Preparation method of ultra-fine grain pure magnesium
By employing low-temperature secondary forging technology, combining hot extrusion and low-temperature forging, the problem of refining pure magnesium grains in existing technologies has been solved, resulting in the production of ultrafine-grained high-purity magnesium rods suitable for clinical medical use. These rods possess excellent corrosion resistance and strength, while reducing equipment requirements and production costs.
Patent Information
- Application Number
- CN202411058432.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-08
AI Technical Summary
Existing technologies for preparing ultrafine-grained pure magnesium often employ alloying methods, which leads to problems such as biotoxicity, high equipment requirements, and high production costs. It is difficult to effectively refine pure magnesium grains without using alloying.
Ultrafine-grained high-purity magnesium rods were prepared by using low-temperature secondary forging technology, including hot extrusion and low-temperature forging, with the temperature controlled within the range of 150 to 350°C and the speed at 2 mm/s.
This method enables the preparation of ultrafine-grained high-purity magnesium rods with a grain size of 2–20 μm without adding other metal elements. These rods possess excellent corrosion resistance and strength, making them suitable for clinical medical applications. Furthermore, the process is simple and requires minimal equipment.
Smart Images

Figure CN118910522A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of magnesium alloy processing, and in particular to a method for preparing ultrafine-grained pure magnesium. Background Art
[0002] In recent years, compared with inert metals and polymer materials, biological magnesium alloys have shown higher safety, degradability and other characteristics, and have attracted much attention in the research and application of new generation implant materials. As a biomedical material, magnesium alloys are easily corroded in clinical applications, resulting in premature failure of its mechanical properties, which has always been a key problem that has troubled researchers. The faster degradation rate causes severe corrosion of the implant material before the body has recovered, causing the workpiece to lose mechanical support prematurely and causing the material to fail. Refining the structure of magnesium alloys is one of the effective ways to improve this phenomenon. At present, the main alloying method is used. During the extrusion or rolling process of magnesium alloys, alloying elements or second phases pin the grain boundaries, thereby inhibiting excessive grain growth.
[0003] The Chinese patent with publication number CN 116103549 A discloses an ultrafine-grained magnesium alloy containing Mn and Sb and its preparation method. The Sb element forms a network second phase in the magnesium alloy, provides nucleation points for dynamic recrystallization during the hot deformation of the magnesium alloy, and cooperates with the Mn particles to refine the grain size to obtain an ultrafine-grained magnesium alloy with a grain size of 3-4μm. However, the Sb element has chronic toxicity and carcinogenicity to organisms, and the alloy cannot be used in the biological field.
[0004] The Chinese patent with publication number CN 114075629 A discloses a Mg-Zn-Si-Gd-Y biodegradable ultrafine bio-magnesium alloy. The strength and toughness of the cast bio-magnesium alloy are improved by alloying modification, and stir friction processing is further used to assist deep cryogenic treatment and ultrasonic vibration to achieve the preparation of ultrafine-grained bio-magnesium alloy, and its grain size reaches ~5μm. However, this method has high requirements for equipment, resulting in high production costs. In addition, the added Gd element is a heavy metal element. Although it will be used in some medical applications (such as magnetic resonance imaging (MRI) contrast agents), the toxicity of gadolinium cannot be ignored. If it is improperly used or poorly metabolized, gadolinium can accumulate in the body and cause damage to organs such as the kidneys.
[0005] However, some pure magnesium medical devices that have been disclosed cannot use similar alloying methods to refine the grain size. For example: Chinese patent with publication number CN 219680933 U - aqueous humor drainage device for treating glaucoma, Chinese patent with publication number CN105056309 A - pure magnesium bone screw, etc. If the microstructure of pure magnesium can be controlled and its grains can be refined, the corrosion resistance and strength of pure magnesium medical devices will also be improved. Therefore, how to effectively refine pure magnesium grains without using alloying methods and develop ultrafine pure magnesium is a technical problem that needs to be solved urgently. Summary of the invention
[0006] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a method for preparing ultrafine-grained pure magnesium, so as to solve the problems in the prior art that adding other elements to achieve the effect of refining the grains but will have biological toxicity, and other methods for refining pure magnesium grains have high requirements on equipment and increase production costs and energy consumption.
