Ion nitriding method for inner cavity of annular part and annular part with nitrided inner cavity
By using the auxiliary anode and gaseous rare earth permeable agent in the cavity of the annular part, the problems of uneven and low efficiency of the nitride layer in the deep cavity in traditional nitriding technology are solved, and an efficient and uniform nitriding layer is achieved. Formation and energy consumption are reduced.
Patent Information
- Application Number
- CN202410960219.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional ion nitriding technology is difficult to form a uniform nitriding layer in the deep cavity of annular parts, and the stability of rare earth permeable agents limits their permeable performance, resulting in low nitriding efficiency and high energy consumption.
The internal cavity of the anode is ionic nitriding process is carried out by the auxiliary anode composite gaseous rare earth permeate, and the volatilization of the gaseous rare earth permeate and the auxiliary anode are triggered to strong glow discharge, which promotes the active release and uniform distribution of rare earth elements. , enhance nitriding efficiency and layer thickness.
It significantly improves the thickness and uniformity of the nitriding layer in the cavity of the annular parts, reduces the nitriding time and energy consumption, and has obvious energy-saving and environmentally friendly benefits.
Smart Images

Figure CN118910538A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of surface treatment, in particular to an ion nitriding method for the inner cavity of an annular part and an annular part with nitrided inner cavity. Background Art
[0002] Ion nitriding technology is an advanced process that uses rarefied nitrogen-containing gas in a vacuum or low-pressure environment to heat and nitride the surface of metal materials through glow discharge. Traditionally, this technology mainly focuses on nitriding strengthening of the outer surface of parts, while local nitriding of the inner cavity of parts has higher technical requirements, especially when the inner cavity is deep. The cathode voltage drop characteristics of glow discharge limit the effective penetration depth of the glow layer, which often makes it difficult to form or unevenly distribute the nitrided layer in the deep cavity, and cannot meet the needs of practical applications.
[0003] In addition, during the ion nitriding process, a passivation film mainly composed of compounds such as CrN and Cr2N3 will naturally form on the surface of the material. Although this film can protect the substrate, it will also hinder further penetration of nitrogen atoms, thereby limiting the thickness and uniformity of the nitride layer.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] The object of the present invention is to provide an ion nitriding method for the inner cavity of an annular part and an annular part with nitrided inner cavity, so as to solve or improve the above technical problems.
[0006] The present invention can be implemented like this:
[0007] In a first aspect, the present invention provides an ion nitriding method for the inner cavity of an annular part, wherein the inner cavity of the annular part is ion nitrided by using an auxiliary anode composite gaseous rare earth catalyst;
[0008] The gaseous rare earth catalyst is formed by a saturated solution containing the rare earth catalyst during ion nitriding accompanied by the volatilization of the solvent. The rare earth catalyst includes at least one of yttrium oxide, cerium oxide and lanthanum oxide.
[0009] In an optional embodiment, the nitriding method includes the following steps: introducing nitriding gas into an ion nitriding device to perform ion nitriding treatment on an inner cavity of the annular component located in the ion nitriding device.
[0010] In an optional embodiment, the ion nitriding treatment includes: evacuating the ion nitriding equipment to below 5 Pa, introducing argon and hydrogen for glow cleaning; then introducing nitriding gas, raising the temperature to 400°C to 800°C under the conditions of a nitriding voltage of 500V to 700V and a gas pressure of 300Pa to 700Pa, and keeping the temperature until a preset nitriding layer depth is obtained.
[0011] In an optional embodiment, the nitriding gas includes nitrogen, hydrogen and a gaseous rare earth catalyst.
[0012] In an optional embodiment, the nitriding gas includes 30% to 80% of hydrogen and 0.5% to 10% of a gaseous rare earth catalyst, with the remainder being nitrogen, by volume percentage.
[0013] In an optional embodiment, the nitriding gas further includes argon.
[0014] In an optional embodiment, the nitriding gas includes 30% to 80% of hydrogen, 2% to 20% of argon and 0.5% to 10% of a gaseous rare earth catalyst, with the remainder being nitrogen.
[0015] In an optional embodiment, the annular component and the auxiliary anode are arranged opposite to each other in the ion nitriding device, and the annular component is located on the cathode disk.
[0016] In an optional embodiment, the auxiliary anode is a circular anode made of the same material as the annular part.
[0017] In an optional embodiment, the shortest distance between the auxiliary anode and the end surface of the inner cavity of the annular component is 100 mm to 300 mm.
