Nitriding layer for improving corrosion and wear resistance of martensitic stainless steel and preparation method of nitriding layer
Low-temperature and low-pressure nitriding is carried out through a vacuum arc coating machine to form a nitriding layer with nanocrystal structure, solving the problems of unevenness and brittleness of the nitriding layer on the surface of martensitic stainless steel, significantly improving its corrosion and wear resistance and reducing hydrogen Brittle sensitivity.
Patent Information
- Application Number
- CN202410952404.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
AI Technical Summary
Traditional plasma nitriding technology is difficult to form a uniform high-quality nitriding layer on martensite stainless steel, which makes it difficult to coordinate its wear resistance and corrosion resistance, and there are brittleness problems and hydrogen embrittlement sensitivity.
The vacuum arc coating machine is used to perform low-temperature and low-pressure nitriding, and the passivation film on the surface of the stainless steel is removed by bombardment with high-density argon ions, and more electrons are generated by arc discharge to form the expanded martensite αN phase and ε-Fe2- in nanocrystal structure. The nitriding layer of the 3N phase and the γ'-Fe4N phase avoids the accumulation of the brittle phase and the edge-angle effect.
The formation of a uniform surface thickness and high-quality nitriding layer of martensitic stainless steel is achieved, which significantly improves its corrosion and wear resistance, reduces brittleness and avoids hydrogen embrittlement sensitivity. It is suitable for precision parts in marine environments.
Smart Images

Figure CN118910539A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of surface strengthening, and in particular to a nitriding layer for improving the corrosion and wear resistance of martensitic stainless steel and a preparation method thereof. Background Art
[0002] As a key moving parts material, stainless steel is widely used in aerospace, petrochemical, shipbuilding and ocean industries. With the improvement of equipment performance and service durability, the wear resistance and corrosion resistance of stainless steel are facing severe challenges. The corrosion resistance of stainless steel mainly relies on the formation of a dense passivation film on the surface. As the friction amplitude continuously acts on the passivation film on the surface of stainless steel, the passivation film layer is broken, exposing the fresh surface of stainless steel. The corrosion of stainless steel is accelerated under the action of the corrosive medium. At the same time, under the action of shear force, plastic deformation is formed on the surface of stainless steel, thereby aggravating the wear of stainless steel. Surface modification of stainless steel can improve the corrosion and wear resistance of stainless steel, such as vapor deposition coating, thermal diffusion, laser cladding and other technologies, but there are also problems such as weak bonding strength of surface ceramic strengthening coating, poor corrosion resistance of high-temperature nitriding layer, and easy cracking of laser cladding layer.
[0003] As a means of surface strengthening, plasma nitriding has the advantages of clean nitriding gas, high efficiency, small deformation of workpiece, and easy control of physical phase structure. It can efficiently penetrate nitrogen atoms into the surface of stainless steel, and form a high-hardness nitride layer through the interaction of sputtering and deposition, thereby improving the wear resistance of stainless steel. However, when the nitriding temperature exceeds 460°C, chromium nitrides are easily precipitated, resulting in a decrease in the corrosion resistance of stainless steel. At present, low-temperature ion nitriding of austenitic stainless steel can obtain a nitrogen-rich supersaturated austenite nitride layer, which ensures the corrosion resistance of austenitic stainless steel, but pickling and shot peening are required to remove the surface passivation film. Low-temperature nitriding of ferritic stainless steel requires solution annealing pre-treatment. For martensitic stainless steel, nitriding is prone to produce defective structures, and the quality is even more difficult to guarantee. Traditional plasma nitriding not only has an "edge effect" that causes uneven organization and performance of the nitrided layer, but also has arcing and hollow cathode effects, which cause local overtemperature to burn the material surface. At the same time, at a lower temperature, the passivation film on the surface of stainless steel cannot be effectively removed, which hinders the nitriding process and leads to unsatisfactory wear resistance and corrosion resistance of stainless steel. Moreover, plasma nitriding is basically carried out in a hydrogen-containing atmosphere, which is unfavorable to the hydrogen embrittlement sensitivity of ultra-high strength martensitic stainless steel.
