Chromium-nickel co-permeation coating as well as preparation method and application thereof

The preparation method of chromium-nickel co-diffusion coating solves the problems of poor coating adhesion and small thickness in the existing technology, and realizes high efficiency, wide applicability and excellent corrosion resistance of metal workpieces.

CN118910541AActive Publication Date: 2024-11-08HUANENG HUNAN YUEYANG POWER GENERATION CO LTD +1

Patent Information

Application Number
CN202410975833.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

Existing co-diffusion technology for metal workpieces suffers from poor coating adhesion, small thickness, the need for multiple coatings, and a narrow range of applications. Furthermore, it is prone to increased porosity and brittleness in metal workpieces such as high-carbon steel and high-alloy steel, which affects performance.

Method used

The preparation method of chromium-nickel co-diffusion coating includes surface pretreatment, shot peening treatment and one-time coating of chromium-nickel co-diffusion slurry. The coating components include chromium powder, nickel powder, alumina, chromium oxide, etc., and a dense coating is formed through a segmented gradient curing process.

Benefits of technology

It achieves good adhesion between the coating and the substrate, eliminates the need for multiple coatings, is suitable for various metal workpieces, improves resistance to high and low temperature corrosion and steam oxidation, and extends the coating life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910541A_ABST
    Figure CN118910541A_ABST
Patent Text Reader

Abstract

The invention provides a chromium-nickel co-permeation coating and a preparation method and application thereof. The preparation method comprises the following steps: carrying out surface pretreatment on a metal workpiece; the pretreated metal workpiece is subjected to shot blasting treatment; the surface of the metal workpiece subjected to shot blasting treatment is coated with the chromium-nickel co-permeation slurry at a time, and a chromium-nickel co-permeation coating is obtained on the surface of the metal workpiece through drying, curing and sintering treatment; wherein the chromium-nickel co-permeation slurry comprises a solid phase component and a liquid phase component; the solid phase component comprises chromium powder, nickel powder, aluminum oxide and chromium oxide, and the liquid phase component comprises Al (H2PO4) 3, water glass, ammonium iodide, chromium oxide and magnesium oxide. The coating is suitable for various metal workpieces with the surfaces needing to be strengthened, the metal workpieces comprise carbon steel workpieces, austenitic stainless steel workpieces, high-temperature alloy workpieces and the like, the application range is wide, the practicability is extremely high, the coating has very high adhesiveness, and the high and low temperature corrosion resistance and the steam oxidation resistance of the metal workpieces can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of material surface coatings, and in particular relates to a chromium-nickel co-penetration coating and a preparation method and application thereof. Background Art

[0002] The most commonly used anti-corrosion method for metal workpieces is to cover the metal surface with a metal, non-metal or metal-non-metal composite film as a protective layer through physical, chemical or electrochemical metal surface treatment processes to prevent or slow down the chemical reaction between the metal and the contact medium. Related metal surface treatment technologies include thermal spraying, electroplating, thermal diffusion, surface phosphating, metal or non-metal coating, etc., which can improve the surface performance, corrosion resistance and wear resistance of the workpiece, and extend the service life of the workpiece by constructing a coating on the workpiece surface to change the composition, organization and structure of the material surface.

[0003] Among them, thermal diffusion technology is a process that uses heating and diffusion to make the metal or non-metallic elements to be infiltrated penetrate into the surface of the metal workpiece, thereby forming a surface alloy layer. Co-infiltration is the most widely used treatment process of thermal diffusion technology. Through one heating and diffusion, multiple elements are infiltrated into the surface of the workpiece at the same time. The emergence of co-infiltration absorbs the advantages of various unit infiltrations, and makes up for the shortcomings of unit infiltration through the coordination of elements, so that the workpiece surface can obtain better comprehensive performance.

[0004] At present, there are co-penetration mainly based on metal elements, co-penetration mainly based on non-metallic elements and co-penetration of rare earths. For example, aluminum-chromium co-penetration is performed on the surface of high-temperature alloy workpieces to form an element coating of a dense oxide film. The stable physical and chemical properties of its oxide under high temperature conditions are used to improve the service life of the workpiece. However, most of the current co-penetration of metal workpieces adopts a solid method, which requires a combination of multiple metal elements and components such as catalysts. The co-penetration time is long and the experimental requirements are high. In addition, the formed coating has poor adhesion and small thickness. Multiple coatings are required to achieve the required thickness, and the scope of application is narrow. Especially for metal workpieces such as high-carbon steel and high-alloy steel, in the process of element diffusion, due to the different diffusion rates of Cr or Al and Fe, there is a Kirkendall effect of atomic diffusion. The diffusion of Cr or Al is accompanied by the appearance of voids, resulting in a large number of pores in the coating, the coating is not dense, the brittleness increases, and it may even cause the coating to fall off, seriously affecting the performance. Secondly, there is also a gas method, in which aluminum oxide, chromium powder, aluminum powder and ammonium chloride are used to form an aluminum-chromium co-penetration agent, and the chromium-aluminum co-penetration agent and parts are placed in a crucible, and heated under an argon atmosphere to obtain parts containing an aluminum-chromium coating. This method needs to be carried out in a vacuum environment and the preparation process needs to be strictly controlled. In addition, there is also a neutral salt bath chromium-aluminum co-penetration method, in which sodium chloride, barium chloride, sodium fluoride, aluminum powder and chromium powder are used to form a co-penetration agent, and the co-penetration agent is loaded into a crucible, and the crucible containing the salt bath chromium-aluminum co-penetration agent is placed in a resistance furnace for heating, and then the sample is placed in the prepared chromium-aluminum co-penetration salt bath so that the main working surface of the sample is kept as perpendicular to the flow direction of the salt bath as possible, and the oil quenching is taken out after 4 hours of heat preservation, that is, a chromium-aluminum co-penetration layer is obtained on the surface of the nickel-based high-temperature alloy. This method has a long heat preservation time and high requirements on the placement of the sample. The thickness of the coating formed is thin, only about 20μm, and the corrosion and wear resistance is poor. Summary of the invention