[0018] In an optional embodiment, the surface of the cathode disk is provided with through holes.
[0019] In an optional embodiment, there are multiple through holes, and the multiple through holes are evenly distributed on the surface of the cathode disk along the circumference of the cathode disk.
[0020] In an optional embodiment, the diameter of the through hole is larger than the maximum transverse length of the inner cavity of the annular part.
[0021] In an alternative embodiment, the area of the auxiliary anode is equal to the area of the cathode disk.
[0022] In an optional embodiment, the material of the annular part includes at least one of stainless steel, nickel-based alloy and titanium alloy.
[0023] In a second aspect, the present invention provides an inner cavity nitrided annular component, wherein the inner cavity of the annular component is ion nitrided by the ion nitriding method of any one of the aforementioned embodiments.
[0024] In an optional embodiment, the hardness of the nitrided layer of the inner cavity of the annular component is not less than 800 HV.
[0025] The beneficial effects of the present invention include:
[0026] The present invention performs ion nitriding treatment on the rare earth catalyst in gaseous form, which is beneficial to ensure that the rare earth elements can be evenly distributed in the target area of the part to be nitrided, and is not limited by the sample loading position in the nitriding equipment; by adding an auxiliary anode, an environment that triggers a stronger glow discharge in a specific area can be constructed, which can greatly enhance the bombardment effect of charged particles on the rare earth catalyst, so that the originally stable rare earth catalyst can be effectively decomposed to release active rare earth elements, thereby giving full play to its catalytic effect; by adopting a method of combining the auxiliary anode and the gaseous rare earth catalyst, the problem of the thickness and uniformity of the nitriding layer in the inner cavity of the annular part can be effectively solved, the nitriding time can be significantly reduced, the efficiency can be improved, and the energy consumption can be greatly reduced, which has obvious energy-saving and environmental protection benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0028] Figure 1 It is a schematic diagram of the structure of the cathode disk in the present invention;
[0029] Figure 2 This is a cross-sectional metallographic image of the nitrided layer of the inner cavity of a stainless steel annular part obtained in Example 1 of the present invention;
[0030] Figure 3 This is a cross-sectional metallographic image of the nitrided layer of the inner cavity of a nickel-based alloy annular part obtained in Example 2 of the present invention;
[0031] Figure 4 This is a cross-sectional metallographic image of the nitrided layer of the inner cavity of a titanium alloy annular part obtained in Example 3 of the present invention. DETAILED DESCRIPTION
[0032] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0033] The ion nitriding method for the inner cavity of an annular part and the annular part with nitrided inner cavity provided by the present invention are described in detail below.
[0034] In order to solve the problems of low nitriding efficiency, insufficient nitriding layer thickness and uniformity that are common in the ion nitriding process of the inner cavity of the annular part, the addition of rare earth elements in the nitriding process can promote nitriding efficiency and increase nitriding layer thickness to a certain extent, but the traditional method is often realized by directly placing high-purity rare earth blocks in the nitriding furnace to add rare earth elements, and this method is easy to cause nitriding uniformity to be limited (such as the number and position arrangement of rare earth blocks will cause the thickness of the nitriding layer and the uniformity of the organization of the samples at different positions in the furnace to have significant differences, thereby affecting the overall performance stability and predictability of the material after nitriding). In order to solve this difficult problem, the present invention specifically proposes to directly pass the rare earth catalyst into the ion nitriding furnace in a gaseous form after the rare earth catalyst is volatilized with alcohol, so as to ensure that the rare earth elements can be evenly distributed in the target area of the parts to be infiltrated. However, in view of the extreme stability of the rare earth catalyst, conventional ion nitriding conditions are difficult to effectively stimulate its activity, thereby limiting the performance of its catalytic performance.
[0035] To this end, the present invention proposes an ion nitriding method for the inner cavity of an annular part, which uses an auxiliary anode composite gaseous rare earth catalyst to perform ion nitriding treatment on the inner cavity of the annular part.
