Crack-free glazing method for thermal barrier coating and application
By using excimer lasers with wavelengths of 157~353 nm for laser glazing of ceramic thermal barrier coatings, the problem of mesh cracks caused by infrared laser glazing is solved, forming a dense glazing layer without cracks or nano-scale cracks, improving the The coating has high temperature oxidation and corrosion resistance, extending the blade life.
Patent Information
- Application Number
- CN202411359433.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing infrared laser glazing technology produces mesh cracks on the surface of ceramic thermal barrier coatings, reducing the thermal insulation and thermal shock properties of the coating. The cracks become corrosion channels for high-temperature gas and external media, resulting in coating failure and shortening of blade life. .
The ceramic thermal barrier coating is laser glazed by excimer laser with a wavelength of 157~353 nm. Through photochemical action with high single photon energy, a dense glazing layer without cracks or nano-scale cracks is formed, reducing the number and size of cracks and improving the The coating has high temperature oxidation and corrosion resistance.
It significantly reduces the number and width of the glazed layer, forms a smooth and dense surface, enhances the coating's resistance to high-temperature oxidation and corrosion, extends the service life of the blade, and reduces the heat influence during processing.
Smart Images

Figure CN118910536A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of laser surface modification, and in particular relates to a method for crack-free glazing of a thermal barrier coating and an application thereof. Background Art
[0002] With the increasing requirements for high thrust and high thrust-to-weight ratio, the temperature of the hot end components of the two engines has exceeded the use limit of the base high-temperature alloy. Therefore, coating the surface of the metal blade with a ceramic thermal barrier coating is one of the key technologies to improve the temperature bearing capacity of the turbine blade. The thermal barrier coating prepared by atmospheric plasma spraying has a large number of pores, microcracks and a rough surface. The pores can provide effective thermal protection for the coating, but at the same time, in the blade service environment, there are thermal shock temperature difference stress mismatch, high temperature oxidation, high temperature corrosion, and gas / carbon sulfur ash adhesion factors that cause the failure of the thermal barrier coating. For example, the rough surface of the plasma sprayed thermal barrier coating is easy to adhere to dust in the atmosphere (the main component of the dust is a mixture of calcium / magnesium / aluminum / silicon oxides, namely CMAS). At the same time, the pores in the coating become corrosion channels for CMAS and oxygen, and the volume expansion of the thermally grown oxides at high temperatures causes the coating to peel off and fail, thereby reducing the service life of the coating.
[0003] Post-treatment of thermal barrier coatings is one of the methods to improve the service life of blades. Post-treatment includes vacuum heat treatment, hot isostatic pressing and laser surface modification of the coating. Among them, laser glazing technology uses a high-energy focused laser beam to melt the surface of the material without contact, and then eliminates defects through rapid solidification of the surface layer to achieve the goal of a dense surface layer. Laser glazing technology can form a smooth and dense remelting layer on the surface of the ceramic material, thereby effectively reducing the porosity and roughness of the surface layer, improving the coating's resistance to molten salt and oxygen corrosion, and has no significant effect on other properties of the ceramic material. The existing technology uses infrared wavelength lasers to laser glaze thermal barrier coatings, which can eliminate lamellar structures and pores to a certain extent, improve density and reduce roughness. However, the rapid solidification process during infrared laser glazing inevitably produces reticular cracks on the surface of the ceramic material. These through-the-net cracks will become corrosion channels for high-temperature gas and foreign media under long-term service conditions, which is not conducive to improving the life of the blade. In addition, the infrared laser glazing has a large depth, which will reduce the thermal insulation and thermal shock properties of the coating. Therefore, it is urgent to develop a method that can reduce the number and size of surface cracks on the glaze layer of ceramic materials to improve the coating's resistance to high-temperature oxidation and corrosion and extend the life of the blade. Summary of the invention
[0004] In order to solve all or part of the above technical problems, the present invention provides the following technical solutions: One of the purposes of the present invention is to provide a method for crack-free glazing of a thermal barrier coating, the method comprising: using an excimer laser to irradiate the surface of a ceramic layer of the thermal barrier coating to form a glazing layer on the surface of the ceramic layer; the wavelength of the excimer laser is 157-353 nm, the laser power of the excimer laser irradiating the thermal barrier coating is 1-30 W, and the energy density is 1-10 J / cm 2 , the scanning speed is 0.5~20 mm / s, the frequency is 5~100 Hz, and the spot overlap rate is 10%~70%; when the excimer laser irradiates the thermal barrier coating, the laser beam is in a defocused state, and the defocus amount is 10~60 mm.
