Island-shaped nickel oxide nanosheet array electrochromic film oriented to multiple scenes and preparation method and application of island-shaped nickel oxide nanosheet array electrochromic film
Through magnetron sputtering technology and rapid annealing treatment, an island-shaped nickel oxide nanosheet array electrochromic film was prepared, which solved the shortcomings of nickel oxide film in optical modulation and response speed, and achieved high-performance electricity in multiple scenarios Discoloration effect.
Patent Information
- Application Number
- CN202410966856.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-18
AI Technical Summary
The existing nickel oxide electrochromic films have shortcomings in optical modulation range, response speed and multi-scene application capabilities, and it is difficult to achieve high optical modulation, high response speed and multi-scene application capabilities at the same time.
Magneto-controlled sputtering technology is used to deposit nickel oxide nanosheet array film on the substrate surface and process it in a rapid annealing device to obtain an island-shaped nickel oxide nanosheet array electrochromic film for multiple scenes, with a uniform island structure and (111) The crystal surface is optimally oriented, improving electrochromic performance.
High optical modulation amplitude and rapid reversible changes in the 550nm band are achieved, and are suitable for multi-scenario environments, including potassium hydroxide and lithium ion electrolyte environments, simplifying the process flow and reducing costs.
Smart Images

Figure CN118910545A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of electrochromic films, and in particular to an island-shaped nickel oxide nanosheet array electrochromic film for multiple scenarios, and a preparation method and application thereof. Background Art
[0002] Electrochromic phenomenon refers to the phenomenon that the color of a material changes reversibly under an external electric field. Due to the huge application prospects of electrochromic materials in the fields of stealth materials and smart color-changing films, they have attracted more and more attention in recent years. The preparation of electrochromic films with a high optical modulation range and application in multiple scenarios is the current research focus.
[0003] Nickel oxide is a typical inorganic electrochromic material, which has the characteristics of low price and simple preparation method, but its slow color change speed, poor cycle stability and low conductivity will also affect its performance in practical applications. For example: CN113277744B discloses a method for regulating the morphology of nickel oxide electrochromic film with solvent, and obtains nickel oxide with various morphologies, and the modulation range of the prepared film is only 20% to 80%; CN115745418A discloses a fast-response nickel oxide electrochromic film and its preparation method and application, with a coloring and fading time of 3.5s and 1.5s, but an optical modulation range of 69.4% to 92%; CN107382091B discloses a method for preparing a nickel oxide electrochromic film, and the optical modulation range of the film obtained by inkjet technology is only 23% to 59%. CN112456813B discloses a nickel oxide electrochromic film and its preparation method and application, which has a preferred orientation of (111) and can improve the storage capacity of lithium ions, but requires a higher sputtering temperature and cumbersome subsequent annealing treatment. The resulting optical modulation amplitude is 37%, and it has no ability in alkaline electrolyte scenarios.
[0004] From the above, we can see that the film obtained by the existing magnetron technology is very dense, which hinders the rapid diffusion of ions. At the same time, it is difficult to directly obtain a three-dimensional porous spatial structure, which makes it difficult for the internal components to deeply participate in the reaction. + The color-changing ability in electrolyte and KOH is limited; although other technical means such as hydrothermal can obtain a relatively high optical modulation range in KOH, the process is cumbersome and the reactions are numerous, making it difficult to achieve large-area uniform growth of the film. The most critical disadvantage is that it is difficult to grow the film in Li due to the presence of impurities in the water phase or precursor. + Therefore, it is difficult for existing technologies to simultaneously achieve high optical modulation, high response speed and multi-scenario application capabilities of nickel oxide films. Summary of the invention
[0005] The purpose of the present invention is to provide an island-shaped nickel oxide nanosheet array electrochromic film for multiple scenarios, and a preparation method and application thereof, which simultaneously improves the optical modulation range and fading response time of the nickel oxide electrochromic film, obtains application functions in multiple scenarios, and meets the application requirements for the next generation of high-performance electrochromic devices, wherein multiple scenarios refer to multiple electrolyte environments, including potassium hydroxide electrolyte environments and lithium ion electrolyte environments.