[0036] The present invention performs ion nitriding treatment on the rare earth catalyst in gaseous form, which is beneficial to ensure that the rare earth elements can be evenly distributed in the target area of the part to be nitrided, and is not limited by the sample loading position in the nitriding equipment; by adding an auxiliary anode, an environment that triggers a more intense glow discharge in a specific area can be constructed, which can greatly enhance the bombardment effect of charged particles on the rare earth catalyst, so that the originally stable rare earth catalyst can be effectively decomposed to release active rare earth elements, thereby giving full play to its catalytic effect; by adopting a method of combining the auxiliary anode and the gaseous rare earth catalyst, the problem of the thickness and uniformity of the nitriding layer in the inner cavity of the annular part can be effectively solved, the nitriding time can be significantly reduced, the energy consumption can be greatly reduced, and obvious energy-saving and environmental protection benefits are achieved.
[0037] In some embodiments, the material of the annular component may illustratively but not limitatively include at least one of stainless steel, nickel-based alloys, and titanium alloys.
[0038] During operation, the annular part and the auxiliary anode are arranged opposite to each other in the ion nitriding equipment, and the annular part is located on the cathode disk. It can be understood that the annular part is located on the cathode disk, and the auxiliary anode is located above the annular part. The auxiliary anode is parallel to the annular part.
[0039] The auxiliary anode can be a circular anode made of the same material as the annular part. The thickness of the auxiliary anode can be 2 mm to 5 mm, such as 2 mm, 3 mm, 4 mm or 5 mm, or other values within the range of 2 mm to 5 mm.
[0040] The shortest distance between the auxiliary anode and the end face of the inner cavity of the annular part is 100 mm to 300 mm. It can also be understood that the distance between the auxiliary anode and the upper end face of the annular part is 100 mm to 300 mm, such as 100 mm, 150 mm, 200 mm, 250 mm or 300 mm, or other values within the range of 100 mm to 300 mm.
[0041] By placing the auxiliary anode in parallel at an appropriate position above the inner cavity of the annular part to be nitrided, an environment that can induce a more intense glow discharge in a specific area can be constructed. This enhanced glow discharge not only strengthens the nitrogen potential and promotes the in-depth nitriding process, but more importantly, it greatly enhances the bombardment effect of charged particles on the rare earth catalyst, allowing the originally stable rare earth catalyst to be effectively decomposed and release active rare earth elements, thereby giving full play to its catalytic effect.
[0042] In some embodiments, reference Figure 1 The surface of the cathode disk is provided with through holes. The number of through holes can be multiple, and the multiple through holes are evenly distributed on the surface of the cathode disk along the circumference of the cathode disk.
[0043] The aperture of the through hole is larger than the maximum transverse length of the inner cavity of the annular part. It can also be understood that the size of the through hole is larger than the maximum size of the inner cavity of the annular part, and smaller than the maximum size of the outer ring of the protective tooling.
[0044] In some embodiments, the area of the auxiliary anode is equal to the area of the cathode disk.
[0045] In some embodiments, the gaseous rare earth catalyst is formed by the saturated solution containing the rare earth catalyst during the ion nitriding process accompanied by the volatilization of the solvent, and the rare earth catalyst includes at least one of yttrium oxide, cerium oxide and lanthanum oxide. The solvent can be, for example, alcohol or acetone. During the ion nitriding process, the rare earth catalyst is continuously brought into the ion nitriding equipment in a gaseous state after the solvent evaporates and through a mass flow meter.
[0046] In the present invention, the nitriding method comprises the following steps: introducing nitriding gas into an ion nitriding device (such as an ion nitriding furnace) to perform ion nitriding treatment on the inner cavity of the annular part located in the ion nitriding device.
[0047] In some embodiments, the following steps may be followed:
[0048] S1. According to the shape and size of the annular part, a protective tool and a cathode disc with uniform holes are made. The above protective tool can completely cover the parts of the annular part that are not allowed to be nitrided, and expose all the inner cavity parts that need to be nitrided. By using the nitriding protective tool, it can be ensured that there is no nitriding layer on the outer surface of the annular part and other positions that are not allowed to be nitrided, and it can also ensure that the nitriding of the inner cavity of the part is not affected. The perforated cathode disc is used in combination with the protective tool to completely expose the inner cavity of the part, so as to better ensure the glow nitriding process and achieve uniform nitriding of the deep inner cavity.
[0049] S2. Ultrasonic cleaning of the annular parts and protective tooling, dehydration and placing in an oven for later use; the cathode disk and the auxiliary anode are polished with sandpaper and wiped with alcohol or acetone for later use. For example, the annular parts and protective tooling can be placed in an ultrasonic cleaning machine, ultrasonically treated in an alkaline solution tank and a deionized water tank to remove surface oil stains.