[0005] The "crack-free" mentioned in the present invention means that the surface of the glaze layer formed by the method of the present invention is magnified 400 times under a scanning electron microscope and still no cracks can be seen, and the crack width is less than 50 nm. The morphology of the nano-scale cracks produced by the present invention is completely different from that of conventional treatment methods.
[0006] The present invention finds that the glaze layer formed by laser glazing with an excimer laser of wavelength between 157 and 353 nm has a smooth surface without obvious cracks and no transverse cracks inside, which can significantly reduce the number of cracks in the glaze layer, and the crack width can be reduced to the nanometer level, solving the problem of large number and large size of reticular cracks in the glaze layer formed by laser glazing with infrared wavelength in the prior art, thereby improving the high temperature oxidation resistance and corrosion resistance of the thermal barrier coating. This is because the single photon energy of the excimer laser is high, which is 5 times the energy of the laser with a wavelength of 1.06 microns, and can directly destroy the molecular bonds to ablate the surface layer of the material. The thickness of the glaze layer obtained by processing is less than 2 microns, and the thinner glaze layer reduces the stress during the remelting process of the material.
[0007] In addition, the excimer laser energy in this band is relatively large, which can directly destroy the chemical bonds of ceramic materials, mainly manifested as photochemical effects. The glazing process is not accompanied by or is accompanied by only a small amount of heat, which is a cold processing method. Compared with the hot processing method in the prior art that uses the high heat of the laser to melt the material, the method of the present invention has a smaller thermal effect, which can reduce the impact of the heat generated during the processing on the temperature-sensitive substrate and increase the application scenarios of the technology.
[0008] In addition, compared with the prior art, this technology can reduce the roughness of the glaze layer without mechanical / electrolytic polishing.
[0009] In some embodiments, the wavelength of the excimer laser is 157 nm, 193 nm, 248 nm, 308 nm, 351 nm or 353 nm.
[0010] In some preferred embodiments, the wavelength of the excimer laser is 248 nm.
[0011] The preparation method of the ceramic material can be one or more of sintering, spraying, and physical vapor deposition, but is not limited thereto. The thermal barrier coating can be post-processed during preparation, and the post-processing method includes heat treatment, laser remelting, chemical etching, etc., which is not particularly limited in the present invention.
[0012] The method of the present invention is suitable for existing high-melting-point ceramic materials commonly used in thermal barrier coatings and has universal applicability. In some embodiments, the material of the ceramic layer of the thermal barrier coating includes one or more combinations of oxide ceramics, nitride ceramics or carbide ceramics. For example, the material of the ceramic layer includes ZrO2, Y2O3, RE2Zr2O7, RETaO4, ABO3, 6~8wt% Y2O3 stabilized ZrO2, etc. These ceramic materials have stable high-temperature performance and a laser absorption rate of more than 90%.
[0013] In some embodiments, the laser glazing is performed in a vacuum environment, an inert atmosphere protection, or an atmospheric environment.
[0014] The second object of the present invention is to provide a surface treatment method for ceramic materials, comprising: irradiating the surface of the ceramic material with an excimer laser to form a glaze layer on the surface of the ceramic material; the wavelength of the excimer laser is 157-353 nm, the laser power of the excimer laser irradiating the thermal barrier coating is 1-30 W, and the energy density is 1-10 J / cm 2 , the scanning speed is 0.5~20 mm / s, the frequency is 5~100 Hz, and the spot overlap rate is 10%~70%; when the excimer laser irradiates the thermal barrier coating, the laser beam is in a defocused state, and the defocus amount is 10~60 mm.
[0015] In some embodiments, the wavelength of the excimer laser is 157 nm, 193 nm, 248 nm, 308 nm, 351 nm or 353 nm.
[0016] In some embodiments, the wavelength of the excimer laser is 248 nm.
[0017] In some embodiments, the ceramic material includes one or a combination of oxide ceramics, nitride ceramics, or carbide ceramics.
[0018] In some embodiments, the ceramic material includes ZrO2, Y2O3, RE2Zr2O7, ReTaO4, ABO3 or 6~8wt% Y2O3 stabilized ZrO2.