[0006] In one aspect of the present invention, the present invention proposes a method for preparing an island-shaped nickel oxide nanosheet array electrochromic film for multiple scenarios. According to an embodiment of the present invention, the method comprises the following steps:
[0007] (1) Using magnetron sputtering technology, pure Ni target is used as cathode target material, inert gas Ar and reactive gas O2 are used as working gas, and nickel oxide nanosheet array thin film is deposited on the substrate surface;
[0008] (2) placing the nickel oxide nanosheet array film in a rapid annealing device, heating it to 100° C. at a heating rate of 5 to 10° C. / min in an air atmosphere, and keeping it warm for 5 to 30 minutes. After natural cooling, taking it out, and obtaining an island-shaped nickel oxide nanosheet array electrochromic film for multiple scenarios.
[0009] In addition, the method for preparing a multi-scenario island nickel oxide nanosheet array electrochromic film according to the above embodiment of the present invention may also have the following additional technical features:
[0010] In some embodiments of the present invention, in step (1), the sputtering method of the magnetron sputtering technology is direct current sputtering or radio frequency sputtering.
[0011] In some embodiments of the present invention, in step (1), the substrate temperature is 25-100°C, and the vacuum degree of the reaction chamber is 0.8×10 -4 ~1.2×10 -4 Pa, the sputtering gas pressure is 0.5-3.0 Pa, the proportion of sputtered oxygen is 0.25-0.75, the sputtering power density is 25-75 W, and the deposition time is 10-40 min.
[0012] In some embodiments of the present invention, in step (2), the thickness of the multi-scenario island-shaped nickel oxide nanosheet array electrochromic film is 150 to 300 nm.
[0013] In another aspect of the present invention, the present invention proposes an island-shaped nickel oxide nanosheet array electrochromic film for multiple scenarios prepared according to the method for preparing the island-shaped nickel oxide nanosheet array electrochromic film for multiple scenarios.
[0014] In addition, the multi-scenario island-shaped nickel oxide nanosheet array electrochromic film according to the above embodiment of the present invention may also have the following additional technical features:
[0015] In some embodiments of the present invention, the multi-scenario island-shaped nickel oxide nanosheet array electrochromic film exhibits a uniform island structure with gaps between islands. Each island exhibits a nano-prism-like morphology and exhibits a strong (111) crystal plane preferred orientation. A large amount of active reaction area can be exposed during the electrochromic process, and the (111) crystal plane orientation can provide a large amount of trivalent nickel (Ni in the XPS spectrum). 3+ / Ni 2+ The value of is 3.93), and the (111) crystal plane is conducive to the adsorption of Li ions. The combined effect of the two can improve the electrochromic performance.
[0016] At 550nm, the transmittance of the faded state is 94.0%, the transmittance of the colored state is 8.8%, the optical modulation amplitude is 85.2%, it is almost transparent when faded, and almost completely shielded when colored, the coloring and fading response times are 3.8s and 2.6s respectively, which can achieve rapid reversible changes between transparent and dark brown. At 1000nm in the near-infrared band, it has an optical modulation range of 50.4%.
[0017] In Li + Under electrolyte, in the 550nm band, the optical modulation amplitude is 35.3%, showing good application potential in multiple scenarios.
[0018] In another aspect of the present invention, the present invention proposes an application of an island-shaped nickel oxide nanosheet array electrochromic film for multiple scenarios. According to an embodiment of the present invention, the island-shaped nickel oxide nanosheet array electrochromic film for multiple scenarios is used to prepare an electrochromic device.