[0050] S3. Place the annular parts and the auxiliary anode loaded in the protective tooling into the ion nitriding equipment opposite to each other, and place the annular parts evenly on the cathode disk in an annular shape. For example, the parts loaded in the protective tooling are evenly placed on the cathode disk in an annular shape, the opening of the protective tooling is aligned with the through hole on the cathode disk, and the inner cavity of the parts is unobstructed; the distance between the auxiliary anode and the upper end surface of the inner cavity of the annular parts is controlled to be 100mm to 300mm, and the area of the auxiliary anode is equivalent to the cathode disk. The distance between each tooling is greater than 5mm, and the spacing is uniform.
[0051] S4. Introduce nitriding gas to perform enhanced ion nitriding treatment on the inner cavity of the annular part.
[0052] In some embodiments, the ion nitriding treatment includes: evacuating the ion nitriding equipment to below 5 Pa, introducing argon and hydrogen for glow cleaning; then introducing nitriding gas, raising the temperature to 400°C to 800°C under the conditions of a nitriding voltage of 500V to 700V and a gas pressure of 300Pa to 700Pa, and keeping the temperature until a preset nitriding layer depth is obtained.
[0053] The nitriding voltage may be 500V, 550V, 600V, 650V or 700V, or any other value within the range of 500V to 700V.
[0054] The nitriding gas pressure may be 300Pa, 350Pa, 400Pa, 450Pa, 500Pa, 550Pa, 600Pa, 650Pa or 700Pa, etc., or any other value within the range of 300Pa to 700Pa.
[0055] The temperature after heating may be 400°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C or 800°C, or any other value within the range of 400°C to 800°C.
[0056] If the nitriding temperature is too low, it is not conducive to the formation of the nitriding layer; if the nitriding temperature is too high, it is not conducive to maintaining the original structure and hardness of the substrate.
[0057] In some embodiments, the temperature may be first raised to about 400° C. within 1 h, and then raised to about 500° C. within 0.5 h to 1 h.
[0058] In some embodiments, the nitriding gas may include nitrogen, hydrogen and a rare earth gas infiltration agent. For example, by volume percentage, the nitriding gas may include 30% to 80% (such as 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75% or 80%) of hydrogen and 0.5% to 10% (such as 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%) of a rare earth gas infiltration agent, and the balance is nitrogen.
[0059] Further, the nitriding gas may also include argon. For example, by volume percentage, the nitriding gas may include 30% to 80% (such as 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75% or 80%) of hydrogen, 2% to 20% (such as 2%, 4%, 6%, 8%, 10%, 12%, 14%, 16%, 18% or 20%) of argon and 0.5% to 10% (such as 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%) of a rare earth catalyst, and the balance is nitrogen.
[0060] If the volume percentage of the rare earth catalyst in the nitriding gas is too low, it is not conducive to the catalytic effect; if the volume percentage of the rare earth catalyst in the nitriding gas is too high, it is not conducive to the continuous progress of ion nitriding.
[0061] The preset depth of the nitriding layer can be set according to different product requirements. For example, in some embodiments, the nitriding layer can be 120 μm to 150 μm; in other embodiments, the nitriding layer can be 10 μm to 20 μm; in other embodiments, the nitriding layer can be 100 μm to 120 μm.
[0062] After nitriding treatment, the furnace is slowly cooled down and the product can be taken out of the furnace.
[0063] In line with the above, the present invention creatively combines the auxiliary anode technology with the gaseous rare earth catalyst, constructs a highly concentrated plasma energy field by setting up the auxiliary anode, and stimulates the rare earth catalyst introduced into the nitriding furnace in gaseous form to release rare earth elements, thereby achieving enhanced ion nitriding. This method realizes the uniform distribution and efficient utilization of rare earth elements on the surface of samples in various regions of the nitriding furnace, so as to maximize its catalytic effect and improve the uniformity of nitriding, which not only helps to increase the thickness and hardness of the nitrided layer, but also optimizes the organizational structure of the nitrided layer, thereby comprehensively improving the quality and efficiency of the nitriding treatment.
[0064] Correspondingly, the present invention also provides an inner cavity nitrided annular component, which is obtained by subjecting the inner cavity of the annular component to ion nitriding treatment using the above-mentioned ion nitriding method.
[0065] In some embodiments, the hardness of the nitrided layer of the inner cavity of the annular component is not less than 800 HV, for example, 800-1200 HV.