[0019] The further technical scheme of laser glazing in the "surface treatment method of ceramic materials" has been specifically described in one of the purposes of the present invention, "a method for crack-free glazing of thermal barrier coatings", and will not be repeated here.
[0020] The third object of the present invention is to provide a thermal barrier coating structure, which includes a bonding layer and a ceramic layer, wherein the bonding layer is used to combine with a base material, and a glaze layer is formed on the side of the ceramic layer away from the bonding layer, and the glaze layer is formed by the method described in any of the above technical solutions.
[0021] In some embodiments, the thickness of the glaze layer is less than 2 μm, preferably 200-1000 nm.
[0022] The method provided by the present invention can transform the rough structure of the surface of the thermal barrier coating in the sprayed state into a smooth glaze layer, eliminating the rough surface characteristics of the original ceramic material; the glaze layer is a dense columnar crystal structure, dense and non-porous, and non-layered structure, eliminating the pores and layered structures existing in the thermal spray layer.
[0023] The width of the mesh cracks formed by the existing technology using infrared lasers is usually 1 to 20 microns. Although the width of the cracks can be reduced by adjusting the process, the number of cracks will increase, and the crack area will account for about 2.8%. The method of the present invention can make the surface of the glaze layer magnified 400 times under a scanning electron microscope still invisible cracks, and the crack width is less than 50 nm, that is, the "crack-free" described in the present invention is achieved. According to the relationship between the depth of erosion of the crack along the typical external medium and the crack width, it can be seen that when the crack width is reduced by one order of magnitude, the time taken by the external medium to erode the same depth will increase by 10 times, thereby significantly improving the service life of the material.
[0024] A fourth object of the present invention is to provide an application of the method described in any of the above technical solutions or the thermal barrier coating structure described in any of the technical solutions in the preparation of aircraft engine turbine blades or gas turbine turbine blades.
[0025] A fifth object of the present invention is to provide an engine turbine blade, wherein the engine turbine blade comprises the thermal barrier coating structure of the blade substrate, and the thermal barrier coating structure is formed on the surface of the blade substrate.
[0026] A sixth object of the present invention is to provide a gas turbine turbine blade, wherein the gas turbine turbine blade comprises a blade substrate and the thermal barrier coating structure, wherein the thermal barrier coating structure is formed on the surface of the blade substrate.
[0027] Compared with the prior art, the present invention has at least the following beneficial effects: (1) The present invention uses an excimer laser with a wavelength in the ultraviolet band to laser glaze the ceramic-based thermal barrier coating to obtain a smooth and dense glaze layer with no surface cracks and no transverse cracks inside; the formed glaze layer has good bonding with the ceramic-based thermal barrier coating; the glaze layer can effectively prevent high-temperature combustion gas, oxygen, etc. from penetrating into the interior of the ceramic material, improve the anti-CMAS corrosion performance of the ceramic material, and the smooth surface of the glaze layer can reduce the adhesion of impurities such as sand, stone, and dust, and is suitable for application in aircraft engine turbine blades or gas turbine turbine blades; (2) The method adopted by the present invention can form a glaze layer with a thickness not exceeding 2 microns on the surface of the thermal barrier coating, without affecting other properties of the base material. It is suitable for surface modification of various ceramic materials and difficult-to-process materials, has a wide range of applications, high processing efficiency, and can be industrially produced and applied. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0029] Figure 1 This is the untreated surface morphology of the 8YSZ thermal barrier coating material of Example 1 of the present invention; Figure 2 This is the untreated cross-sectional morphology of the 8YSZ thermal barrier coating material of Example 1 of the present invention; Figure 3 This is the surface morphology of the 8YSZ thermal barrier coating of Example 1 of the present invention after laser glazing by an ultraviolet excimer laser with a wavelength of 248 nm; Figure 4 This is the cross-sectional morphology of the 8YSZ thermal barrier coating of Example 1 of the present invention after being laser glazed by an ultraviolet excimer laser with a wavelength of 248 nm; Figure 5 is an element distribution diagram of Si in the thermal barrier coating with a glaze layer in Example 1 of the present invention after being corroded at 1250° C. for 10 h in a CMAS environment; Figure 6 This is the cross-sectional morphology of the thermal barrier coating with a glaze layer according to Example 1 of the present invention oxidized at 1050° C. for 100 h. DETAILED DESCRIPTION
[0030] The technical solution of the present invention is described in detail below in conjunction with specific embodiments so that those skilled in the art can better understand and implement the technical solution of the present invention. The specific functional details disclosed herein should not be interpreted as limiting, but only as the basis for the claims and as a representative basis for teaching those skilled in the art to adopt the present invention in different ways in any appropriate detailed embodiment.