[0004] In view of the above-mentioned defects, the inventors of the present invention finally obtained the present invention after a long period of research and practice. Summary of the invention
[0005] The purpose of the present invention is to solve the problems of uneven structure of stainless steel nitriding layer and difficulty in coordinating wear resistance and corrosion resistance caused by traditional nitriding, so as to achieve martensitic stainless steel precision parts with good strength, toughness, wear resistance and corrosion resistance, and provide a nitriding layer for improving the corrosion and wear resistance of martensitic stainless steel and a preparation method thereof.
[0006] In order to achieve the above-mentioned object, the present invention also discloses a nitriding layer for improving the corrosion and wear resistance of martensitic stainless steel, wherein the nitriding layer is a nanocrystalline structure, and the structure of the nitriding layer includes expanded martensite α N Phase, ε-Fe 2-3 A mixed phase of N phase and γ'-Fe4N phase.
[0007] The thickness of the nitriding layer is ≥8 μm.
[0008] The present invention also discloses a method for preparing the nitriding layer for improving the corrosion and wear resistance of martensitic stainless steel, comprising the following steps:
[0009] S1, surface finishing treatment: the martensitic stainless steel substrate is ground and polished, and then degreased and rusted by ultrasonic cleaning in an alcohol solution to obtain a clean surface with a surface roughness Ra less than 1.5 microns;
[0010] S2, Glow Ion Cleaning: Place the clean martensitic stainless steel into a vacuum arc coating machine and heat and evacuate until the background vacuum is less than 1×10 -3 Pa, introduce argon gas, the argon gas flow rate is 400-500sccm, maintain the gas pressure at 3-4Pa, the substrate negative bias voltage is 400V, and perform glow plasma etching cleaning for 10-20min;
[0011] S3, arc-enhanced ion cleaning: adjust the argon flow rate, maintain the working pressure at 2.5-3.5 Pa, turn on the titanium arc target, and close the target front baffle at the same time. The arc current is 80-120A, the anode layer ion source current is 60-100A, the substrate negative bias voltage is 200-400V, and Ti arc discharge is used to assist in enhanced ion etching. The etching time is 20-30min.
[0012] S4, low temperature plasma nitriding: nitrogen and argon are introduced, the nitrogen flow rate is 30-70 sccm, the working pressure is 0.5-4 Pa, the substrate negative bias voltage is 400 V, the nitriding time is 1-5 hours, and a corrosion-resistant and wear-resistant nitriding layer is formed on the surface of the martensitic stainless steel;
[0013] S5, furnace cooling: After nitriding is completed, turn off the heating, vacuum cool to below 50°C, turn off the exhaust system, and take out the sample.
[0014] In the step S2, the vacuum arc coating machine is an ion source-column arc-plane arc composite deposition system.
[0015] In the step S3, the negative bias voltage of the substrate for arc-enhanced ion cleaning is gradually increased from 200V to 400V at a rate of 20V / min.
[0016] In the step S4, the nitriding temperature of the low-temperature plasma nitriding is 350-450° C., the nitriding working gases are nitrogen and argon, and the flow ratio of nitrogen to argon is 1:3.
[0017] In step S4, the self-corrosion current density of the corrosion-resistant nitriding layer obtained is less than 3.0×10 -8 A / cm 2 , microhardness is not less than HV700.
