Nickel-plated conductive microsphere and preparation method thereof
By using 2-mercaptoethanesulfonic acid and electroless plating components such as sulfuric acid roughening and nickel salt on the surface of the conductive microspheres, the problem of low flatness of the conductive microspheres is solved, and high binding force and excellent conductivity are achieved. Performance preparation of nickel-plated conductive microspheres.
Patent Information
- Application Number
- CN202410966349.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
AI Technical Summary
The plating of existing conductive microspheres has low flatness, which makes the plating easy to fall off and reduces the conductivity.
Using 2-mercaptoethanesulfonic acid and sulfuric acid as crude agents to increase the sulfonic acid group on the surface of polystyrene microspheres, combining nickel salts, complexing agents, buffers, stabilizers and eutectic solvents in the electroless plating solution Interactions to form a flat nickel-plated conductive layer.
The coating flatness and conductivity of conductive microspheres are improved, the risk of coating shedding is reduced, the preparation process is simplified, and the mass production is suitable.
Smart Images

Figure CN118910595A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of conductive microspheres, and in particular relates to a nickel-plated conductive microsphere and a preparation method thereof. Background Art
[0002] Anisotropic conductive film (ACF) is an emerging green and environmentally friendly microelectronic packaging interconnection material. Research has found that when a certain amount of conductive microspheres are added to ACF, the larger the contact area between the conductive microspheres and the chip boss or substrate chassis under the bonding temperature and pressure during the softening process of ACF, the better the conductive performance of ACF will be.
[0003] The conductive microspheres currently on the market are mainly core-shell conductive microspheres, that is, polymer microspheres are used as cores, and a layer of metal is plated on the surface as a shell by chemical plating. Compared with pure metal conductive microspheres, core-shell conductive microspheres have the advantages of low cost, low density, and high roundness. However, the surface of conductive microspheres prepared by conventional chemical plating often has problems such as coarse unit cells and unit cell accumulation on the coating surface, which will cause the coating to fall off easily at the protrusions of the unit cells, thereby reducing the conductivity of the conductive microspheres. Summary of the invention
[0004] One of the purposes of the present invention is to provide a method for preparing conductive microspheres with high coating flatness, good bonding strength and good conductive performance.
[0005] To achieve the above object, the present invention adopts the following technical scheme: a method for preparing conductive microspheres, comprising the following steps:
[0006] S1, subjecting the polystyrene microspheres to a coarsening treatment, a sensitization treatment and an activation treatment in sequence, and then dispersing them in deionized water, adjusting the pH value to 9-11, to obtain a microsphere dispersion;
[0007] S2. Heat the chemical plating solution to 40-60°C, add the microsphere dispersion and stir for 10-15 minutes, adjust the pH to 9-10 and add the reducing agent replenisher, continue stirring for 10-15 minutes and adjust the pH to 9-10 again and add the reducing agent replenisher, stop stirring after no bubbles are generated in the plating solution for 5-10 minutes, filter, wash with deionized water until neutral and then dry to obtain nickel-plated conductive microspheres.
[0008] As a further improvement of the preparation method of conductive microspheres:
[0009] Preferably, the specific process of the roughening treatment is as follows: 50wt% sulfuric acid and 3M 2-mercaptoethanesulfonic acid solution are mixed in a volume ratio of 10:(1-5) as a roughening agent; polystyrene microspheres are added to the roughening agent in a ratio of 1g:(10-20)mL, stirred at 55-65°C for 1-2h, filtered, washed with deionized water until neutral, and then dried to obtain roughened microspheres.
[0010] Preferably, the specific process of sensitization treatment is as follows: the roughened microspheres are added to a 40g / L stannous chloride solution at a ratio of 1g:(30-40)mL, stirred in a constant temperature water bath at 55-60°C for 30-45min, filtered, washed with deionized water until neutral, and then dried to obtain sensitized microspheres.
[0011] Preferably, the specific process of activation treatment is as follows: add the sensitized microspheres to 4g / L palladium nitrate solution at a ratio of 1g:(30-40)mL, stir for 1-2h in a constant temperature water bath at 45-55°C, filter, wash with deionized water until neutral, and then dry to obtain activated polystyrene microspheres.
[0012] Preferably, the dispersion concentration of the activated polystyrene microspheres in deionized water in step S1 is 0.02-0.05 g / mL, and the addition amount of the microsphere dispersion in the chemical plating solution in step S2 is 1.5-2.5 wt %.
[0013] Preferably, the chemical plating solution includes the following components by mass: 10-20g of nickel salt, 5-20g of complexing agent, 15-40g of buffer, 5-15g of reducing agent, 0.01-0.02g of stabilizer, 10-20g of low eutectic solvent, and 1000g of deionized water.
[0014] Preferably, the nickel salt is one or a combination of two or more of nickel sulfate, nickel chloride, nickel hypophosphite, and nickel carbonate; or, the chelating agent is one or a combination of two or more of EDTA, citric acid, citrate, ammonium chloride, succinic acid, succinate, triethanolamine, ethylenediamine, and lactic acid; or, the buffer is sodium acetate; or, the reducing agent is sodium hypophosphite.