[0031] Unless otherwise specified, the raw materials and reagents used in the specific embodiments of the present invention are all commercially available.
[0032] Example 1 Using nickel-based high-temperature alloy as the substrate material, an 8YSZ thermal barrier coating is formed on the nickel-based high-temperature alloy by atmospheric plasma spraying. The thickness of the bonding layer in the thermal barrier coating is about 70 μm, and the thickness of the ceramic layer is about 190 μm. The thermal barrier coating was laser glazed using a 248 nm ultraviolet excimer laser with a laser power of 16 W and a laser energy density of 1.42 J / cm 2 , frequency is 100 Hz, defocus is 40 mm, spot overlap is 50%, laser scanning speed is 1 mm / s, and a glazing layer with a thickness of 1000 nm is formed on the ceramic layer of the thermal barrier coating.
[0033] Figure 1 and Figure 2 These are the surface morphology and cross-sectional morphology of the 8YSZ thermal barrier coating before laser glazing. It can be seen that the surface is relatively rough, with a large number of unmelted particles, and a large number of pores and layered features in the cross section. The porosity is approximately 8.07% through statistical calculation.
[0034] Figure 3 This is the surface morphology after glazing in this embodiment. There are no unmelted particles on the surface, and the surface is smooth, dense and crack-free. By further enlarging the image and measuring, the width of the crack is about 34 nm. Figure 4 This is a cross-sectional view of the coating after glazing cut by a focused ion beam. The top is a dense glaze layer, and the bottom is still the original morphology of the thermal spray coating. The preservation of cracks and holes at the bottom will not lead to a decrease in the thermal insulation and thermal shock properties of the coating, while the thin dense layer on the top eliminates this feature and can effectively prevent corrosion from external media and air.
[0035] The CMAS corrosion test was carried out on the thermal barrier coating containing the glaze layer, as follows: CaO, MgO, Al2O3 and SiO2 powders are mixed in a mass ratio of 33.2:6.5:11.8:48.5, the mixture is ball-milled and sieved, and then dispersed in ethanol to prepare a viscous suspension. As the alcohol evaporates, the viscosity will increase during the coating process. The suspension is coated on the glaze layer prepared above as soon as possible, dried and then weighed; the non-glazed surface of the material is sealed with high-temperature glue, and then the sample is placed in a high-temperature tubular furnace, heated to 1250 ℃ at a heating rate of 10 ℃ / min, and kept warm for 10 h, and then cooled with the furnace.
[0036] The samples after 10 h of CMAS corrosion were characterized. Figure 5 The element distribution diagram of Si after corrosion is shown. The Si element is mainly on the top of the coating, without obvious diffusion into the interior. However, after 10 h of corrosion, CMAS of the untreated coating spreads throughout the coating through pores and cracks.
[0037] The thermal barrier coating containing the glaze layer was subjected to high temperature tests as follows: The sample was placed in a high-temperature tube furnace, heated to 1050 °C at a heating rate of 10 °C / min, kept at this temperature for 100 h, and then cooled in the furnace.
[0038] Figure 6 The morphology of the cross-section thermally grown oxide after high-temperature oxidation is shown, and the thickness of the thermally grown oxide is measured to be 1.92 microns, while the thickness of the oxide layer of the untreated coating is 2.73 microns, an increase of 42.2% over that after glazing.
[0039] Example 2 Using nickel-based high-temperature alloy as the substrate material, an 8YSZ thermal barrier coating is formed on the nickel-based high-temperature alloy by atmospheric plasma spraying. The thickness of the bonding layer in the thermal barrier coating is about 70 μm, and the thickness of the ceramic layer is about 190 μm. The thermal barrier coating was laser glazed using a 248 nm ultraviolet excimer laser with a laser power of 5.6 W and a laser energy density of 1 J / cm 2 , frequency is 50 Hz, defocus is 10 mm, spot overlap is 10%, and laser scanning speed is 10 mm / s. The surface of the obtained glaze layer is still smooth without unmelted particles. Due to the low energy, the surface roughness is slightly improved compared with Example 1, but there is still no micron-level crack on the coating surface.