[0005] The present disclosure aims to solve at least one of the technical problems existing in the prior art and to provide a chromium-nickel co-penetration coating and a preparation method and application thereof.

[0006] In one aspect of the present disclosure, a method for preparing a chromium-nickel co-penetration coating is provided.

[0007] The preparation method comprises:

[0008] Surface pretreatment of metal workpieces;

[0009] Shot peening is performed on the pretreated metal workpiece;

[0010] The chromium-nickel co-penetration slurry is coated once on the surface of the metal workpiece after shot peening, and then dried, solidified and sintered to obtain a chromium-nickel co-penetration coating on the surface of the metal workpiece; wherein,

[0011] The chromium-nickel co-diffusion slurry includes a solid phase component and a liquid phase component; the solid phase component includes chromium powder, nickel powder, aluminum oxide and chromium oxide, and the liquid phase component includes Al(H2PO4)3, water glass, ammonium iodide, chromium oxide and magnesium oxide.

[0012] Optionally, the solid-liquid ratio of the solid phase component to the liquid phase component is 10:(1-5).

[0013] Optionally, the solid phase components include, by mass percentage:

[0014] 50-80% chromium powder;

[0015] 1-10% nickel powder;

[0016] 10-20% alumina;

[0017] 0-20% chromium oxide;

[0018] The sum of the mass percentages of the above solid phase components is 100%.

[0019] Optionally, the chromium powder, nickel powder, aluminum oxide and chromium oxide are ball-milled at a rotation speed of 350 to 400 r / min for 6 to 24 hours to obtain a solid phase component.

[0020] Optionally, the liquid phase components include, by mass percentage:

[0021] 10-30% Al(H2PO4)3;

[0022] 15-25% water glass;

[0023] 5-10% ammonium iodide;

[0024] 10-40% chromium oxide;

[0025] 15-35% magnesium oxide;

[0026] The sum of the mass percentages of the above liquid phase components is 100%.

[0027] Optionally, the coating thickness of the chromium-nickel co-diffusion slurry coated on the surface of the metal workpiece is 0.1 to 1.0 mm.

[0028] Optionally, in the shot peening treatment, the diameter of the shot peening particles is 0.1 to 1.0 mm, the shot peening pressure is 0.5 to 2.0 MPa, and the shot peening time is 10 to 30 min.

[0029] Optionally, the metal workpiece coated with the chromium-nickel co-diffusion slurry is dried, solidified, and sintered, including:

[0030] Pre-dry the metal workpiece coated with the chromium-nickel co-diffusion slurry at 60-85°C for 5-30 minutes, then dry at 100-160°C for 30-60 minutes, and finally cure at 250-300°C for 20-60 minutes;

[0031] The dried and solidified metal workpiece is sintered at 500-650°C for 5-30 minutes.

[0032] Another aspect of the present disclosure provides a chromium-nickel co-penetration coating, which is prepared according to the preparation method described above.

[0033] Another aspect of the present disclosure provides an application of a chromium-nickel co-diffusion coating, wherein the chromium-nickel co-diffusion coating described above is applied to the surface of a metal workpiece of carbon steel, austenitic steel and high-temperature alloy.

[0034] The present disclosure provides a chromium-nickel co-penetration coating and its preparation method and application. The preparation method includes: performing surface pretreatment on a metal workpiece; performing shot peening on the pretreated metal workpiece; applying the chromium-nickel co-penetration slurry once on the surface of the metal workpiece after the shot peening, drying, curing and sintering to obtain a chromium-nickel co-penetration coating on the surface of the metal workpiece; the chromium-nickel co-penetration slurry includes a solid phase component and a liquid phase component; the solid phase component includes chromium powder, nickel powder, aluminum oxide and chromium oxide, and the liquid phase component includes Al(H2PO4)3, water glass, ammonium iodide, chromium oxide and magnesium oxide. The coating is suitable for various metal workpieces whose surfaces need to be strengthened, including carbon steel, austenitic stainless steel and high-temperature alloy workpieces, with a wide range of applications and strong practicality. The coating has strong adhesion and can further improve the high and low temperature corrosion resistance and steam oxidation resistance of the metal workpiece. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 It is a flowchart of a method for preparing a chromium-nickel co-penetration coating according to an embodiment of the present disclosure;

[0036] Figure 2 This is an electron microscope image of the chromium-nickel co-diffusion coating prepared in Example 3 of the present disclosure. DETAILED DESCRIPTION

[0037] In order to enable those skilled in the art to better understand the technical solution of the present disclosure, the present disclosure is further described in detail below in conjunction with the accompanying drawings and specific implementation methods. Obviously, the described embodiments are part of the embodiments of the present disclosure, rather than all of the embodiments. Based on the described embodiments of the present disclosure, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present disclosure.

