw materials are heated to 1200°C in a vacuum in a vacuum medium frequency furnace for alloying and smelting, and then cast to obtain a Cu-10Ag ingot; the alloy structure diagram obtained in this step is as follows: Figure 1 (b) shown.

[0026] 2) Homogenization treatment: The Cu-10Ag ingot obtained in step (1) is placed in a muffle furnace, heated to 800°C and kept for 6 hours, then quenched and the surface of the ingot is polished to a bright finish; the alloy structure obtained in this step is shown in FIG. Figure 2 (b) shown.

[0027] 3) Rough rolling: rolling the homogenized Cu-10Ag ingot obtained in step (2) using a two-roll reversible rolling mill, with the total deformation amount controlled to 40%, to obtain a Cu-10Ag block; 4) Aging treatment: The Cu-10Ag block after rough rolling in step 3) is subjected to aging treatment at a temperature of 450°C for 10 hours. After air cooling, the surface of the block is polished to a bright finish. The alloy structure diagram obtained in this step is shown in FIG. Figure 2 (f) shown.

[0028] 5) Intermediate rolling: The Cu-10Ag block after aging treatment in step 4) is subjected to multiple cold rolling by a two-roll reversible rolling mill, with the deformation of each pass controlled to 8% and the total deformation controlled to 95%, to obtain a Cu-10Ag plate; 6) Intermediate annealing: The Cu-10Ag sheet after intermediate rolling in step 5) is subjected to intermediate annealing at a temperature of 350° C. for a holding time of 2 h. After air cooling, the surface of the sheet is polished to a bright finish; 7) Finish rolling: The Cu-10Ag sheet after intermediate annealing in step 6) is finish rolled using a precision four-roller rolling mill. The single pass deformation of the finish rolling is controlled to be 5%, and the total deformation is controlled to be 99.85%, to obtain a 55μm ultra-thin strip of Cu-10Ag alloy.

[0029] 8) Strip tension leveling annealing: A vacuum annealing furnace is used to perform strip tension leveling annealing on the ultra-thin strip after finishing in step 7). The vacuum strip tension leveling annealing temperature is 220°C, the temperature is kept for 1 hour, and the leveling annealing vacuum degree is 5×10 -3 Pa, tension is 400MPa.

[0030] Example 3 1) Melting and casting: Cu and Ag with a purity of ≥99.99% are selected as raw materials, wherein the Ag content is 20wt% and the rest is Cu. The Cu and Ag raw materials are heated to 1200°C in a vacuum in a vacuum medium frequency furnace for alloying and melting, and then cast to obtain a Cu-20Ag ingot; the alloy structure diagram obtained in this step is as follows: Figure 1 (c) shown.

[0031] 2) Homogenization treatment: The Cu-20Ag ingot obtained in step 1) is placed in a muffle furnace, heated to 780°C and kept for 4 hours, then quenched and the surface of the ingot is polished to a bright finish; the alloy structure obtained in this step is shown in FIG. Figure 2 (c) shown.

[0032] 3) Rough rolling: The Cu-20Ag ingot obtained in step 2) after homogenization treatment is rolled using a two-roll reversible rolling mill, and the total deformation is controlled to be 60% to obtain a Cu-20Ag block; 4) Aging treatment: The Cu-20Ag block after rough rolling in step 3) is subjected to aging treatment at a temperature of 450°C for 15 hours. After air cooling, the block surface is polished to a bright finish. The alloy structure diagram obtained in this step is shown in FIG. Figure 2 (g) shown.

[0033] 5) Intermediate rolling: The Cu-20Ag block after aging treatment in step 4) is subjected to multiple cold rolling by a two-roll reversible rolling mill, with the deformation of each pass controlled to 10% and the total deformation controlled to 90%, to obtain a Cu-20Ag plate; 6) Intermediate annealing: The Cu-20Ag sheet after intermediate rolling in step 5) is subjected to intermediate annealing at a temperature of 300°C for 2 hours, and then air-cooled and the surface of the sheet is polished to a bright finish; 7) Finish rolling: The plate after intermediate annealing in step 6) is finish rolled using a precision four-roller rolling mill. The deformation of a single pass of the finish rolling is controlled to be 5%, and the total deformation is controlled to be 99.8%, to obtain a 60μm ultra-thin strip of Cu-20Ag alloy.

[0034] 8) Strip tension leveling annealing: A vacuum annealing furnace is used to perform strip tension leveling annealing on the ultra-thin strip after finishing in step 7). The vacuum strip tension leveling annealing temperature is 240°C, the temperature is kept for 1 hour, and the leveling annealing vacuum degree is 5×10 -3 Pa, tension is 400MPa.