[0015] Preferably, the stabilizer is formed by mixing zinc phytate and lanthanum acetate in a mass ratio of 1:3; or, the low eutectic solvent is formed by mixing betaine and lauryl alcohol in a mass ratio of 1:(1-3).
[0016] Preferably, in steps S1 and S2, sodium hydroxide with a concentration of 4 g / L is used to adjust the pH; and the reducing agent supplement solution is a sodium hypophosphite solution with a concentration of 8-15 g / L.
[0017] A second object of the present invention is to provide a conductive microsphere prepared by any one of the above-mentioned methods for preparing the conductive microsphere.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] 1) The conductive microspheres prepared by the prior art have a low flatness of the coating, which may cause the conductive microsphere coating to partially fall off, thereby reducing the conductivity. In the present invention, 2-mercaptoethanesulfonic acid and sulfuric acid are mixed as a coarsening agent in the coarsening stage of the polystyrene microspheres, so that the surface of the polystyrene microspheres has sulfonic acid groups, which increases the hydrophilicity and specific surface area, improves the bonding ability between the coating and the polystyrene microspheres, makes the nickel layer better attached to the surface of the polystyrene microspheres, improves the coarsening effect of the polystyrene microspheres, and forms conductive microspheres with stable performance.
[0020] 2) The chemical plating solution of the present invention comprises a nickel salt, a complexing agent, a buffer, a reducing agent, a stabilizer, a low eutectic solvent and deionized water. The components interact with each other to jointly improve the flatness of the coating of the conductive microspheres and improve the conductive properties of the conductive microspheres.
[0021] The nickel salt of the invention is the main salt in the plating solution and mainly serves as a supply source of divalent nickel ions. The nickel ions are reduced to metallic nickel under the action of a reducing agent and deposited on the surface of a microsphere to form a nickel-plated conductive layer. The complexing agent can react with the nickel ions in the chemical plating solution to generate a complex, thereby reducing the concentration of free metal ions and reducing the hydrolysis reaction of the metal ions, thereby helping to control the reaction rate in the plating solution and the deposition process of the plating layer, maintaining the stability of the plating solution, ensuring the smooth progress of the nickel plating process, and improving the flatness of the plating layer of the conductive microspheres.
[0022] After zinc phytate and lanthanum acetate are added as stabilizers into the plating solution, zinc ions and lanthanum ions with different valence electron configurations are used, and the synergistic effect of the two ions is adsorbed on the surface of the active center, reducing the activity of the active site, blocking the reduction process of the metal ions, and well inhibiting the spontaneous decomposition of the chemical plating solution, so that nickel-phosphorus crystals are orderly deposited on the surface of the microspheres, which plays a role in refining the crystal grains of the coating, and further forms a flat conductive microsphere coating without obvious grain accumulation.
[0023] The present invention uses betaine and lauryl alcohol as the low eutectic solvent in the chemical plating solution, betaine is a hydrogen bond acceptor, and lauryl alcohol is a hydrogen bond donor. On the one hand, they have good solubility for metal salts and metal oxides, reduce the surface tension of the chemical plating solution, prevent the plating solution from "rebounding" from the surface of the base metal, and help form a smooth, hole-free deposited nickel layer; on the other hand, they can accelerate electron conduction, thereby cooperating with the reducing agent to increase the speed of chemical plating.
[0024] 3) The conductive microspheres prepared by the present invention have a smooth coating, and there is no obvious grain accumulation on the coating surface, which reduces the risk of reduced conductivity caused by accumulation and shedding on the coating surface. The operation method of the present invention is simple and has no complicated steps, and no other equipment is required for mass production. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 is a SEM image of the nickel-plated conductive microspheres prepared in Example 1;
[0026] Figure 2 is a SEM image of the nickel-plated conductive microspheres prepared in Example 2;
[0027] Figure 3 is a SEM image of the nickel-plated conductive microspheres prepared in Example 3;
[0028] Figure 4 is a SEM image of the nickel-plated conductive microspheres prepared in Comparative Example 1;
[0029] Figure 5 is a SEM image of nickel-plated conductive microspheres prepared in Comparative Example 2;
[0030] Figure 6 is a SEM image of nickel-plated conductive microspheres prepared in Comparative Example 3;
[0031] Figure 7 is a SEM image of nickel-plated conductive microspheres prepared in Comparative Example 4;
[0032] Figure 8 is a SEM image of nickel-plated conductive microspheres prepared in Comparative Example 5;
[0033] Fig. 9 This is the SEM image of the nickel-plated conductive microspheres prepared in Comparative Example 6. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention.
[0035] Example 1
[0036] This embodiment provides a method for preparing nickel-plated conductive microspheres, which specifically comprises the following steps:
[0037] Step 1: Roughening of polystyrene microspheres
[0038] 10 mL of 50 wt% sulfuric acid and 5 mL of 3 M 2-mercaptoethanesulfonic acid solution were mixed as a roughening agent; 1 g of polystyrene microspheres were added to 15 mL of the roughening agent at a ratio of 1 g:15 mL, stirred at 60° C. for 1 h, filtered, washed with deionized water until neutral, and dried at 60° C. to obtain roughened microspheres.