[0038] like Figure 1As shown, in one aspect of the present disclosure, a method for preparing a chromium-nickel co-penetration coating is provided S100, which specifically includes the following steps S110 to S130:

[0039] S110, performing surface pretreatment on the metal workpiece.

[0040] Specifically, organic reagents such as alcohol or acetone are used to clean the oil stains and dust on the surface of the metal workpiece. At the same time, the oxide scale on the surface of the metal workpiece can be removed by using a steel brush, sandpaper or polishing.

[0041] It should be noted that the present embodiment does not specifically limit the material and type of the metal workpiece, for example, it can be a high temperature alloy metal workpiece, various types of carbon steel metal workpieces, or austenitic steel metal workpieces. Of course, such metal workpieces can be pipeline workpieces, turbine blades in the aviation field, or other types of workpieces.

[0042] S120, performing shot peening on the pretreated metal workpiece.

[0043] Specifically, during the shot peening process, shot peening particles are sprayed at high speed onto the surface of the metal workpiece to cause its surface to undergo plastic deformation, forming a strengthening layer of a certain thickness, wherein the shot peening particle diameter is 0.1 to 1.0 mm, the shot peening pressure is 0.5 to 2.0 MPa, and the shot peening time is 10 to 30 min.

[0044] In this embodiment, by activating the surface of the metal workpiece, the physical properties and bonding strength of the metal workpiece such as surface adhesion, roughness, and specific surface area are improved, which is beneficial to increase the adhesion of the subsequent penetration coating, further improve the penetration effect of the subsequent co-penetration coating, and make the coating thickness thicker.

[0045] S130, coating the chromium-nickel co-diffusion slurry once on the surface of the metal workpiece after shot peening, and obtaining a chromium-nickel co-diffusion coating on the surface of the metal workpiece through drying, curing and sintering.

[0046] It should be noted that the present embodiment does not specifically limit the method of coating the chromium-nickel co-diffusion slurry on the surface of the metal workpiece. For example, the chromium-nickel co-diffusion slurry is coated on the surface of the metal workpiece by spraying or brushing.

[0047] It should be further explained that the chromium-aluminum co-diffusion coating currently prepared is relatively thin, and multiple coatings are required to increase the thickness of the coating, and the stability is poor. However, the present embodiment does not require multiple coatings, and only one coating process can achieve the required thickness, and the coating thickness can be adjusted according to actual needs.

[0048] Specifically, in the coating process of this embodiment, the chrome-nickel co-penetration slurry is coated to a suitable thickness at one time, without the need for multiple layered coatings, wherein the coating thickness of the chrome-nickel co-penetration slurry is 0.1 to 1.0 mm. In other words, in this embodiment, the chrome-nickel co-penetration slurry is coated on the surface of the metal workpiece at one time to form a layer of chrome-nickel co-penetration coating, and the thickness of the chrome-nickel co-penetration coating is 0.1 to 1.0 mm. Within the above thickness range, the applicability of the metal workpiece itself can be guaranteed, and the high-temperature corrosion resistance of the metal workpiece can also be improved.

[0049] In some preferred embodiments, the slurry coating thickness of the chromium-nickel co-diffusion coating is 0.1 mm, 0.2 mm, 0.3 mm, 0.4 mm, 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, 1.0 mm, etc.

[0050] It should be understood that the service life of the coating is not only related to the thickness of the coating, but also has a certain correlation with the material of the coating itself and its bonding with the substrate. Most of the current coatings are chromium-aluminum coatings, which mix chromium powder, aluminum powder, and some chloride powders together. They need to go through a complex pretreatment process such as grinding, calcination, and cooling to obtain a co-penetrating agent, which is then applied to the surface of the workpiece. Since the co-penetrating agent is composed of powder, this method has a complicated processing process for the co-penetrating agent, and the bonding force between the coating and the workpiece is weak, and the coating is easy to fall off. In view of this, the chromium-nickel co-penetrating slurry of this embodiment includes not only a solid phase component, but also a liquid phase component to reduce the pretreatment process of the co-penetrating agent.

[0051] Specifically, the chromium-nickel co-diffusion slurry includes a solid phase component and a liquid phase component; the solid phase component includes chromium powder, nickel powder, aluminum oxide and chromium oxide, and the liquid phase component includes Al(H2PO4)3, water glass, ammonium iodide, chromium oxide and magnesium oxide.

[0052] In this embodiment, the liquid phase component is mixed with the solid phase component to improve the adhesion between the chromium-nickel co-diffusion slurry and the workpiece, thereby avoiding the coating from falling off. There is no need to perform a complicated pretreatment process on the solid phase component, thereby simplifying the slurry preparation process.