[0007] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0008] A method for preparing ultrafine-grained pure magnesium comprises the following steps:
[0009] Step 1: Processing and obtaining pure magnesium ingot;
[0010] Step 2: directly hot extrude the pure magnesium ingot obtained in step 1 without heat preservation, the extrusion temperature is 150-350° C., and after extrusion, cool to obtain a semi-finished product of 25 mm high-purity magnesium rod;
[0011] Step 3: processing the high-purity magnesium rod obtained in step 2 into a high-purity magnesium ingot again;
[0012] Step 4: forging the high-purity magnesium ingot obtained in step 3 at 150-350° C. without heat preservation, and obtaining the ultrafine-grained high-purity magnesium rod after cooling.
[0013] Preferably, in step 1, calculated by mass percentage, the Mg content in the pure magnesium ingot is not less than 99.99%, and the pure magnesium ingot also contains inevitable impurities, and the content of the inevitable impurities does not exceed 0.01%.
[0014] Preferably, in step 2, the extrusion temperature is 150°C.
[0015] Preferably, in steps 2 and 4, the pure magnesium ingot does not need to be subjected to a heat preservation treatment before extrusion or forging.
[0016] Preferably, in step 4, forging is performed at a speed of 2 mm / s.
[0017] Preferably, the grain size of the ultrafine-grained high-purity magnesium rod is 2 to 20 μm.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] 1. The present invention adopts pure magnesium as raw material and adjusts the preparation method of pure magnesium rod. By adopting low-temperature secondary forging technology, the grain size in pure magnesium is further reduced. Without adding other metal elements, the effect of grain refinement is achieved, so that the prepared ultrafine-grained high-purity magnesium rod has good corrosion resistance and sufficient strength. Moreover, since no other metal elements are added, the prepared rod is harmless to the human body and can be well used in clinical medicine.
[0020] 2. The process flow of the preparation method of the present invention is simple and clear, does not require complicated operations, has low requirements on equipment, can be applied to the production of large-size and large-batch high-purity magnesium bars, and has good industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is the flow chart for the preparation of ultrafine-grained high-purity magnesium rods.
[0022] Figure 2 Recrystallization structure diagrams of high-purity magnesium rods were prepared for Comparative Examples 1 to 3 and Examples 1 to 3.
[0023] Figure 3 The specific fraction ratio diagram of the recrystallization structure of high-purity magnesium rods prepared for Comparative Examples 1 to 3 and Examples 1 to 3.
[0024] Figure 4 These are the test results of the microstructure of the high-purity magnesium rods prepared in Comparative Examples 1 to 3 and Examples 1 to 3.
[0025] Figure 5 These are the mechanical property test results of the high-purity magnesium rods prepared in Comparative Examples 1 to 3 and Examples 1 to 3.
[0026] Figure 6 These are the hydrogen evolution test results of the high-purity magnesium rods prepared in Comparative Examples 1 to 3 and Examples 1 to 3.
[0027] Figure 7 These are the corrosion rate test results of high-purity magnesium rods prepared in Comparative Examples 1 to 3 and Examples 1 to 3. DETAILED DESCRIPTION
[0028] The present invention will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. All other embodiments obtained by ordinary technicians in this field based on the present invention belong to the scope of protection of the present invention.
[0029] Unless otherwise indicated in specific cases in the present invention, the numerical ranges listed herein include the upper and lower limits, and all integers and fractions within the range, and are not limited to the specific values listed when defining the range.
[0030] 1. A method for preparing ultrafine-grained pure magnesium
[0031] Step 1: Processing and obtaining pure magnesium ingot;
[0032] Step 2: directly hot extrude the pure magnesium ingot obtained in step 1 without heat preservation, the extrusion temperature is 150-350° C., and after extrusion, cool to obtain a semi-finished product of 25 mm high-purity magnesium rod;
[0033] Step 3: Processing the high-purity magnesium rod obtained in step 2 again into a 25 mm high-purity magnesium ingot;
[0034] Step 4: The Φ25 mm high-purity magnesium ingot obtained in step 3 is forged at a speed of 2 mm / s at 150-350° C. without heat preservation, and the ultrafine-grained high-purity magnesium rod is obtained after cooling.
[0035] In the prior art, when refining the grains of medical pure magnesium metal, methods such as modification, increasing supercooling, mechanical vibration or stirring, heat treatment and plastic deformation are often used to achieve this, but these methods all have problems: although other elements added during modification can have a good effect of refining the grains, they may be biologically toxic, and the amount of addition needs to be strictly controlled to ensure biological safety; increasing the supercooling will affect the density of the material and cause internal stress concentration; mechanical vibration or stirring has high requirements on equipment, increasing production costs and energy consumption; the heat treatment process is complicated, requiring precise control of temperature and time, which may affect other properties of the material; plastic deformation also has high requirements on equipment, increasing production costs and causing anisotropy of the material. The present invention improves the preparation method of high-purity magnesium rods, and it is expected that ultrafine high-purity magnesium rods can be obtained by a simple method that does not require high equipment, thereby reducing the difficulty of refining the grains of medical pure magnesium metal.