[0066] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0067] Example 1
[0068] This embodiment provides a stainless steel annular part with inner cavity nitriding, which is obtained by the following ion nitriding treatment:
[0069] S1. Make protective tooling and cathode discs with uniform holes according to the shape and size of the annular parts.
[0070] The material of the annular part is 0Cr17Ni4Cu4Nb. Multiple through holes are evenly distributed on the surface of the cathode disk along the circumference of the cathode disk. The size of the through hole is larger than the maximum size of the inner cavity of the annular part and smaller than the maximum size of the outer ring of the protective tooling. The aperture of the through hole is 60 mm, the maximum size of the inner cavity of the annular part is 55 mm, and the maximum size of the outer ring of the protective tooling is 65 mm.
[0071] S2. Place the annular parts and protective tooling in an ultrasonic cleaning machine, perform ultrasonic treatment in an alkaline solution tank and a deionized water tank to remove surface oil stains, and place them in an oven after dehydration for later use; polish the cathode disk and auxiliary anode with sandpaper, and wipe them with alcohol or acetone for later use.
[0072] The auxiliary anode is a circular anode made of the same material as the annular part, and the thickness of the auxiliary anode is 3.5 mm. The area of the auxiliary anode is equal to the area of the cathode disk.
[0073] S3. Place the annular part and the auxiliary anode loaded with the protective tooling into the ion nitriding equipment opposite to each other. The annular part is located on the cathode disc, and the auxiliary anode is located above the annular part, and the auxiliary anode is parallel to the annular part. The opening of the protective tooling is aligned with the through hole on the cathode disc, and the inner cavity of the part is unobstructed; the distance between the auxiliary anode and the upper end face of the inner cavity of the annular part is controlled at 200mm. The distance between each tooling is greater than 5mm, and the spacing is uniform.
[0074] S4. Introduce nitriding gas to perform enhanced ion nitriding treatment on the inner cavity of the annular part.
[0075] The ion nitriding treatment includes: evacuating the ion nitriding equipment to below 5Pa, introducing argon and hydrogen (volume is 1:1) for glow cleaning for 60 minutes; then introducing nitriding gas, slowly heating to 500°C (heating time is 1h) under the conditions of nitriding voltage of 600V and gas pressure of 400Pa, and keeping warm for 40h to obtain the preset nitriding layer depth; then slowly cooling down and taking out of the furnace.
[0076] The nitriding gas includes 65% hydrogen, 11% argon and 5% rare earth catalyst by volume, and the balance is nitrogen. The rare earth catalyst is formed by saturated solution of yttrium oxide in alcohol during the ion nitriding process accompanied by the volatilization of alcohol.
[0077] Example 2
[0078] The difference between this embodiment and embodiment 1 is that the material of the annular part is nickel-based alloy Inconel718, the nitriding temperature is 600° C. and the holding time is 20 h.
[0079] Example 3
[0080] The difference between this embodiment and embodiment 1 is that the material of the annular part is titanium alloy TC4, the nitriding temperature is 800° C. and the holding time is 10 hours.
[0081] Example 4
[0082] The difference between this embodiment and embodiment 1 is that the thickness of the auxiliary anode is 2 mm, and the distance between the auxiliary anode and the upper end surface of the inner cavity of the annular component is 100 mm.
[0083] During the ion nitriding treatment, the temperature was slowly raised to 400°C under the conditions of a nitriding voltage of 500V and a gas pressure of 300Pa, and kept at that temperature for 40h to obtain the corresponding nitriding layer depth.
[0084] The nitriding gas includes 30% hydrogen, 20% argon and 10% rare earth catalyst by volume, and the balance is nitrogen. The rare earth catalyst is formed by a saturated solution of cerium oxide in alcohol during the ion nitriding process accompanied by the volatilization of alcohol.
[0085] Example 5
[0086] The difference between this embodiment and embodiment 1 is that the thickness of the auxiliary anode is 5 mm and the distance between the auxiliary anode and the upper end surface of the inner cavity of the annular component is 300 mm.
[0087] During the ion nitriding treatment, the temperature was slowly raised to 700°C under the conditions of a nitriding voltage of 700V and a gas pressure of 700Pa, and kept at that temperature for 40h to obtain the corresponding nitriding layer depth.
[0088] In terms of volume percentage, the nitriding gas includes 80% hydrogen, 2% argon and 0.5% rare earth catalyst, and the balance is nitrogen. The rare earth catalyst is formed by a saturated solution of lanthanum oxide in alcohol during the ion nitriding process accompanied by the volatilization of alcohol.