[0018] Compared with the prior art, the present invention has the following beneficial effects: the present invention uses a vacuum arc coating machine to perform low-temperature and low-pressure nitriding on martensitic stainless steel, utilizes high-density argon ion bombardment to efficiently remove the passivation film on the surface of the stainless steel, and uses the arc discharge effect of arc ion plating to generate more electrons. Under the action of gas discharge, the energy and density of nitrogen ions are increased, and the low-temperature, fast and efficient nitriding of stainless steel is achieved, thereby inhibiting the accumulation of brittle phases and forming a high-quality nitriding layer with uniform thickness. The nitriding layer does not contain CrN precipitation phase, and is mainly composed of expanded martensite α N The nanocrystalline structure formed on the surface promotes the diffusion of oxygen elements to form a passivation film, improves the corrosion resistance of stainless steel, and contains a small amount of ε-Fe 2-3 The N phase and γ'-Fe4N phase not only ensure that the nitriding layer has good toughness, but also improve the hardness and wear resistance of stainless steel, thereby significantly improving the corrosion and wear resistance of stainless steel. In addition, the low-temperature, low-pressure, and low-voltage plasma nitriding method does not require the addition of an additional hollow cathode ion source, which avoids the corner effect and arcing problems of parts with complex shapes and effectively reduces the surface brittleness of the nitriding layer. At the same time, the nitriding atmosphere does not contain hydrogen, which improves the hydrogen embrittlement resistance of high-strength stainless steel. The nitriding layer is expected to be used in martensitic stainless steel precision parts in marine environments to improve the corrosion and wear resistance of stainless steel materials and ensure the long-term and stable service of high-end equipment. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 A schematic diagram of a method for preparing a nitriding layer using an arc coating machine according to the present invention;
[0020] Figure 2 XRD spectrum of the corrosion-resistant and wear-resistant nitriding layer in Example 1;
[0021] Figure 3 TEM analysis diagram of the cross-sectional structure of the corrosion-resistant and wear-resistant nitriding layer in Example 1;
[0022] Figure 4is the thickness of the corrosion-resistant and wear-resistant nitriding layer in Example 1;
[0023] Figure 5 The test results of wear performance of Examples 2 to 4 and Comparative Example 1 under dry friction conditions are shown in FIG.
[0024] Figure 6 The corrosion performance test results of Examples 1 to 2 and Comparative Examples 1 to 2 are shown in FIG.
[0025] Figure 7 These are the surface morphologies of Examples 1-2 and Comparative Examples 1-2 after corrosion and wear. DETAILED DESCRIPTION
[0026] The above and other technical features and advantages of the present invention are described in more detail below in conjunction with the accompanying drawings.
[0027] Figure 1 This is a schematic diagram of the method for preparing a corrosion-resistant and wear-resistant nitriding layer in an embodiment. Figure 1 The Ti column arc is turned on to obtain high-density and high-energy nitrogen ions, thereby realizing the preparation of a high-quality nitriding layer of martensitic stainless steel. The martensitic stainless steel material used in the specific implementation is PH13-8Mo martensitic precipitation hardening stainless steel.
[0028] Example 1
[0029] In this embodiment, the method for preparing a nitriding layer for improving the corrosion and wear resistance of martensitic stainless steel comprises the following steps:
[0030] S1, surface finishing treatment: the martensitic stainless steel substrate is ground and polished, and then degreased and rusted by ultrasonic cleaning in an alcohol solution to obtain a clean surface with a surface roughness Ra less than 1.5 microns.
[0031] S2, Glow Ion Cleaning: Place the clean martensitic stainless steel into a vacuum arc coating machine and heat and evacuate until the background vacuum is less than 1×10 -3 Pa, introduce argon gas with a flow rate of 400-500 sccm, maintain the gas pressure at 4 Pa, the substrate negative bias voltage is 400 V, and perform glow plasma etching cleaning for 20 minutes.
[0032] S3, arc enhanced ion cleaning: adjust the argon flow rate, maintain the working gas pressure at 2.8Pa, turn on the metal titanium arc target, and close the target front baffle. The arc current is 100A, the anode layer ion source current is 80A, and the substrate negative bias voltage is gradually increased from 200V to 400V at a rate of 20V / min. The etching time is 30min.
[0033] S4, low-temperature plasma nitriding: nitrogen and argon are introduced, the nitrogen flow rate is 50sccm, the argon flow rate is 150sccm, the working gas pressure is 2.8Pa, the substrate negative bias voltage is 400V, the nitriding temperature is 440℃, the nitriding time is 1 hour, and a corrosion-resistant and wear-resistant nitriding layer is formed on the surface of martensitic stainless steel.
[0034] S5, furnace cooling: After nitriding is completed, turn off the heating, vacuum cool to below 50°C, turn off the exhaust system, and take out the sample.
[0035] The test results show that the hardness of the prepared nitriding layer is 840HV and the wear rate is 7.019×10 -6 mm 3 N -1 m -1 .
[0036] Example 2
[0037] In this embodiment, the method for preparing a nitriding layer for improving the corrosion and wear resistance of martensitic stainless steel comprises the following steps:
[0038] S1, surface finishing treatment: the martensitic stainless steel substrate is ground and polished, and then degreased and rusted by ultrasonic cleaning in an alcohol solution to obtain a clean surface with a surface roughness Ra less than 1.5 microns.