[0036] In some embodiments, the pure magnesium ingot obtained in step 1 is hot extruded at a temperature of 150 to 350°C, and then cooled to obtain a semi-finished Φ25 mm high-purity magnesium rod. More preferably, the pure magnesium ingot obtained in step 1 is hot extruded at 150°C, and then cooled to obtain a semi-finished Φ25 mm high-purity magnesium rod. When the hot extrusion temperature is lower than 150℃, the atomic activity in the pure magnesium ingot is weak, and the process of recrystallization and grain refinement is not sufficient. Even if it is processed into an ingot and then subjected to low-temperature forging and extrusion, the refinement effect brought by the forging and extrusion will be affected, and it may also cause the performance of cracks in the extrusion process, making it difficult to flow evenly, thereby adversely affecting the final mechanical properties of the product; when the hot extrusion temperature is higher than 250℃, although it can significantly accelerate the diffusion of atoms and the boundary migration of grains in the pure magnesium ingot, which is beneficial to grain refinement, it will also cause excessive grain growth, especially when the holding time is too long. This is because the recovery and recrystallization speed of the material at high temperature is accelerated, which in turn causes the newly formed fine grains to merge into larger grains; at the same time, too high a temperature may cause the grain boundary sliding to be too active, causing the material to be over-softened before hot extrusion, affecting the precision and surface quality of extrusion molding, thereby causing the dimensional stability of the extruded part to deteriorate. Therefore, the temperature for hot extrusion of the pure magnesium ingot can be 150℃, 250℃, 350℃, etc., as well as all ranges and sub-ranges between the above values.
[0037] In some embodiments, the high-purity magnesium rod obtained in step 2 is subjected to secondary processing to obtain a Ф25mm×40mm high-purity magnesium ingot, and then the high-purity magnesium ingot obtained after the secondary processing is forged and extruded under the condition of 150-350°C, and the ultrafine-grained high-purity magnesium rod is obtained after cooling. The present invention performs low-temperature forging and extrusion on the high-purity magnesium ingot obtained after the secondary processing, and within this range, the pure magnesium grains after the previous hot extrusion treatment can be further refined, thereby obtaining a more uniform and fine grain structure. However, if the low-temperature forging and extrusion temperature is too low, the grain boundary movement and texture evolution inside the high-purity magnesium ingot during the forging and extrusion process are not active enough, which is not conducive to obtaining a uniform and fine grain structure and an ideal texture distribution, and also leads to limited plastic deformation capacity of the high-purity magnesium ingot, large deformation resistance, and thus difficult processing, and it is easy to crack or break; and, too low a temperature will make the recrystallization process insufficient, the grain refinement effect is not clear, and because the local area may produce a high density of dislocations due to uneven deformation, it will affect the mechanical properties of the pure magnesium rod finally obtained. However, if the temperature of low-temperature forging is too high, the grains formed during the previous hot extrusion will undergo excessive dynamic recovery or even recrystallization, resulting in grain growth, especially if the forging rate is not fast enough and the movement of the grain boundaries cannot be effectively suppressed, which may offset the effect of grain refinement brought about by the previous hot extrusion and affect the strength and toughness of the final product. Moreover, too high a temperature may cause oxidation of the surface of the pure magnesium ingot, affecting the surface quality and purity. Therefore, the temperature during low-temperature forging can be 150°C, 250°C, 350°C, etc., as well as all ranges and sub-ranges between the above values. At the same time, the low-temperature forging speed is controlled at 2mm / s. A speed lower than this may result in insufficient optimization of grain refinement and texture distribution, and may even offset the favorable effects of the previous hot extrusion. A speed higher than this may cause excessive deformation inside the material in a short period of time, uneven deformation area, and thus affect the mechanical properties of the pure magnesium rod. It should be understood that in the implementation scheme, any of the above ranges can be combined with any other ranges.
[0038] In some embodiments, the ultrafine-grained high-purity magnesium rod obtained by the method of the present invention can have a grain size of 2 to 20 μm. The grain size can be 2 to 5 μm, 10 to 16 μm, 16 to 20 μm, etc., and all ranges and sub-ranges between the above values. It should be understood that in embodiments, any of the above ranges can be combined with any other ranges.