[0053] In other preferred embodiments, the solid-to-liquid ratio (g:mL) of the solid phase component to the liquid phase component is 10:(1-5).

[0054] In other preferred embodiments, the liquid phase components include, by mass percentage: 10-30% Al(H2PO4)3; 15-25% water glass; 5-10% ammonium iodide; 10-40% chromium oxide; and 15-35% magnesium oxide.

[0055] Among them, in the liquid phase components, Al(H2PO4)3 and water glass are used as binders, and the bonding strength between them and the metal substrate is high, and the coating thickness required for preparing the coating can be achieved in one coating treatment; secondly, in the process of drying the slurry, Al(H2PO4)3 and water glass can be directly decomposed without producing harmful gases, which can avoid the formation of bubbles inside the coating, thereby making the structure inside the coating layer dense and free of pores; and the above-mentioned binder component has good high-temperature toughness and is not easy to crack during the drying process.

[0056] Furthermore, in the liquid phase component, ammonium iodide is used as a penetration aid to form active transition halide gas, which accelerates the penetration rate of active chromium atoms and nickel atoms into the matrix.

[0057] Furthermore, in the liquid phase component, magnesium oxide is used as a curing agent to dehydrate and polycondense the acid phosphate in the binder, which can effectively reduce the curing and film-forming temperature of the slurry. At the same time, adding an appropriate amount of chromium oxide can reduce the curing reaction speed of magnesium oxide and the binder, preventing problems such as cracks on the surface of the cured coating and failure to form a film due to too fast a curing speed.

[0058] As a further preferred embodiment, the content of Al(H2PO4)3 is preferably 10%, 15%, 20%, 25%, 30%, the content of water glass is preferably 15%, 20%, 25%, the content of ammonium iodide is preferably 5%, 7%, 10%, the content of chromium oxide is preferably 10%, 15%, 20%, 28%, 35%, 40%, and the content of magnesium oxide is preferably 15%, 25%, 30%, 35%.

[0059] In other preferred embodiments, the solid phase components include, by mass percentage: 50-80% chromium powder; 1-10% nickel powder; 10-20% aluminum oxide; 0-20% chromium oxide.

[0060] Among them, in the solid phase components, alumina and chromium oxide are used as fillers, which can effectively prevent the adhesion between chromium powder and nickel powder and between chromium powder, nickel powder and the matrix during the slurry preparation process, resulting in uneven diffusion layer; secondly, adding a small amount of nickel can increase the chromization speed, reduce the chromization temperature, and reduce the adverse effects of heat treatment on the comprehensive mechanical properties of the matrix while achieving the required diffusion layer thickness.

[0061] It is worth noting that the chromium and nickel elements in this embodiment are respectively infiltrated into the base metal, and the chromium and nickel infiltrated into the base can also form intermetallic compounds with the base respectively. Compared with a single chromizing coating, the chromium-nickel co-infiltrating layer has better wear resistance and corrosion resistance.

[0062] As a further preferred embodiment, the chromium powder content is preferably 50%, 60%, 70%, 80%, the nickel powder content is preferably 1%, 5%, 10%, the aluminum oxide content is preferably 10%, 15%, 20%, and the chromium oxide content is preferably 1%, 5%, 12%, 15%, 20%.

[0063] In other preferred embodiments, chromium powder, nickel powder, aluminum oxide and chromium oxide are ball-milled in a star-shaped ball mill to obtain a solid phase component. The ball milling speed is 350-400 r / min and the ball milling time is 6-24 hours. By ball-milling the mixed metal powders and then mixing them with the liquid phase components, it is beneficial to mix the components evenly.

[0064] Furthermore, the metal workpiece coated with the chromium-nickel co-diffusion slurry is dried, solidified and sintered, including the following specific steps:

[0065] The metal workpiece coated with the chromium-nickel co-diffusion slurry is pre-dried at a low temperature of 60 to 85°C for 5 to 30 minutes, then dried at a low temperature of 100 to 160°C for 30 to 60 minutes, and finally cured at a medium temperature of 250 to 300°C for 20 to 60 minutes;

[0066] The dried and solidified metal workpiece is sintered at 500-650°C for 5-30 minutes.

[0067] In some preferred embodiments, the low-temperature pre-drying temperature is preferably 60°C, 70°C, or 80°C, and the time is preferably 5 min, 10 min, 15 min, 20 min, 25 min, or 30 min.

[0068] In other preferred embodiments, the temperature of low-temperature drying is preferably 100°C, 120°C, 140°C, 150°C, 160°C, and the time is preferably 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, 60 min.

[0069] In other preferred embodiments, the medium-temperature curing temperature is preferably 250°C, 260°C, 270°C, 280°C, 290°C, 300°C, and the time is preferably 20 min, 30 min, 40 min, 50 min, 60 min.

[0070] In other preferred embodiments, the sintering temperature is preferably 500°C, 550°C, 600°C, 650°C, and the sintering time is preferably 5 min, 10 min, 15 min, 20 min, 25 min, 30 min.