[0019] In another aspect of the present invention, the present invention proposes an application of an island-shaped nickel oxide nanosheet array electrochromic film for multiple scenarios. According to an embodiment of the present invention, the island-shaped nickel oxide nanosheet array electrochromic film for multiple scenarios is used to prepare smart display materials and smart color-changing energy storage materials.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] 1. The multi-scenario island-shaped nickel oxide nanosheet array electrochromic film of the present invention has a uniform island structure with gaps between islands. Each island exhibits a nano-prism-like morphology, which can effectively increase the electrochemical active area, improve the electron transmission speed and ion diffusion rate, accelerate the reaction kinetics process, and greatly improve the coloring efficiency of the electrochromic material;
[0022] 2. The multi-scenario island-shaped nickel oxide nanosheet array electrochromic film of the present invention has an obvious (111) crystal plane preferred orientation. A large number of (111) crystal planes are conducive to the adsorption of Li ions, while also bringing a high proportion of high-valent metal ions Ni 3+ , which enhances OH - The chemical adsorption promotes electron transfer and has a good kinetic promotion effect. + It has good electrochromic performance in both electrolyte and alkaline electrolyte;
[0023] 3. The multi-scenario island-shaped nickel oxide nanosheet array electrochromic film of the present invention has excellent electrochromic control performance in multiple scenarios. At a wavelength of 550nm, the transmittance of the faded state is 94.0%, the transmittance of the colored state is 8.8%, and the optical modulation amplitude is 85.2%. It can achieve rapid and reversible transformation between transparent and dark brown under different applied voltages. In the near-infrared 1000nm band, it also has an optical modulation range of 50.4%; in Li + Under electrolyte, in the 550nm band, the optical modulation amplitude is 35.3%, showing good application potential in multiple scenarios;
[0024] 4. The one-step magnetron sputtering method used in the present invention has simple steps, easy equipment operation, good repeatability, short production cycle, low process cost, and is conducive to large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a scanning electron microscope morphology image of the multi-scenario island-shaped nickel oxide nanosheet array electrochromic film prepared in Example 1 of the present invention;
[0026] Figure 2 This is a scanning electron microscope morphology image of the multi-scenario island-shaped nickel oxide nanosheet array electrochromic film prepared in Example 2 of the present invention;
[0027] Figure 3 This is a cross-sectional morphology image of a scanning electron microscope of an island-shaped nickel oxide nanosheet array electrochromic film for multiple scenarios prepared in Example 1 of the present invention;
[0028] Figure 4 This is a cross-sectional morphology image of a multi-scenario island-shaped nickel oxide nanosheet array electrochromic film prepared in Example 2 of the present invention, taken under a scanning electron microscope;
[0029] Figure 5 This is an X-ray electron diffraction pattern of the island-shaped nickel oxide nanosheet array electrochromic film for multiple scenarios prepared in Example 1 of the present invention;
[0030] Figure 6The cyclic voltammogram of the multi-scenario island-shaped nickel oxide nanosheet array electrochromic film prepared in Example 1 of the present invention;
[0031] Figure 7 The cyclic voltammogram of the multi-scenario island-shaped nickel oxide nanosheet array electrochromic film prepared in Example 2 of the present invention;
[0032] Figure 8 The Ni 2p spectrum of the X-ray photoelectron spectrum of nickel element in the multi-scenario island-shaped nickel oxide nanosheet array electrochromic thin film prepared in Example 1 of the present invention;
[0033] Fig. 9 The O1s energy spectrum of the X-ray photoelectron spectrum of nickel element in the multi-scenario island-shaped nickel oxide nanosheet array electrochromic thin film prepared in Example 1 of the present invention;
[0034] Fig.10 This is a spectrum diagram of the electrochromic performance of the multi-scenario island-shaped nickel oxide nanosheet array electrochromic film prepared in Example 1 of the present invention in a 1 mol / L KOH electrolyte solution;