[0039] S2, Glow Ion Cleaning: Place the clean martensitic stainless steel into a vacuum arc coating machine and heat and evacuate until the background vacuum is less than 1×10 -3 Pa, introduce argon gas with a flow rate of 400-500 sccm, maintain the gas pressure at 4 Pa, the substrate negative bias voltage is 400 V, and perform glow plasma etching cleaning for 20 minutes.
[0040] S3, arc enhanced ion cleaning: adjust the argon flow rate, maintain the working gas pressure at 2.8Pa, turn on the metal titanium arc target, and close the target front baffle. The arc current is 100A, the anode layer ion source current is 80A, and the substrate negative bias voltage is gradually increased from 200V to 400V at a rate of 20V / min. The etching time is 30min.
[0041] S4, low-temperature plasma nitriding: nitrogen and argon are introduced, the nitrogen flow rate is 50sccm, the argon flow rate is 150sccm, the working gas pressure is 2.8Pa, the substrate negative bias voltage is 400V, the nitriding temperature is 400℃, the nitriding time is 1 hour, and a corrosion-resistant and wear-resistant nitriding layer is formed on the surface of martensitic stainless steel.
[0042] S5, furnace cooling: After nitriding is completed, turn off the heating, vacuum cool to below 50°C, turn off the exhaust system, and take out the sample.
[0043] The test results show that the hardness of the prepared nitriding layer is 744HV and the wear rate is 8.418×10 -6 mm 3 N -1 m -1 .
[0044] Example 3
[0045] In this embodiment, the method for preparing a nitriding layer for improving the corrosion and wear resistance of martensitic stainless steel comprises the following steps:
[0046] S1, surface finishing treatment: the martensitic stainless steel substrate is ground and polished, and then degreased and rusted by ultrasonic cleaning in an alcohol solution to obtain a clean surface with a surface roughness Ra less than 1.5 microns.
[0047] S2, Glow Ion Cleaning: Place the clean martensitic stainless steel into a vacuum arc coating machine and heat and evacuate until the background vacuum is less than 1×10 -3 Pa, introduce argon gas with a flow rate of 400-500 sccm, maintain the gas pressure at 4 Pa, the substrate negative bias voltage is 400 V, and perform glow plasma etching cleaning for 20 minutes.
[0048] S3, arc enhanced ion cleaning: adjust the argon flow rate, maintain the working gas pressure at 2.8Pa, turn on the metal titanium arc target, and close the target front baffle. The arc current is 100A, the anode layer ion source current is 60A, and the substrate negative bias voltage is gradually increased from 200V to 400V at a rate of 20V / min. The etching time is 30min.
[0049] S4, low-temperature plasma nitriding: nitrogen and argon are introduced, the nitrogen flow rate is 50sccm, the argon flow rate is 150sccm, the working gas pressure is 2.8Pa, the substrate negative bias voltage is 400V, the nitriding temperature is 400℃, the nitriding time is 1 hour, and a corrosion-resistant and wear-resistant nitriding layer is formed on the surface of martensitic stainless steel.
[0050] S5, furnace cooling: After nitriding is completed, turn off the heating, vacuum cool to below 50°C, turn off the exhaust system, and take out the sample.
[0051] The test results show that the wear rate of the prepared nitriding layer is 8.834×10 -6 mm 3 N -1 m -1 , self-corrosion current density I corr 2.2×10 -8 A / cm 2
[0052] Example 4
[0053] In this embodiment, the method for preparing a nitriding layer for improving the corrosion and wear resistance of martensitic stainless steel comprises the following steps:
[0054] S1, surface finishing treatment: the martensitic stainless steel substrate is ground and polished, and then degreased and rusted by ultrasonic cleaning in an alcohol solution to obtain a clean surface with a surface roughness Ra less than 1.5 microns.
[0055] S2, Glow Ion Cleaning: Place the clean martensitic stainless steel into a vacuum arc coating machine and heat and evacuate until the background vacuum is less than 1×10 -3 Pa, introduce argon gas with a flow rate of 400-500 sccm, maintain the gas pressure at 4 Pa, the substrate negative bias voltage is 400 V, and perform glow plasma etching cleaning for 20 minutes.