[0071] In this embodiment, by adopting a segmented gradient curing process, it is ensured that the co-infiltration slurry will not have surface quality problems due to local stress during the curing process. At the same time, it is beneficial to increase the adhesion of the co-infiltration slurry, improve the coating effect, shorten the curing time, and reduce energy consumption.

[0072] The preparation method of the chromium-nickel co-diffusion coating of this embodiment is simple, does not need to be carried out under vacuum conditions, has high production efficiency, and has little pollution during the production process. The chromium-nickel co-diffusion coating formed based on the above components has good bonding with the substrate, effectively preventing the coating from falling off during use, thereby achieving the purpose of extending the life of the coating. In addition, the chromium-nickel co-diffusion coating has a wide range of applications and strong practicality. It is not only suitable for high-temperature alloys, but also can be applied to various types of carbon steels and other metal workpieces such as austenitic steel.

[0073] Another aspect of the present disclosure provides a chromium-nickel co-penetration coating, which is prepared according to the preparation method described above.

[0074] In this embodiment, the chromium-nickel co-diffusion coating formed on various metal workpieces has a thickness of 5-50 μm. The coating corresponding to this thickness has good adhesion to the surface of the metal workpiece and also has excellent resistance to high and low temperature corrosion and steam oxidation.

[0075] Another aspect of the present disclosure provides an application of a chromium-nickel co-diffusion coating, wherein the chromium-nickel co-diffusion coating described above is applied to the surface of a metal workpiece of carbon steel, austenitic steel and high-temperature alloy.

[0076] The preparation method of the chromium-nickel co-penetration coating will be further described below in conjunction with several specific examples:

[0077] Example 1

[0078] This example uses a large boiler pipe made of carbon steel as the metal workpiece to be processed. The pipe specifications are 55mm in outer diameter, 8mm in wall thickness, and 4000mm in length. The surface chromium-nickel treatment is performed on the metal workpiece, including the following steps:

[0079] S1. Pipeline surface cleaning:

[0080] Use alcohol / acetone to clean the surface oil stains, dust, etc. of the pipeline workpiece, and use a steel brush to remove the surface oxide scale.

[0081] S2. Surface shot peening treatment:

[0082] The cleaned pipe workpiece is shot peened with a shot peening particle diameter of 0.3 mm, a shot peening pressure of 0.5 MPa, and a shot peening time of 10 min.

[0083] S3. Surface slurry coating

[0084] Use spraying (brushing or other methods are also possible) to apply the chromium-nickel co-diffusion slurry to a thickness of 0.5 mm at one time. Do not apply it in layers multiple times.

[0085] Among them, the preparation method of the chromium-nickel co-penetration slurry is as follows: according to the mass percentage of the solid phase components, 70% of chromium powder, 5% of nickel powder, 15% of aluminum oxide and 10% of chromium oxide are weighed respectively, and the mixed metal mixed powder is ball-milled at a ball milling speed of 350r / min and a ball milling time of 8h to obtain the final solid phase component. According to the mass percentage of the liquid phase component, 25% of Al(H2PO4)3, 18% of water glass, 7% of ammonium iodide, 15% of chromium oxide and 35% of magnesium oxide are measured and mixed to obtain the liquid phase component. The solid phase component and the liquid phase component are mixed at a solid-liquid (g:ml) ratio of 10:2 to obtain the final metal powder coating raw material.

[0086] S4, drying and curing

[0087] Using a segmented gradient curing process, the metal pipe workpiece coated with chromium-nickel material is pre-dried at 75°C for 5 minutes, then dried at 140°C for 55 minutes, and finally cured at 250°C for 30 minutes.

[0088] S5, fast sintering

[0089] The metal pipe workpiece is rapidly sintered, diffused and chromized by rapid heating, and then air-cooled to room temperature; the heating rate is set to 1000°C / min, the holding temperature is 500°C, and the holding time is 30min, to obtain a chromium-nickel co-diffusion coating coated on the metal pipe workpiece.

[0090] In this Example 1, the obtained chromium-nickel co-penetration coating was subjected to an oxidation resistance test, as follows: After cyclic oxidation at 500°C for 100 hours, the oxidation weight gain of the prepared chromium-nickel co-penetration coating sample was 0.15 mg / mm 2 The oxidation weight gain of carbon steel matrix is ​​1.47mg / mm 2 , the oxidation rate decreased by 89.8%.

[0091] In this embodiment 1, the obtained chromium-nickel co-penetration coating was subjected to a wear resistance test, specifically as follows: under the test conditions of a load of 10g and a holding time of 10s, the microhardness of the prepared chromium-nickel co-penetration coating was about 412HV, and the microhardness of the carbon steel substrate was about 320HV, which was about 1.3 times higher. Secondly, in accordance with the national standard GB / T 12444-2006 "Metallic Material Wear Test Method", this embodiment 1 tested the wear resistance of carbon steel and the coating. Under the same test conditions, the friction and wear of the coating sample was reduced by about 21.7%, and the friction coefficient was reduced by about 6.8%.