[0039] 2. Examples and Comparative Examples
[0040] Example 1
[0041] Step 1: Prepare corresponding raw materials according to 99.99wt.% Mg and unavoidable impurities <0.01wt.% to obtain a pure magnesium ingot;
[0042] Step 2: machining: machining the high-purity magnesium raw material into an ingot with a cross-sectional diameter of 70 to 80 mm and a height of 10 to 15 mm;
[0043] Step 3: hot extrusion: the high-purity magnesium ingot in step 2 is directly hot extruded without heat preservation, the extrusion temperature is 150°C, the diameter of the extrusion barrel is 80mm, and after extrusion, air cooling is performed to obtain a semi-finished product of 25mm high-purity magnesium rod; the extruder model used for hot extrusion is XJ-500 horizontal extruder;
[0044] Step 4: Secondary processing: Process the 25 mm diameter high-purity magnesium rod in step 3 into a 25 mm × 40 mm diameter high-purity magnesium ingot;
[0045] Step 5 low-temperature forging: The 25 mm × 40 mm high-purity magnesium ingot in step 4 is forged at 150° C. without heat preservation, and the diameter of the forging die is 25 mm. After forging, air cooling is performed to obtain a 16 mm high-purity magnesium rod; wherein the forging machine model for low-temperature forging is a YQ32-2006 vertical hydraulic press.
[0046] According to the method of Example 1 and the process parameters in Table 1, examples and comparative examples were prepared.
[0047] Table 1
[0048] Examples Hot extrusion temperature Low temperature forging temperature Low temperature forging speed Recrystallization fraction 1 150℃ 150℃ 2mm / s 90.6 2 250℃ 250℃ 2mm / s 46 3 350℃ 350℃ 2mm / s 92.6 Comparative Example 1 150℃ 150℃ -- 44.2 Comparative Example 2 250℃ 250℃ -- 80.8 Comparative Example 3 350℃ 350℃ -- 91.5
[0049] Note: -- indicates that the step is not processed.
[0050] Among them, comparative examples 1 to 3 were not subjected to low temperature forging and extrusion, but only to hot extrusion. Figure 1 shown.
[0051] The pure magnesium rods prepared in Examples 1 to 3 have undergone two refinement processes in their internal grains. Hot extrusion performed the first grain refinement on the pure magnesium rods, and most of the grains in the pure magnesium rods were refined at a relatively low extrusion temperature. After low-temperature forging and extrusion, the already refined grains were further refined. Controlling the low-temperature forging and extrusion temperature within the range of 150 to 350°C can have a certain refinement effect on the grains. The average particle size of the magnesium alloy rods finally prepared can be controlled within 20μm. However, as the temperature of the low-temperature forging and extrusion gradually increased, some of the grains in the pure magnesium rods grew. Comparative Examples 1 to 3 studied the extrusion temperature. Figure 2As shown. The white area in the figure is the substructure, the gray is the unrecrystallized structure, and the black is the recrystallized structure. After 150°C extrusion, the unrecrystallized area structure of the comparative example 1 sample accounts for as high as 52%. This shows that although 150°C extrusion can refine some pure magnesium structures, the refinement effect is very limited, and most of the structures are in an unrecrystallized state due to insufficient energy. The same situation exists in comparative example 2. Compared with example 3, although there are not many unrecrystallized areas in comparative example 3, there are more substructures in comparative example 3 than in example 3, and the area of recrystallized structure is also smaller than that in example 3. Therefore, this series of differences will lead to very significant differences in corrosion resistance between comparative example 3 and example 3.
[0052] Then, Examples 1 to 3 were subjected to low temperature forging treatment, so that Examples 1 to 3 all showed a higher degree of recrystallization, and the proportion of non-recrystallized areas was significantly reduced, which were 3.47%, 1.03% and 0.25% respectively. Figure 3 shown.
[0053] The metallographic structures of Comparative Examples 1 to 3 and Examples 1 to 3 were observed. Figure 4 As shown. Among them, the grain structure of Example 1 is the finest, with a grain size of 2.31±0.3μm. Due to the increase in the subsequent forging temperature, Examples 2 and 3 cause the grains formed during the previous hot extrusion to undergo excessive dynamic recovery and recrystallization, resulting in grain growth. The grain size increases to 14.50±4.81μm and 17.40±2.20μm, which can still be controlled within 20μm. Comparative Example 1 shows a large area of deformed structure. Due to the increase in the subsequent extrusion temperature, Comparative Example 2 causes some of the deformed areas formed during hot extrusion to recrystallize, resulting in grain growth, but there are still a small number of deformed areas. In Comparative Example 3, the extrusion temperature is raised to 350°C, and the grains are completely recrystallized and there is no deformation area. However, since it is only hot extruded and no low-temperature forging treatment is performed, compared with Example 3, the recrystallization area is relatively small.