[0035] Comparative Example 1 1) Melting and casting: Cu and Ag with a purity of ≥99.99% are selected as raw materials, wherein the Ag content is 6wt% and the rest is Cu. The Cu and Ag raw materials are heated to 1200°C in a vacuum in a vacuum medium frequency furnace for alloying and smelting, and then cast to obtain a Cu-6Ag ingot; the alloy structure diagram obtained in this step is as follows: Figure 1 (d) shows that Figure 1 Basically the same as in (a).

[0036] 2) Homogenization treatment: The Cu-6Ag ingot obtained in step 1) is placed in a muffle furnace, heated to 780°C and kept for 4 hours, then quenched and the surface of the ingot is polished to a bright finish; the alloy structure obtained in this step is shown in FIG. Figure 2 (d) shown.

[0037] 3) Aging treatment: The Cu-6Ag block after solid solution in step 2) is subjected to aging treatment at a temperature of 450°C for 24 hours. After air cooling, the block surface is polished to bright rolling. The alloy structure diagram obtained in this step is as follows: Figure 2 (h) shown.

[0038] 4) Multi-pass cold rolling: The Cu-6Ag ingot after aging treatment in step 3) is subjected to multi-pass cold rolling by a two-roll reversible rolling mill, and the total deformation is controlled to be 90%, thereby obtaining a Cu-6Ag plate; 5) Intermediate annealing: The Cu-6Ag sheet after cold rolling in step 4) is subjected to intermediate annealing at a temperature of 450°C for a holding time of 2 hours. After air cooling, the surface of the sheet is polished to a bright finish; 6) Multi-pass cold rolling: cold rolling the Cu-6Ag block after aging in step 4) using a two-roll reversible rolling mill, with the total deformation amount controlled to 99%, to obtain a Cu-6Ag sheet; 7) Intermediate annealing: The Cu-6Ag sheet after cold rolling in step 6) is subjected to intermediate annealing at a temperature of 350° C. for a holding time of 2 h. After air cooling, the surface of the sheet is polished to a bright finish; 8) Finish rolling: The plate after annealing in step 6) is finish rolled using a precision four-roller rolling mill. The deformation of a single pass of the finish rolling is controlled to be 5%, and the total deformation is controlled to be 99.9%, to obtain a 40 μm ultra-thin strip of Cu-6Ag alloy.

[0039] 9) Belt tension annealing and leveling: A vacuum annealing furnace is used to perform belt tension leveling annealing on the ultra-thin strip after finishing in step 8). The vacuum belt tension leveling annealing temperature is 260°C, the temperature is kept for 1 hour, and the leveling annealing vacuum degree is 5×10 -3 Pa, tension is 400MPa.

[0040] from Figure 2 It can be seen that after homogenization treatment, part of the Ag in the cast structure of the alloys of Examples 1-3 and Comparative Example 1 is dissolved into the Cu matrix structure, and then after rolling-aging treatment, the Ag dissolved in the Cu matrix will precipitate in the form of small-sized precipitation phases, and after subsequent rolling, Ag fibers are formed to improve strength. The alloy composition of Example 1 and Comparative Example 1 is the same, but the alloy of Example 1 undergoes plastic deformation before aging. Compared with the aging treatment of the alloy of Comparative Example 1 at 450°C for 24 hours, the aging treatment time can be shortened to 5 hours, and a precipitation phase structure similar to that of Comparative Example 1 can be achieved.

[0041] Experimental Example Performance Test of Strips Prepared in Examples 1-3 1. Strength test The tensile strength and yield strength of the Cu-Ag ultra-thin strips prepared in Examples 1 to 3 and Comparative Example 1 were tested on a universal mechanical properties testing machine, respectively. The test results are shown in Table 1.

[0042] 2. Conductivity test The electrical conductivity of the Cu-Ag ultra-thin strips prepared in Examples 1-3 and Comparative Example 1 was tested using an eddy current conductivity meter. The test results are shown in Table 1.

[0043] 3. Microhardness test The hardness of the Cu-Ag ultra-thin strips prepared in Examples 1-3 and Comparative Example 1 was tested using a microhardness tester, with a load of 0.2 kg and a load holding time of 10 s. The test results are shown in Table 1.