[0092] Example 2

[0093] This example uses a large boiler pipe made of austenitic steel as the metal workpiece to be processed. The specifications of the pipe are 55mm in outer diameter, 8mm in wall thickness, and 4000mm in length. The surface chromium-nickel treatment is performed on the metal pipe workpiece, including the following steps:

[0094] S1. Pipeline surface cleaning:

[0095] Use alcohol / acetone to clean the surface oil stains, dust, etc. of the pipeline workpiece, and use a steel brush to remove the surface oxide scale.

[0096] S2. Surface shot peening treatment:

[0097] The cleaned pipe workpiece is shot peened with a shot peening particle diameter of 0.5 mm, a shot peening pressure of 1.0 MPa, and a shot peening time of 10 min.

[0098] S3. Surface slurry coating

[0099] Use spraying (brushing or other methods are also possible) to apply the chromium-nickel co-diffusion slurry to a thickness of 0.5 mm at one time. Do not apply it in layers multiple times.

[0100] Among them, the preparation method of the chromium-nickel co-diffusion slurry is as follows: according to the mass percentage of the solid phase components, 75% of chromium powder, 3% of nickel powder, 10% of aluminum oxide and 12% of chromium oxide are weighed respectively, and the mixed metal mixed powder is ball-milled at a ball milling speed of 350r / min and a ball milling time of 10h to obtain the final solid phase component. According to the mass percentage of the liquid phase component, 30% of Al(H2PO4)3, 25% of water glass, 10% of ammonium iodide, 20% of chromium oxide and 15% of magnesium oxide are measured and mixed to obtain the liquid phase component. The solid phase component and the liquid phase component are mixed at a solid-liquid (g:ml) ratio of 10:3 to obtain the final metal powder coating raw material.

[0101] S4, drying and curing

[0102] Using a segmented gradient curing process, the metal pipe workpiece coated with chromium-nickel material was pre-dried at 85°C for 5 minutes, then dried at 160°C for 55 minutes, and finally cured at 300°C for 30 minutes.

[0103] S5, fast sintering

[0104] The metal pipe workpiece is rapidly sintered, diffused and chromized by rapid heating, and then air-cooled to room temperature; the heating rate is set to 1000°C / min, the holding temperature is 550°C, and the holding time is 30min, to obtain a chromium-nickel co-diffusion coating coated on the metal pipe workpiece.

[0105] In Example 2, the obtained chromium-nickel co-penetration coating was subjected to an oxidation resistance test, as follows: After cyclic oxidation at 650°C for 100 hours, the oxidation weight gain of the prepared chromium-nickel co-penetration coating sample was 0.000078 mg / mm 2 The oxidation weight gain of the stainless steel matrix is ​​0.0047 mg / mm 2 , the oxidation rate decreased by 98.3%.

[0106] In Example 2, the obtained chromium-nickel co-penetration coating was subjected to a wear resistance test, as follows: under the test conditions of a load of 10 g and a holding time of 10 s, the microhardness of the prepared chromium-nickel co-penetration coating was about 400 HV, and the microhardness of the austenitic steel substrate was about 190 HV, which was about 2.1 times higher. Secondly, in accordance with the national standard GB / T 12444-2006 "Metallic Material Wear Test Method", the wear resistance of austenitic steel and the coating was tested. Under the same test conditions, the friction and wear of the coating sample was reduced by about 39%, and the friction coefficient was reduced by about 13%.

[0107] Example 3

[0108] This example uses a large boiler pipe made of high-temperature alloy as the metal workpiece to be processed. The pipe specifications are 55mm in outer diameter, 8mm in wall thickness, and 4000mm in length. The surface chromium-nickel treatment is performed on the metal pipe workpiece, including the following steps:

[0109] S1. Pipeline surface cleaning:

[0110] Use alcohol / acetone to clean the surface oil stains, dust, etc. of the pipeline workpiece, and use a steel brush to remove the surface oxide scale.

[0111] S2. Surface shot peening treatment:

[0112] The cleaned pipe workpiece is shot peened with a shot peening particle diameter of 0.5 mm, a shot peening pressure of 1.5 MPa, and a shot peening time of 15 min.

[0113] S3. Surface slurry coating

[0114] Use spraying (brushing or other methods are also possible) to apply the chromium-nickel co-diffusion slurry to a thickness of 1.0 mm at one time. Do not apply it in layers multiple times.

[0115] Among them, the preparation method of the chromium-nickel co-penetration slurry is as follows: according to the mass percentage of the solid phase components, 60% of chromium powder, 5% of nickel powder, 20% of aluminum oxide and 15% of chromium oxide are weighed respectively, and the mixed metal mixed powder is ball-milled at a ball milling speed of 350r / min and a ball milling time of 12h to obtain the final solid phase component. According to the mass percentage of the liquid phase component, 25% of Al(H2PO4)3, 20% of water glass, 5% of ammonium iodide, 35% of chromium oxide and 15% of magnesium oxide are measured and mixed to obtain the liquid phase component. The solid phase component and the liquid phase component are mixed at a solid-liquid (g:ml) ratio of 10:5 to obtain the final metal powder coating raw material.

[0116] S4, drying and curing

[0117] Using a segmented gradient curing process, the metal pipe workpiece coated with chromium-nickel material is pre-dried at 80°C for 10 minutes, then dried at 150°C for 30 minutes, and finally cured at 300°C for 20 minutes.