[0035] Fig.11 This is a spectrum diagram of the electrochromic performance of the multi-scenario island-shaped nickel oxide nanosheet array electrochromic film prepared in Example 2 of the present invention in a 1 mol / L KOH electrolyte solution;
[0036] Fig.12 Schematic diagram of the kinetic electrochromic performance of the multi-scenario island-shaped nickel oxide nanosheet array electrochromic film prepared in Example 1 of the present invention in a 1 mol / L KOH electrolyte solution (550 nm ± 1.0 V);
[0037] Fig.13 Schematic diagram of the kinetic electrochromic performance of the multi-scenario island-shaped nickel oxide nanosheet array electrochromic film prepared in Example 2 of the present invention in a 1 mol / L KOH electrolyte solution (550 nm ± 1.0 V);
[0038] Fig.14 This is a spectrum of electrochromic performance of the multi-scenario island-shaped nickel oxide nanosheet array electrochromic film prepared in Example 1 of the present invention in a 1 mol / L LiClO4 / PC electrolyte solution;
[0039] Fig.15 This is a spectrum of electrochromic performance of the multi-scenario island-shaped nickel oxide nanosheet array electrochromic film prepared in Example 2 of the present invention in a 1 mol / L LiClO4 / PC electrolyte solution;
[0040] Fig.16 Schematic diagram of the kinetic electrochromic performance of the multi-scenario island-shaped nickel oxide nanosheet array electrochromic film prepared in Example 1 of the present invention in a 1 mol / L LiClO4 / PC electrolyte solution (550nm±1.5V);
[0041] Fig.17 Schematic diagram of the kinetic electrochromic performance of the multi-scenario island-shaped nickel oxide nanosheet array electrochromic film prepared in Example 2 of the present invention in a 1 mol / L LiClO4 / PC electrolyte solution (550nm±1.5V);
[0042] Fig.18 These are optical photographs of the initial state (a, d), faded state (b, e) and colored state (c, f) of the island-shaped nickel oxide nanosheet array electrochromic film for multiple scenarios prepared in Example 1 and Example 2 of the present invention. DETAILED DESCRIPTION
[0043] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0044] Embodiment 1
[0045] A method for preparing an island-shaped nickel oxide nanosheet array electrochromic film for multiple scenarios, the specific steps are as follows:
[0046] (1) Using magnetron sputtering technology, pure Ni target was used as cathode target material, inert gas Ar and reactive gas O2 were used as working gas, and nickel oxide nanosheet array thin film was deposited on the surface of FTO conductive glass. The sputtering method was DC sputtering, the substrate temperature was 25°C, and the vacuum degree of the reaction chamber was 1.0×10 -4 Pa, the sputtering gas pressure is 1.0 Pa, the sputtering oxygen ratio is 0.25, the sputtering power density is 50 W, and the deposition time is 25 min.
[0047] (2) The nickel oxide nanosheet array film is placed in a rapid annealing device, heated to 100°C at a heating rate of 2°C / min in an air atmosphere, and kept warm for 25 minutes. After natural cooling, it is taken out to obtain an island-shaped nickel oxide nanosheet array electrochromic film for multiple scenarios, with a cross-sectional thickness of approximately 150 nm.
[0048] The nickel oxide nano-array electrochromic material prepared in this embodiment has an island nanosheet array structure. Figure 1 and Figure 3 As shown, the high-resolution scanning image shows a uniform island structure with gaps between islands, and each island exhibits a nanoprism-like morphology. Figure 5 The X-ray electron diffraction pattern shows a clear (111) crystal plane orientation and no peaks from other crystal planes.
[0049] The cyclic voltammetry curves, spectra and kinetics of the island-shaped nickel oxide nanosheet array electrochromic film for multiple scenarios were tested as follows:
[0050] The electrochemical and electrochromic properties of the samples were recorded using an electrochemical workstation (CHI 760E) and a UV-Vis-NIR spectrophotometer (UV-3600, Japan) in a three-electrode system (the electrochromic film on the FTO conductive glass substrate was the working electrode, Ag / AgCl was the reference electrode, platinum wire was the counter electrode, and 1 mol / L KOH and 1 mol / L LiClO4 / PC solutions were the alkaline electrolyte and lithium ion electrolyte, respectively). To ensure that the light path was unobstructed, the reference electrode and the counter electrode were placed on one side of the working electrode, and the reference electrode and the counter electrode were placed on the other side.