[0044] Table 1 Comparison of performance data of Examples 1-3 and Comparative Example 1 Results analysis: It can be clearly seen from Table 1 that the tensile strength, yield strength and microhardness of the alloy strips prepared in Examples 1-3 of the present invention are greatly improved compared with Comparative Example 1, with a strength improvement of more than 200 MPa and a conductivity of about 70%. Compared with the homogenization-aging treatment-rolling method used in Comparative Example 1, the present invention adopts homogenization-rolling-aging treatment. On the one hand, the Ag phase is induced to precipitate from the Cu matrix to improve the strength of the alloy. The large deformation rolling causes the Ag precipitation phase to form an Ag fiber structure to produce a strengthening effect. Combined with the work hardening of the Cu matrix, the high strength of the Cu-Ag alloy ultra-thin strip is achieved. On the other hand, rolling with a certain deformation after solid solution can increase deformation energy storage and improve the recrystallization driving force of the Cu-Ag alloy. After aging treatment, the Cu-Ag alloy is more likely to recrystallize, achieving refinement and homogenization effects, thereby improving the plasticity of the Cu-Ag alloy material, which is beneficial to subsequent large deformation rolling. In addition, a suitable intermediate annealing process is added during the preparation process, and the high strength and high conductivity of the Cu-Ag alloy ultra-thin strip are achieved through synergistic effect. The Cu-Ag alloy ultra-thin strip obtained by the present invention has a grain size of 470-600nm and a texture mainly of {211} <111> Copper texture, strip tensile strength 1132-1180MPa, yield strength 1052-1101MPa, conductivity 70%IACS, hardness 274-303HV 0.2 , which can be used as materials for medium-power wafer inspection probes.

[0045] The above is only a preferred embodiment of the present invention, and does not limit the present invention in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still belongs to the protection scope of the technical solution of the present invention.

Claims

1. A high-strength and high-conductivity Cu-Ag alloy ultra-thin strip, characterized in that: The Cu-Ag alloy ultra-thin strip has an Ag content of 6-20wt%, and the rest is Cu and unavoidable impurities, and the impurity content is less than 0.01wt%; The Cu-Ag alloy ultra-thin strip is mainly composed of a Cu-based solid solution and an Ag-based solid solution, and the Ag-rich phase is distributed in the Cu-based solid solution in the form of a fibrous structure; The Cu-Ag alloy ultra-thin strip has an average grain size of 470-600 nm and a texture mainly of {211} <111> Copper texture; The Cu-Ag alloy ultra-thin strip has a thickness of 30-60 μm; The Cu-Ag alloy ultra-thin strip has a tensile strength of 1132-1180 MPa, a yield strength of 1052-1101 MPa, an electrical conductivity of 69-70.4% IACS, and a hardness of 274-303 HV 0.2 .

2. The method for preparing the high-strength and high-conductivity Cu-Ag alloy ultra-thin strip according to claim 1, characterized in that: It includes melting and casting, homogenizing treatment, rough rolling, aging treatment, intermediate rolling, intermediate annealing, finishing rolling, and strip tension leveling annealing processes; Among them, in the aging treatment process, the aging temperature is 400~500℃ and the time is 5~15h; The intermediate rolling process adopts multi-pass rolling, with the deformation of a single pass not exceeding 10% and the total deformation of 90~95%; In the intermediate annealing process, the annealing temperature is 250~350℃ and the holding time is 0.5h~2h.

3. The method for preparing the high-strength and high-conductivity Cu-Ag alloy ultra-thin strip according to claim 2, characterized in that: In the homogenization process, the homogenization temperature is 750-800° C. and the temperature is kept for 4-6 hours.

4. The method for preparing the high-strength and high-conductivity Cu-Ag alloy ultra-thin strip according to claim 2, characterized in that: In the rough rolling process, the total deformation of the rough rolling is 40-60%.

5. The method for preparing the high-strength and high-conductivity Cu-Ag alloy ultra-thin strip according to claim 2, characterized in that: In the finishing rolling process, the deformation of a single pass is controlled to be no higher than 5%, and the total deformation is controlled to be 99.8-99.95%.

6. The method for preparing the high-strength and high-conductivity Cu-Ag alloy ultra-thin strip according to claim 2, characterized in that: In the belt tension leveling annealing process, the annealing temperature is 200-300°C, the insulation time is 0.5h-1h, and the vacuum degree is not less than 5×10 -3 Pa, tension is not less than 400MPa.

7. Use of the high-strength and high-conductivity Cu-Ag alloy ultra-thin strip according to claim 1 in the preparation of wafer test probes.

Citation Information

Patent Citations

  • Method for preparing in-situ deformation Cu-Ag composite material by using magnetic field

    CN102031467A

  • High-strength high-electro-conductivity copper-based composite and preparation method thereof

    CN105803246A

  • Preparation method for high-strength high-conductivity Cu-Ag-Fe alloy

    CN105839038A

  • Cu-Ag alloy wire and manufacturing method thereof

    CN117545865A

  • Preparation method and application of endogenous fiber reinforced copper-silver alloy plate

    CN117926048A