[0118] S5, fast sintering

[0119] The metal pipe workpiece is rapidly sintered, diffused and chromized by a rapid heating method, and then air-cooled to room temperature; the heating rate is set to 1000°C / min, the holding temperature is 650°C, and the holding time is 20min, to obtain a chromium-nickel co-diffusion coating coated on the metal pipe workpiece.

[0120] In Example 3, the obtained chromium-nickel co-penetration coating was subjected to an oxidation resistance test, as follows: After cyclic oxidation at 1000°C for 100 h, the oxidation weight gain of the prepared chromium-nickel co-penetration coating sample was 0.012 mg / mm 2 The oxidation weight gain of the high-temperature alloy matrix is ​​0.108 mg / mm 2 , the oxidation rate decreased by 88.9%.

[0121] In this embodiment 3, the wear resistance test of the obtained chromium-nickel co-penetration coating is carried out, and the specific results are as follows: the microhardness of the prepared chromium-nickel co-penetration coating is about 437HV, and the microhardness of the high-temperature alloy substrate is about 300HV, and the hardness thereof is increased by about 1.5 times. Secondly, in this embodiment 3, the wear resistance of the high-temperature alloy and the coating is tested in accordance with the national standard GB / T 12444-2006 "Metallic Material Wear Test Method", and under the same test conditions, the friction and wear of the coating sample is reduced by about 20.3%, and the friction coefficient is reduced by about 6.8%.

[0122] like Figure 2As shown, the chromium-nickel co-penetration coating obtained in Example 3 has a thickness of about 31 μm, and the average chromium content and nickel content are 35 wt.% and 6 wt.%, respectively. The co-penetration coating has a uniform and dense structure, has no obvious defects inside, and has good metallurgical bonding with the substrate.

[0123] Example 4

[0124] This example uses a large boiler pipe made of high-temperature alloy as the metal workpiece to be processed. The pipe specifications are 55mm in outer diameter, 8mm in wall thickness, and 4000mm in length. The surface chromium-nickel treatment is performed on the metal pipe workpiece, including the following steps:

[0125] S1. Pipeline surface cleaning:

[0126] Use alcohol / acetone to clean the surface oil stains, dust, etc. of the pipeline workpiece, and use a steel brush to remove the surface oxide scale.

[0127] S2. Surface shot peening treatment:

[0128] The cleaned pipe workpiece is shot peened with a shot peening particle diameter of 0.1 mm, a shot peening pressure of 1.0 MPa, and a shot peening time of 20 min.

[0129] S3. Surface slurry coating

[0130] Use spraying (brushing or other methods are also possible) to apply the chromium-nickel co-diffusion slurry to a thickness of 0.8mm at one time. Do not apply it in layers multiple times.

[0131] Among them, the preparation method of the chromium-nickel co-penetration slurry is as follows: according to the mass percentage of the solid phase components, 70% of chromium powder, 5% of nickel powder, 10% of aluminum oxide and 15% of chromium oxide are weighed respectively, and the mixed metal mixed powder is ball-milled at a ball milling speed of 400r / min and a ball milling time of 24h to obtain the final solid phase component. According to the mass percentage of the liquid phase component, 20% of Al(H2PO4)3, 15% of water glass, 7% of ammonium iodide, 28% of chromium oxide and 30% of magnesium oxide are measured and mixed to obtain the liquid phase component. The solid phase component and the liquid phase component are mixed at a solid-liquid (g:ml) ratio of 10:5 to obtain the final metal powder coating raw material.

[0132] S4, drying and curing

[0133] Using a segmented gradient curing process, the metal pipe workpiece coated with chromium-nickel material was pre-dried at 60°C for 5 minutes, then dried at 100°C for 55 minutes, and finally cured at 250°C for 30 minutes.

[0134] S5, fast sintering

[0135] The metal pipe workpiece is rapidly sintered, diffused and chromized by rapid heating, and then air-cooled to room temperature; the heating rate is set to 1000°C / min, the holding temperature is 500°C, and the holding time is 30min, to obtain a chromium-nickel co-diffusion coating coated on the metal pipe workpiece.

[0136] In Example 4, the obtained chromium-nickel co-penetration coating was subjected to an oxidation resistance test, as follows: After cyclic oxidation at 1000°C for 100 h, the oxidation weight gain of the prepared chromium-nickel co-penetration coating sample was 0.033 mg / mm 2 The oxidation weight gain of the high-temperature alloy matrix is ​​0.108 mg / mm 2 , the oxidation rate decreased by 69.4%.

[0137] In Example 4, the wear resistance test of the obtained chromium-nickel co-penetration coating was carried out, and the details are as follows: the microhardness of the prepared chromium-nickel co-penetration coating is about 419.6HV, and the microhardness of the high-temperature alloy substrate is about 300HV, and the hardness thereof is increased by about 1.4 times. Secondly, in accordance with the national standard GB / T 12444-2006 "Metallic Material Wear Test Method", the wear resistance of the high-temperature alloy and the coating was tested. Under the same test conditions, the friction and wear of the coating sample was reduced by about 18.3%, and the friction coefficient was reduced by about 6.2%.