[0051] Cyclic voltammetry curves were recorded at different scan rates in an alkaline electrolyte over a voltage range of -1.0 V to +1.0 V. At the same time, transmittance spectra were recorded over a wavelength range of 300 to 1300 nm at the corresponding applied voltage (±1.0 V). The kinetic profiles of the thin film samples were recorded by applying square wave voltages of -1.0 V (20 sec) and +1.0 V (20 sec) at 550 nm.
[0052] Cyclic voltammetry curves were recorded at different scan rates in a lithium-ion electrolyte over a voltage range of -1.5 V to +1.5 V. At the same time, transmittance spectra were recorded over a wavelength range of 300 to 1300 nm at the corresponding applied voltages (±1.5 V). Kinetic profiles of thin film samples were recorded by applying square wave voltages of -1.5 V (20 sec) and +1.5 V (20 sec) at 550 nm.
[0053] Figure 6 In the cyclic voltammogram, the curve does not have an obvious deformation trend with the increase of scan rate, showing good reversibility. Figure 8 and Fig. 9 The photoelectron spectrum proves that the trivalent peak area of nickel element is large, which promotes the kinetic process and is conducive to the electrochromic reaction.
[0054] The electrochromic performance spectra, kinetics spectra and optical photographs of the electrochromic devices prepared in this example under alkaline electrolytes are shown in Figure 2. Fig.10 , Fig.12 , Fig.18This electrochromic material can achieve an optical modulation contrast ratio of 85.2% and 50.4% at 550nm and 1000nm, respectively, with a coloring time of 3.8s and a fading time of 2.6s at 550nm.
[0055] The electrochromic performance spectrum and kinetic spectrum of the electrochromic material prepared in this embodiment under lithium ion electrolyte are as follows: Fig.14 and Fig.16 This electrochromic material can achieve an optical modulation contrast ratio of 35.3% and 17.3% at 550nm and 1000nm, respectively, with a coloring time of 5.8s and a fading time of 1.4s at 550nm.
[0056] The initial optical photograph of the film prepared in this example and the photographs of the faded state and the colored state in the alkaline electrolyte are shown in FIG. Fig.18 a, b, and c. The high transmittance in the faded state and the low transmittance in the colored state show a strong visual contrast, and the brown-black color as a neutral color during color development can also meet the needs of commercial applications.
[0057] Embodiment 2
[0058] A method for preparing an island-shaped nickel oxide nanosheet array electrochromic film for multiple scenarios, the specific steps are as follows:
[0059] (1) Using magnetron sputtering technology, pure Ni target was used as cathode target material, inert gas Ar and reactive gas O2 were used as working gas, and nickel oxide nanosheet array thin film was deposited on the surface of FTO conductive glass. The sputtering method was DC sputtering, the substrate temperature was 25°C, and the vacuum degree of the reaction chamber was 1.0×10 -4 Pa, the sputtering gas pressure is 1.0 Pa, the sputtering oxygen ratio is 0.25, the sputtering power density is 50 W, and the deposition time is 50 min.
[0060] (2) The nickel oxide nanosheet array film is placed in a rapid annealing device, heated to 100°C at a heating rate of 5°C / min in an air atmosphere, and kept warm for 30 minutes. After natural cooling, it is taken out to obtain an island-shaped nickel oxide nanosheet array electrochromic film for multiple scenarios, with a cross-sectional thickness of approximately 300 nm.
[0061] The nickel oxide nano-array electrochromic material prepared in this embodiment has an island nanosheet array structure. Figure 2 and Figure 4 As shown, the high-resolution scanning image shows a uniform island structure with gaps between islands, and each island exhibits a nanoprism-like morphology.
[0062] The testing method of the cyclic voltammetry curve, spectrum diagram and kinetic diagram of the island-shaped nickel oxide nanosheet array electrochromic film for multiple scenarios in this embodiment is the same as that in Example 1. Figure 7 The curve in the cyclic voltammogram does not show obvious deformation trend with the increase of scanning rate, showing good reversibility. The electrochromic performance spectrum and kinetic spectrum of the electrochromic performance prepared in this embodiment under alkaline electrolyte are as follows: Fig.11 , Fig.13 This electrochromic material can achieve an optical modulation contrast ratio of 80.1% and 63.4% at 550nm and 1000nm, respectively, with a coloring time of 6.0s and a fading time of 5.8s at 550nm.