[0089] Comparative Example 1
[0090] The difference between this comparative example and Example 1 is that the inner cavity of the annular part is ion nitrided only by means of a gaseous rare earth catalyst, and no auxiliary anode is provided.
[0091] Comparative Example 2
[0092] The difference between this comparative example and Example 1 is that the nitriding temperature is 350°C.
[0093] Comparative Example 3
[0094] The difference between this comparative example and Example 1 is that the nitriding gas includes 65% hydrogen, 11% argon and 15% gaseous rare earth catalyst, and the balance is nitrogen.
[0095] Comparative Example 4
[0096] The difference between this comparative example and Example 1 is that the nitriding gas includes 25% hydrogen, 11% argon and 0.2% gaseous rare earth catalyst, and the balance is nitrogen.
[0097] Comparative Example 5
[0098] The difference between this comparative example and Example 1 is that the nitriding gas includes 85% hydrogen, 8% argon and 5% gaseous rare earth catalyst, and the balance is nitrogen.
[0099] Test example
[0100] The nitriding results of the annular parts with inner cavity nitriding prepared in Examples 1 to 5 and Comparative Examples 1 to 5 were compared. Figures 1 to 3 And as shown in Table 1.
[0101] Among them, the hardness of the nitriding layer is tested with reference to "GB / T 4340.1 Metal Vickers hardness test Part 1: Test method", and the brittleness of the nitriding layer is tested with reference to "GB / T 11354 Nitriding layer depth and metallographic structure inspection of steel parts".
[0102] Table 1 Test results
[0103] Nitriding layer hardness / HV Nitriding layer depth / μm Nitriding layer brittleness Example 1 800~1000 120~150 Level 1-2 Example 2 900~1100 10~12 Level 1-2 Example 3 1000~1200 100~120 Level 1-2 Example 4 800~1000 120~150 Level 1-2 Example 5 800~1000 120~150 Level 1-2 Comparative Example 1 500~600 60~75 Level 1-2 Comparative Example 2 300~400 0 / Comparative Example 3 300~400 0 / Comparative Example 4 600~800 60~80 Level 1-2 Comparative Example 5 700~800 40~60 Level 1-2
[0104] Combination Figure 2 As shown in Table 1, the depth of the inner cavity nitriding layer of the 0Cr17Ni4Cu4Nb annular part obtained in Example 1 is 120 μm to 150 μm, the nitriding layer is uniform, the hardness of the nitriding layer is 800 HV to 1000 HV, and the brittleness of the nitriding layer is level 2.
[0105] Combination Figure 3 As shown in Table 1, the depth of the nitriding layer of the inner cavity of the annular part obtained in Example 2 is 10 μm to 12 μm, the nitriding layer is uniform, the hardness of the nitriding layer is 900 HV to 1100 HV, and the brittleness of the nitriding layer is level 2.
[0106] Combination Figure 4 As shown in Table 1, the depth of the nitriding layer in the inner cavity of the annular part obtained in Example 3 is 100 μm to 120 μm, the white bright layer is 20 μm to 30 μm, the nitriding layer is uniform, the hardness of the nitriding layer is 1000 HV to 1200 HV, and the brittleness of the nitriding layer is level 2.
[0107] It can be seen from Table 1 that the auxiliary anode composite gaseous rare earth catalyst enhanced ion nitriding method of the inner cavity of the annular part adopted in the embodiment of the present invention can obtain a fast nitriding rate (corresponding to nitriding time), high hardness, deep and uniform nitriding layer in the inner cavity of 0Cr17Ni4Cu4Nb, Inconel718 and TC4 annular parts, which can meet the wear resistance requirements of the inner cavity of the annular part and improve the service life.
[0108] By comparing Example 1 with Comparative Examples 1 to 5, it can be seen that when the nitriding conditions change, the nitriding effect will be significantly reduced.