[0056] S3, arc enhanced ion cleaning: adjust the argon flow rate, maintain the working gas pressure at 2.8Pa, turn on the metal titanium arc target, and close the target front baffle. The arc current is 100A, the anode layer ion source current is 100A, and the substrate negative bias voltage is gradually increased from 200V to 400V at a rate of 20V / min. The etching time is 30min.
[0057] S4, low-temperature plasma nitriding: nitrogen and argon are introduced, the nitrogen flow rate is 50sccm, the argon flow rate is 150sccm, the working gas pressure is 2.8Pa, the substrate negative bias voltage is 400V, the nitriding temperature is 400℃, the nitriding time is 1 hour, and a corrosion-resistant and wear-resistant nitriding layer is formed on the surface of martensitic stainless steel.
[0058] S5, furnace cooling: After nitriding is completed, turn off the heating, vacuum cool to below 50°C, turn off the exhaust system, and take out the sample.
[0059] The test results show that the wear rate of the prepared nitriding layer is 7.37×10 -6 mm 3 N -1 m -1 , self-corrosion current density I corr 0.8×10 -8 A / cm 2 .
[0060] Comparative Example 1
[0061] This embodiment is a comparative example of Example 1, and no nitriding treatment is performed on the surface of the martensitic stainless steel.
[0062] Comparative Example 2
[0063] This embodiment is used as a comparative example of Embodiment 1. Steps S1, S2, S3 and S5 are exactly the same as those of Embodiment 1. In step S4, the nitriding temperature is 510° C., and other parameters are the same as those of Embodiment 1.
[0064] Figure 2 This is the XRD analysis diagram of the corrosion-resistant nitriding layer of Example 1. It can be seen that the nitriding layer is mainly composed of expanded martensite α N phase, and ε-Fe 2-3 N phase and γ'-Fe4N phase.
[0065] Figure 3 This is a TEM analysis of the cross-sectional structure of the corrosion-resistant nitriding layer of Example 1. The nitriding layer contains expanded martensite α N Phase, ε-Fe 2-3 N phase and γ'-Fe4N phase, and the relevant results are consistent with the XRD analysis.
[0066] Figure 4 It is the thickness of the corrosion-resistant and wear-resistant nitriding layer of Example 1. It can be clearly seen that the thickness of the nitriding layer is 9.07 μm. Compared with the core structure, the nitriding layer has no obvious metallographic corrosion morphology, and the corrosion resistance of the surface nitriding layer is better than that of the stainless steel substrate.
[0067] Comparative Example and Comparative Example were tested as follows:
[0068] Figure 5 The figure is a test result of the wear performance of Examples 2 to 4 and Comparative Example 1 under dry friction conditions. It can be seen that compared with the untreated martensitic precipitation hardened stainless steel of Comparative Example 1, the wear amount of Examples 2 to 4 under dry friction conditions is reduced by nearly 3 orders of magnitude, indicating that the wear resistance of the stainless steel treated with nitriding is significantly improved.
[0069] Figure 6 The corrosion performance test results of Example 1-2 and Comparative Example 1-2 are shown in FIG. The self-corrosion current density I of Example 1 and Example 2 in NaCl solution (3.5 wt.%) is corr 0.60×10 -8 A / cm 2 and 1.90×10 -8 A / cm 2 , self-corrosion potential E corr The corrosion resistance of the nitrided layer is significantly better than that of the untreated martensitic precipitation hardening stainless steel (8.50×10 -8 A / cm 2 , -0.14V / SCE). However, at the higher nitriding temperature in Example 2, the corrosion resistance of martensitic stainless steel decreased significantly (9.13×10 -7 A / cm 2 , -0.33V / SCE).