[0063] The electrochromic performance spectrum and kinetic spectrum of the electrochromic material prepared in this embodiment under lithium ion electrolyte are as follows: Fig.15 and Fig.17 This electrochromic material can achieve an optical modulation contrast ratio of 52.7% and 31.9% at 550nm and 1000nm, respectively, with a coloring time of 2.4s and a fading time of 1.4s at 550nm.
[0064] The initial optical photograph of the film prepared in this example and the photographs of the faded state and the colored state in the alkaline electrolyte are shown in FIG. Fig.18 d, e, and f. The high transmittance in the faded state and the low transmittance in the colored state show a strong visual contrast, and the brown-black color as a neutral color during color development can also meet the needs of commercial applications.
[0065] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the present invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A method for preparing an island-shaped nickel oxide nanosheet array electrochromic film for multiple scenarios, characterized in that: The following steps are involved: (1) Using magnetron sputtering technology, pure Ni target is used as cathode target material, inert gas Ar and reactive gas O2 are used as working gas, and nickel oxide nanosheet array thin film is deposited on the substrate surface; (2) placing the nickel oxide nanosheet array film in a rapid annealing device, heating it to 100° C. at a heating rate of 5 to 10° C. / min in an air atmosphere, and keeping it warm for 5 to 30 minutes. After natural cooling, taking it out, and obtaining an island-shaped nickel oxide nanosheet array electrochromic film for multiple scenarios.
2. The method for preparing a multi-scenario island nickel oxide nanosheet array electrochromic film according to claim 1, characterized in that: In the step (1), the sputtering method of the magnetron sputtering technology is direct current sputtering or radio frequency sputtering.
3. The method for preparing a multi-scenario island nickel oxide nanosheet array electrochromic film according to claim 1, characterized in that: In the step (1), the substrate temperature is 25-100°C, and the vacuum degree of the reaction chamber is 0.8×10 -4 ~1.2×10 -4 Pa, the sputtering gas pressure is 0.5-3.0 Pa, the proportion of sputtered oxygen is 0.25-0.75, the sputtering power density is 25-75 W, and the deposition time is 10-40 min.
4. The method for preparing a multi-scenario island nickel oxide nanosheet array electrochromic film according to claim 1, characterized in that: In the step (2), the thickness of the multi-scenario island-shaped nickel oxide nanosheet array electrochromic film is 150 to 300 nm.
5. An island-shaped nickel oxide nanosheet array electrochromic film for multiple scenarios prepared according to the method for preparing the island-shaped nickel oxide nanosheet array electrochromic film for multiple scenarios as described in claim 1.
6. The multi-scenario island nickel oxide nanosheet array electrochromic film according to claim 5, characterized in that: The multi-scenario island-shaped nickel oxide nanosheet array electrochromic film exhibits a uniform island structure with gaps between islands. Each island exhibits a nano-prism-like morphology and exhibits a strong (111) crystal plane preferred orientation.
7. An application of the multi-scenario island nickel oxide nanosheet array electrochromic film according to claim 5, characterized in that: The multi-scenario oriented island-shaped nickel oxide nanosheet array electrochromic film is used to prepare electrochromic devices in a potassium hydroxide electrolyte environment and a lithium ion electrolyte environment.
8. An application of the multi-scenario island nickel oxide nanosheet array electrochromic film according to claim 5, characterized in that: The multi-scenario oriented island-shaped nickel oxide nanosheet array electrochromic film is used to prepare smart display materials and smart color-changing energy storage materials in a potassium hydroxide electrolyte environment and a lithium ion electrolyte environment.
Citation Information
Patent Citations
Nickel oxide electrochromic composite film and preparation method and application thereof
CN113867064A
Dual-sided display and method for fabricating the same
US20190035773A1