[0040] Example 3 Using nickel-based high-temperature alloy as the substrate material, an 8YSZ thermal barrier coating is formed on the nickel-based high-temperature alloy by atmospheric plasma spraying. The thickness of the bonding layer in the thermal barrier coating is about 70 μm, and the thickness of the ceramic layer is about 190 μm. The thermal barrier coating was laser glazed using a 248 nm ultraviolet excimer laser with a laser power of 1 W and a laser energy density of 10 J / cm 2 , frequency is 5 Hz, defocus is 60 mm, spot overlap is 70%, and laser scanning speed is 20 mm / s. The surface of the obtained glaze layer is smooth without unmelted particles. The surface roughness of the coating is lower at a higher energy density. There are no micron-level cracks on the coating surface, but the width of the cracks is slightly higher than that of Example 1.
[0041] Example 4 The only difference between Example 4 and Example 1 is that in Example 4, the ultraviolet excimer laser with a wavelength of 248 nm in Example 1 is replaced by an ultraviolet excimer laser with a wavelength of 193 nm.
[0042] The surface of the glaze layer is smooth without unmelted particles. The thickness of the glaze layer becomes smaller under the action of short-wavelength laser, and there are no micron-level cracks on the coating surface.
[0043] Example 5 The only difference between Example 5 and Example 1 is that in Example 5, the 248 nm ultraviolet excimer laser in Example 1 is replaced by an ultraviolet excimer laser with a wavelength of 351 nm.
[0044] The surface of the glaze layer is smooth, without unmelted particles, the thickness of the glaze layer is slightly increased, and there are no micron-level cracks on the coating surface.
[0045] Example 6 The only difference between Example 6 and Example 1 is that the 8YSZ thermal barrier coating in Example 1 is replaced with TiAlN nitride ceramic, and the rest is implemented in the same way as Example 1. The crack state of the glaze layer formed in Example 6 is equivalent to that in Example 1, and the CMAS corrosion resistance and high temperature oxidation resistance of the material are improved.
[0046] Example 7 The only difference between Example 7 and Example 1 is that the 8YSZ thermal barrier coating in Example 1 is replaced by Cr2AlCMAX phase carbide ceramic, and the rest is implemented in the same way as Example 1. The crack state of the glaze layer formed in Example 7 is equivalent to that in Example 1, and the CMAS corrosion resistance and high temperature oxidation resistance of the material are improved.
[0047] Comparative Example 1 This comparative example is basically the same as Example 1, except that: the 8YSZ thermal barrier coating is not subjected to UV excimer laser glazing treatment in Comparative Example 1. The thermal barrier coating of Comparative Example 1 is subjected to CMAS corrosion and high-temperature oxidation tests in the same manner as in Example 1, and it is found that CMAS penetrates into the interior of the coating along the pores and cracks, the coating is severely corroded, and the thickness of the thermally grown oxide at the interface is 2.73 microns, which is 42.2% higher than that of Example 1.
[0048] Comparative Example 2 This comparative example is basically the same as Example 1, except that the ultraviolet excimer laser with a wavelength of 248 nm in Example 1 is replaced by an infrared laser with a wavelength of 1064 nm, and a glazing layer is formed on the 8YSZ thermal barrier coating. The rest is implemented in the same manner as Example 1.
[0049] It was found that the glaze layer formed by infrared laser underwent obvious remelting, with a large number of network cracks and a large depth of the remelted layer, which would lead to a decrease in its thermal insulation and thermal shock properties.
[0050] Comparative Example 3 This comparative example is basically the same as Example 1, except that the 248 nm ultraviolet excimer laser in Example 1 is replaced by a 355 nm ultraviolet picosecond laser, the laser power is 16 W, the frequency is 600 kHz, the spot diameter is 28 nm, the spot overlap rate is 50%, the laser scanning speed is 2000 mm / s, and the rest is implemented in the same way as Example 1.
[0051] By comparing the glaze layers formed in Example 1 and Comparative Example 3, it is found that the width of the surface cracks of the glaze layer of Comparative Example 3 is about 500 nm, and the thickness of the glaze layer is about 2 microns.
[0052] The CMAS corrosion and high temperature oxidation performance tests were performed on the thermal barrier coating with a glaze layer of Comparative Example 3 in the same manner as in Example 1. By comparison, it was found that this example could also hinder the diffusion of CMAS into the interior of the coating, and the thickness of the thermally grown oxide on the interface after high temperature oxidation was 2.19 microns, an increase of 14.1% over Example 1.