[0070] Figure 7The surface morphology of Example 1-2 and Comparative Example 1-2 after friction and corrosion wear with titanium alloy in NaCl solution shows that the corrosion wear width of the nitrided layer prepared at low temperature is narrow, and a small amount of Ti and O elements are detected on the wear scar surface, indicating that the wear is mainly abrasive wear, accompanied by some adhesive wear and oxidation wear. A large amount of wear debris adheres to the wear scar of the martensitic stainless steel sample in Comparative Example 1, and some wear scars are in the shape of plowing furrows, which are the characteristics of abrasive wear, while corrosion occurs in the wear scar area of the martensitic stainless steel sample in Comparative Example 2 after high-temperature nitriding, which reduces the wear resistance and corrosion resistance of the stainless steel.
[0071] The above description is only a preferred embodiment of the present invention, which is only illustrative and not restrictive of the present invention. Those skilled in the art understand that many changes, modifications, and even equivalences may be made to the present invention within the spirit and scope defined by the claims of the present invention, but all of them will fall within the scope of protection of the present invention.
Claims
1. A method for improving the corrosion and wear resistance of martensitic stainless steel nitriding layer, It is characterized in that The nitriding layer has a nanocrystalline structure, and the structure of the nitriding layer includes expanded martensite α N Phase, ε-Fe 2-3 N phase and γ'-Fe 4 Mixed phase of N phase.
2. A nitriding layer for improving the corrosion and wear resistance of martensitic stainless steel as claimed in claim 1, It is characterized in that The thickness of the nitriding layer is ≥8 μm.
3. A method for preparing a nitrided layer for improving the corrosion and wear resistance of martensitic stainless steel as claimed in claim 1 or 2, It is characterized in that The following steps are involved: S1, surface finishing treatment: the martensitic stainless steel substrate is ground and polished, and then degreased and rusted by ultrasonic cleaning in an alcohol solution to obtain a clean surface with a surface roughness Ra less than 1.5μm; S2, Glow Ion Cleaning: Place the clean martensitic stainless steel into a vacuum arc coating machine and heat and evacuate until the background vacuum is less than 1×10 -3 Pa, introduce argon gas, the argon gas flow rate is 400-500sccm, maintain the gas pressure at 3-4Pa, the substrate negative bias voltage is 400V, and perform glow plasma etching cleaning for 10-20min; S3, arc-enhanced ion cleaning: adjust the argon flow rate, maintain the working pressure at 2.5-3.5 Pa, turn on the titanium arc target, and close the target front baffle at the same time. The arc current is 80-120A, the anode layer ion source current is 60-100A, the substrate negative bias voltage is 200-400V, and Ti arc discharge is used to assist in enhanced ion etching. The etching time is 20-30min. S4, low temperature plasma nitriding: nitrogen and argon are introduced, the nitrogen flow rate is 30-70 sccm, the working pressure is 0.5-4 Pa, the substrate negative bias voltage is 400 V, the nitriding time is 1-5 hours, and a corrosion-resistant and wear-resistant nitriding layer is formed on the surface of the martensitic stainless steel; S5, furnace cooling: After nitriding is completed, turn off the heating, vacuum cool to below 50°C, turn off the exhaust system, and take out the sample.
4. A method for preparing a nitrided layer for improving the corrosion and wear resistance of martensitic stainless steel as claimed in claim 3, It is characterized in that In the step S2, the vacuum arc coating machine is an ion source-column arc-plane arc composite deposition system.
5. A method for preparing a nitrided layer for improving the corrosion and wear resistance of martensitic stainless steel as claimed in claim 3, It is characterized in that In the step S3, the negative bias voltage of the substrate for arc-enhanced ion cleaning is increased from 200 V to 400 V at a rate of 20 V / min.
6. A method for preparing a nitrided layer for improving the corrosion and wear resistance of martensitic stainless steel as claimed in claim 3, It is characterized in that In the step S4, the nitriding temperature of the low-temperature plasma nitriding is 350-450° C., the nitriding working gases are nitrogen and argon, and the flow ratio of nitrogen to argon is 1:
3.
7. A method for preparing a nitrided layer for improving the corrosion and wear resistance of martensitic stainless steel as claimed in claim 3, It is characterized in that In step S4, the self-corrosion current density of the corrosion-resistant nitriding layer obtained is less than 3.0×10 -8 A / cm 2 , microhardness is not less than HV700.
Citation Information
Cited By
Preparation method of high-strength corrosion-resistant nitriding layer on surface of ferritic stainless steel
CN121428468A