[0109] In summary, the ion nitriding method for the inner cavity of an annular part and the solution of the inner cavity nitrided annular part provided by the present invention have at least the following advantages:
[0110] (1) The present invention directly introduces the rare earth catalyst into the ion nitriding furnace in gaseous form, ensuring that the rare earth elements can be evenly distributed in the target area of the part to be nitrided, without being restricted by the sample loading position in the nitriding furnace;
[0111] (2) The present invention constructs an environment that can induce a more intense glow discharge in a specific area through a composite auxiliary anode, and at the same time greatly enhances the bombardment effect of charged particles on the rare earth catalyst, so that the originally stable rare earth catalyst can be effectively decomposed and release active rare earth elements, thereby giving full play to its catalytic effect;
[0112] (3) The method of combining an auxiliary anode and a gaseous rare earth catalyst in the present invention can effectively solve the problem of the thickness and uniformity of the inner cavity of the annular part, significantly reduce the nitriding time, greatly reduce energy consumption, and have obvious energy-saving and environmental protection benefits.
[0113] (4) The present invention adopts nitriding protection tooling to ensure that there is no nitriding layer on the outer surface of the annular part and other positions where nitriding is not allowed, and to ensure that the nitriding of the inner cavity of the part is not affected. The inner cavity of the part is completely exposed by using a perforated cathode disk in combination with the protection tooling, thereby better ensuring the glow nitriding process and achieving uniform nitriding of the deep inner cavity.
[0114] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. An ion nitriding method for the inner cavity of an annular part, characterized in that: The inner cavity of the annular part is ion nitrided by using an auxiliary anode composite gaseous rare earth catalyst; The gaseous rare earth catalyst is formed by a saturated solution containing the rare earth catalyst during ion nitriding accompanied by solvent volatilization, and the rare earth catalyst includes at least one of yttrium oxide, cerium oxide and lanthanum oxide.
2. The ion nitriding method according to claim 1, characterized in that: The nitriding method comprises the following steps: introducing nitriding gas into an ion nitriding device to perform ion nitriding treatment on the inner cavity of an annular part located in the ion nitriding device.
3. The ion nitriding method according to claim 2, characterized in that: The ion nitriding treatment includes: evacuating the ion nitriding equipment to below 5Pa, introducing argon and hydrogen for glow cleaning; then introducing nitriding gas, raising the temperature to 400℃~800℃ under the conditions of nitriding voltage of 500V~700V and gas pressure of 300Pa~700Pa, and keeping the temperature until the preset nitriding layer depth is obtained.
4. The ion nitriding method according to claim 3, characterized in that: The nitriding gas includes nitrogen, hydrogen and gaseous rare earth catalyst; Preferably, the nitriding gas includes 30% to 80% of hydrogen and 0.5% to 10% of a rare earth catalyst by volume, with the remainder being nitrogen.
5. The ion nitriding method according to claim 4, characterized in that: The nitriding gas also includes argon; Preferably, the nitriding gas includes 30% to 80% of hydrogen, 2% to 20% of argon and 0.5% to 10% of a gaseous rare earth catalyst, with the remainder being nitrogen.
6. The ion nitriding method according to any one of claims 2 to 5, characterized in that: The annular part and the auxiliary anode are arranged opposite to each other in the ion nitriding equipment, and the annular part is located on the cathode disk; Preferably, the auxiliary anode is a circular anode made of the same material as the annular part; Preferably, the shortest distance between the auxiliary anode and the end surface of the inner cavity of the annular component is 100 mm to 300 mm.
7. The ion nitriding method according to claim 6, characterized in that: The surface of the cathode disk is provided with a through hole; Preferably, there are multiple through holes, and the multiple through holes are evenly distributed on the surface of the cathode disk along the circumference of the cathode disk; Preferably, the aperture of the through hole is larger than the maximum transverse length of the inner cavity of the annular part; Preferably, the area of the auxiliary anode is equal to the area of the cathode disk.
8. The ion nitriding method according to any one of claims 1 to 5, characterized in that: The material of the annular part includes at least one of stainless steel, nickel-based alloy and titanium alloy.
9. An inner cavity nitrided annular part, characterized in that: The inner cavity nitrided annular component is obtained by subjecting the inner cavity of the annular component to ion nitriding treatment using the ion nitriding method described in any one of claims 1 to 8.
10. The inner cavity nitrided annular component according to claim 9, characterized in that: The hardness of the nitrided layer of the inner cavity of the annular component is not less than 800 HV.
Citation Information
Patent Citations
Novel glow ion nitriding equipment
CN102234756A
Ion nitriding method for titanium alloy
CN111270198A
Cited By
Regulation and control process for nitridation gradient permeable layer of die-casting special-shaped die
CN121137511A
Regulation process of nitrogen gradient permeation layer of die casting special-shaped mold