[0053] The various aspects, embodiments, features and examples of the present invention should be considered as illustrative in all aspects and are not intended to limit the present invention, the scope of the present invention is defined only by the claims. Other embodiments, modifications and uses will be apparent to those skilled in the art without departing from the spirit and scope of the claimed invention.
[0054] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.
[0055] Although the present invention has been described with reference to illustrative embodiments, it will be appreciated by those skilled in the art that various other changes, omissions and / or additions may be made without departing from the spirit and scope of the present invention and that the elements of the embodiments may be replaced by substantial equivalents. In addition, many modifications may be made without departing from the scope of the present invention to adapt specific circumstances or materials to the teachings of the present invention. Therefore, it is not intended herein to limit the present invention to the disclosed specific embodiments for performing the present invention, but it is intended that the present invention will include all embodiments within the scope of the appended claims. In addition, unless specifically stated, any use of the terms first, second, etc. does not indicate any order or importance, but rather uses the terms first, second, etc. to distinguish one element from another element.
Claims
1. A method for crack-free glazing of a thermal barrier coating, characterized in that: include: irradiating the surface of the ceramic layer of the thermal barrier coating with an excimer laser to form a glaze layer on the surface of the ceramic layer; The wavelength of the excimer laser is 157-353 nm, the laser power of the excimer laser irradiating the thermal barrier coating is 1-30 W, and the energy density is 1-10 J / cm 2 , the scanning speed is 0.5~20 mm / s, the frequency is 5~100 Hz, and the spot overlap rate is 10%~70%; when the excimer laser irradiates the thermal barrier coating, the laser beam is in a defocused state, and the defocus amount is 10~60 mm.
2. The method according to claim 1, characterized in that: The wavelength of the excimer laser is 157 nm, 193 nm, 248 nm, 308 nm, 351 nm or 353 nm; And / or, the material of the ceramic layer of the thermal barrier coating includes one or a combination of oxide ceramics, nitride ceramics or carbide ceramics.
3. The method according to claim 2, characterized in that: The wavelength of the excimer laser is 248 nm.
4. A method for surface treatment of ceramic materials, characterized in that: include: irradiating the surface of the ceramic material with an excimer laser to form a glaze layer on the surface of the ceramic material; The wavelength of the excimer laser is 157-353 nm, the laser power of the excimer laser irradiating the thermal barrier coating is 1-30 W, and the energy density is 1-10 J / cm 2 , the scanning speed is 0.5~20 mm / s, the frequency is 5~100 Hz, and the spot overlap rate is 10%~70%; when the excimer laser irradiates the thermal barrier coating, the laser beam is in a defocused state, and the defocus amount is 10~60 mm.
5. The surface treatment method of ceramic material according to claim 4, characterized in that: The wavelength of the excimer laser is 157 nm, 193 nm, 248 nm, 308 nm, 351 nm or 353 nm; And / or, the ceramic material includes one or a combination of oxide ceramics, nitride ceramics or carbide ceramics.
6. A thermal barrier coating structure, wherein the thermal barrier coating is a multi-layer structure, including a bonding layer and a ceramic layer, wherein the bonding layer is used to bond with a substrate material, characterized in that: A glaze layer is formed on a side of the ceramic layer away from the bonding layer, and the glaze layer is formed by the method according to any one of claims 1 to 3.
7. The thermal barrier coating structure according to claim 6, characterized in that: The thickness of the glaze layer is less than 2 μm.
8. Use of the method according to any one of claims 1 to 3 or the thermal barrier coating structure according to any one of claims 6 to 7 in the preparation of aircraft engine turbine blades or gas turbine turbine blades.
9. An engine turbine blade, characterized in that: It comprises a blade substrate and the thermal barrier coating structure according to claim 6 or 7, wherein the thermal barrier coating structure is coated on the surface of the blade substrate.
10. A gas turbine blade, characterized in that: It comprises a blade substrate and the thermal barrier coating structure according to claim 6 or 7, wherein the thermal barrier coating structure is coated on the surface of the blade substrate.
Citation Information
Patent Citations
TiAl based alloy type thermal barrier coating and preparation method thereof
CN108441854A
Method for improving high temperature resistance and corrosion resistance of thermal barrier coating
CN112962050A