[0138] The present disclosure provides a chromium-nickel co-penetration coating and a preparation method and application thereof, which have the following beneficial effects compared with the prior art:

[0139] First, the chromium-nickel high-temperature corrosion-resistant coating and its preparation method disclosed in the present invention do not need to be carried out under vacuum conditions, and the preparation process is simple. At the same time, the chromium-nickel co-penetration coating has high preparation efficiency, low pollution, adjustable thickness, good wear resistance, and especially excellent resistance to high and low temperature corrosion and steam oxidation;

[0140] Second, the present invention mixes the solid phase component with the liquid phase component to form a chromium-nickel co-diffusion slurry, which is easy to coat the surface of the metal workpiece and has a strong bonding force with the workpiece surface.

[0141] Third, the metal powder raw material disclosed in the present disclosure is suitable for various metal workpieces whose surfaces need to be strengthened, including carbon steel, austenitic stainless steel, and high-temperature alloy workpieces, and has a wide range of applications and strong practicality;

[0142] Fourthly, the present invention also undergoes a shot peening process before the co-penetration coating to increase the specific surface area of ​​the metal workpiece, improve the penetration of metal elements and the adhesion of the coating, thereby further enhancing the strength and anti-corrosion performance of the surface coating.

[0143] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present disclosure, but the present disclosure is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and substance of the present disclosure, and these modifications and improvements are also considered to be within the scope of protection of the present disclosure.

Claims

1. A method for preparing a chromium-nickel co-penetration coating, characterized in that: The preparation method comprises: Surface pretreatment of metal workpieces; Shot peening is performed on the pretreated metal workpiece; The chromium-nickel co-penetration slurry is coated once on the surface of the metal workpiece after shot peening, and then dried, solidified and sintered to obtain a chromium-nickel co-penetration coating on the surface of the metal workpiece; wherein, The chromium-nickel co-diffusion slurry includes a solid phase component and a liquid phase component; the solid phase component includes chromium powder, nickel powder, aluminum oxide and chromium oxide, and the liquid phase component includes Al(H2PO4)3, water glass, ammonium iodide, chromium oxide and magnesium oxide.

2. The preparation method according to claim 1, characterized in that: The solid-to-liquid ratio of the solid phase component to the liquid phase component is 10:(1-5).

3. The preparation method according to claim 1, characterized in that: In terms of mass percentage, the solid phase components include: 50-80% chromium powder; 1-10% nickel powder; 10-20% alumina; 0-20% chromium oxide; The sum of the mass percentages of the above solid phase components is 100%.

4. The preparation method according to claim 3, characterized in that: The chromium powder, the nickel powder, the aluminum oxide and the chromium oxide are ball-milled for 6 to 24 hours at a rotation speed of 350 to 400 r / min to obtain a solid phase component.

5. The preparation method according to claim 1, characterized in that: In terms of mass percentage, the liquid phase components include: 10-30% Al(H2PO4)3; 15-25% water glass; 5-10% ammonium iodide; 10-40% chromium oxide; 15-35% magnesium oxide; The sum of the mass percentages of the above liquid phase components is 100%.

6. The preparation method according to any one of claims 1 to 5, characterized in that: The coating thickness of the chromium-nickel co-diffusion slurry coated on the surface of the metal workpiece is 0.1 to 1.0 mm.

7. The preparation method according to any one of claims 1 to 5, characterized in that: In the shot peening treatment, the diameter of the shot peening particles is 0.1 to 1.0 mm, the shot peening pressure is 0.5 to 2.0 MPa, and the shot peening time is 10 to 30 minutes.

8. The preparation method according to any one of claims 1 to 5, characterized in that: The metal workpiece coated with the chromium-nickel co-diffusion slurry is subjected to drying, curing and sintering treatment, including: Pre-dry the metal workpiece coated with the chromium-nickel co-diffusion slurry at 60-85°C for 5-30 minutes, then dry at 100-160°C for 30-60 minutes, and finally cure at 250-300°C for 20-60 minutes; The dried and solidified metal workpiece is sintered at 500-650°C for 5-30 minutes.

9. A chromium-nickel co-penetration coating, characterized in that: The chromium-nickel co-penetration coating is prepared by the preparation method according to any one of claims 1 to 8.

10. An application of a chromium-nickel co-penetration coating, characterized in that: The chromium-nickel co-diffusion coating described in claim 9 is applied to the surface of a metal workpiece made of carbon steel, austenitic steel or high-temperature alloy.

Citation Information

Patent Citations

  • Method for preparing SiAl coating by sintering slurry

    CN102312188A

  • Method for preparing hollow blade inner chamber diffusion layer with high temperature resistance, oxidation resistance and corrosion resistance

    CN102485934A

  • Preparation method of chromium-enriched high-temperature corrosion resisting coating deposited through slurry method

    CN109881145A

  • Aluminum-chromium co-permeation protective coating and preparation method and application thereof

    CN110923621A

  • Rare earth reinforced high-temperature aluminizing slurry and coating preparation method thereof

    CN114540748A

Cited By

  • Preparation method of slurry-method chromium-nickel co-permeation coating of liquid-phase multi-component binder

    CN119824364A