[0054] The corrosion resistance and mechanical properties of the examples and comparative examples were tested. The rods prepared in the examples and comparative examples were immersed in human simulated body fluid (m-SBF) for seven days. The results are shown in Tables 2 and Figures 5 to 7 shown.
[0055] Table 2
[0056] Examples Grain size (μm) <![CDATA[Hydrogen evolution rate (ml / cm 2 )]]> Corrosion rate (mm / y) Tensile strength(MPa) Elongation 1 2.31±0.3 0.63±0.002 0.2±0.008 214 25.8% 2 14.50±2.4 0.89±0.1 0.29±0.04 166 21.2% 3 17.4±2.2 0.82±0.06 0.26±0.02 164 22.2% Comparative Example 1 4.72±3.1 8.1±2.6 2.6±0.8 170 15.8% Comparative Example 2 10.9±4.5 11.4±2.6 3.7±0.8 169 24.2% Comparative Example 3 13.5±2.6 14.0±1.1 4.5±0.3 163 22.1%
[0057] From Table 2 we can see that:
[0058] (1) In terms of mechanical properties, low-temperature forging and extrusion will not have an adverse effect on the tensile strength and elongation of the magnesium alloy, especially Example 1. Compared with Comparative Example 1, the tensile strength and elongation are improved to a certain extent, which shows that forging and extrusion at this low-temperature forging and extrusion temperature will have a favorable effect on the mechanical properties of the rod.
[0059] (2) The pure rod prepared in this example has a very low hydrogen evolution rate, which is very important for magnesium alloys for biological use, because it not only indicates that the magnesium alloy has better corrosion resistance and can exist more stably in the body environment, thereby extending the effective service life of the implant, but also means that the pure rod prepared in this example has better biosafety. The rapid evolution of a large amount of hydrogen will bring safety risks and lead to gas embolism. At the same time, for magnesium alloy implants used as temporary stents or fixation devices, a slower hydrogen evolution rate means that the material can maintain structural integrity for a predetermined period of time, and then gradually degrade and eventually be absorbed by the body.
[0060] (3) Among the pure magnesium rods prepared in the comparative example, although the grain size of some pure magnesium rods was refined, their microstructure was not further optimized, which resulted in more unrecrystallized areas in the microstructure of the pure magnesium rods in the comparative example compared with the example, and the recrystallized areas were not as many as those in the example, which also resulted in the pure magnesium rods in the comparative example having lower hydrogen evolution rate and corrosion rate than those in the example.
[0061] (4) In summary, the pure magnesium rod prepared in the example has good corrosion resistance. On the premise that its mechanical properties can meet the required requirements, the corrosion resistance of the pure magnesium rod can be improved without adding other metal elements.
[0062] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the technical solution. Those skilled in the art should understand that those modifications or equivalent substitutions of the technical solution of the present invention that do not depart from the purpose and scope of the technical solution should be included in the scope of the claims of the present invention.
Claims
1. A method for preparing ultrafine-grained pure magnesium, characterized in that: The specific steps include: Step 1: Processing and obtaining pure magnesium ingot; Step 2: directly hot extrude the pure magnesium ingot obtained in step 1 without heat preservation, the extrusion temperature is 150-350° C., and after extrusion, cool to obtain a semi-finished product of 25 mm high-purity magnesium rod; Step 3: Processing the high-purity magnesium rod obtained in step 2 again into a 25 mm × 40 mm high-purity magnesium ingot; Step 4: forging the high-purity magnesium ingot obtained in step 3 at 150-350° C. without heat preservation, and obtaining the ultrafine-grained high-purity magnesium rod after cooling.
2. The method for preparing the ultrafine grain high purity magnesium rod according to claim 1, characterized in that: In step 1, calculated by mass percentage, the Mg content in the pure magnesium ingot is not less than 99.99%, and the pure magnesium ingot also contains inevitable impurities, and the content of the inevitable impurities does not exceed 0.01%.
3. The method for preparing the ultrafine-grained high-purity magnesium rod according to claim 1, characterized in that: In step 2, the extrusion temperature is 150-350°C.
4. The method for preparing the ultrafine-grained high-purity magnesium rod according to claim 1, characterized in that: In step 4, forging is performed at a speed of 2 mm / s.
5. The method for preparing ultrafine-grained high-purity magnesium rod according to claim 1, characterized in that: The grain size of the ultrafine-grained high-purity magnesium rod is 2 to 20 μm.
Citation Information
Cited By