[0039] Step 2: Polystyrene microsphere sensitization
[0040] 1 g of roughened microspheres was added to 35 mL of 40 g / L stannous chloride solution at a ratio of 1 g:35 mL, stirred for 30 min in a 55°C constant temperature water bath, filtered, washed with deionized water until neutral, and dried at 60°C to obtain sensitized microspheres.
[0041] Step 3: Activation of polystyrene microspheres
[0042] 1 g of sensitized microspheres was added to 30 mL of 4 g / L palladium nitrate solution at a ratio of 1 g:30 mL, stirred in a 55°C constant temperature water bath for 1.5 h, filtered, washed with deionized water until neutral, and dried at 60°C to obtain activated polystyrene microspheres.
[0043] Step 4: Preparation of microsphere dispersion
[0044] 1 g of activated polystyrene microspheres was dispersed in 20 mL of deionized water, and the pH value was adjusted to 11 with a pH adjuster (4 g / L of sodium hydroxide) to obtain a microsphere dispersion.
[0045] Step 5: Chemical Plating Process
[0046] The chemical plating solution includes the following components by mass: nickel salt (nickel sulfate) 12g, complexing agent (sodium citrate) 6g, buffer (sodium acetate) 25g, reducing agent (sodium hypophosphite) 12g, stabilizer (zinc phytate and lanthanum acetate mixed in a mass ratio of 1:3) 0.02g, low eutectic solvent (betaine and lauryl alcohol mixed in a mass ratio of 1:1) 10g, deionized water 1000g;
[0047] Heat the chemical plating solution to 55°C, add all the microsphere dispersion prepared in step 4, stir for 15 minutes, add a pH adjuster (4 g / L sodium hydroxide) to adjust the pH to 9, and add 2 mL of reducing agent replenisher (10 g / L sodium hypophosphite solution), continue stirring for 15 minutes, then adjust the pH to 9 with a pH adjuster (4 g / L sodium hydroxide), continue to add 4 mL of reducing agent replenisher (10 g / L sodium hypophosphite solution), stop stirring after no bubbles are generated in the plating solution for 5 minutes, filter, wash with deionized water to neutral, and dry at 60°C to obtain nickel-plated conductive microspheres.
[0048] Example 2
[0049] This embodiment provides a method for preparing nickel-plated conductive microspheres, which specifically comprises the following steps:
[0050] Step 1: Roughening of polystyrene microspheres
[0051] 10 mL of 50 wt% sulfuric acid and 3 mL of 3 M 2-mercaptoethanesulfonic acid solution were mixed as a roughening agent; 1 g of polystyrene microspheres were added to 10 mL of the roughening agent at a ratio of 1 g:10 mL, stirred at 55 ° C for 2 h, filtered, washed with deionized water until neutral, and dried at 60 ° C to obtain roughened microspheres.
[0052] Step 2: Polystyrene microsphere sensitization
[0053] 1 g of roughened microspheres was added to 30 mL of 40 g / L stannous chloride solution at a ratio of 1 g:30 mL, stirred in a 60°C constant temperature water bath for 40 min, filtered, washed with deionized water until neutral, and dried at 60°C to obtain sensitized microspheres.
[0054] Step 3: Activation of polystyrene microspheres
[0055] 1 g of sensitized microspheres was added to 35 mL of 4 g / L palladium nitrate solution at a ratio of 1 g:35 mL, stirred in a 50°C constant temperature water bath for 1 h, filtered, washed with deionized water until neutral, and dried at 60°C to obtain activated polystyrene microspheres.
[0056] Step 4: Preparation of microsphere dispersion
[0057] 1 g of activated polystyrene microspheres was dispersed in 20 mL of deionized water, and the pH value was adjusted to 10 with a pH adjuster (4 g / L of sodium hydroxide) to obtain a microsphere dispersion.
[0058] Step 5: Chemical Plating Process
[0059] The chemical plating solution includes the following components by mass: nickel salt (nickel sulfate) 10g, complexing agent (sodium citrate) 7g, buffer (sodium acetate) 21g, reducing agent (sodium hypophosphite) 10g, stabilizer (zinc phytate and lanthanum acetate mixed in a mass ratio of 1:3) 0.01g, low eutectic solvent (betaine and lauryl alcohol mixed in a mass ratio of 1:1) 15g, deionized water 1000g;
[0060] Heat the chemical plating solution to 60°C, add all the microsphere dispersion prepared in step 4, stir for 10 minutes, add a pH adjuster (4 g / L sodium hydroxide) to adjust the pH to 10, and add 2 mL of reducing agent replenisher (10 g / L sodium hypophosphite solution), continue stirring for 10 minutes, then adjust the pH to 10 with a pH adjuster (4 g / L sodium hydroxide), continue to add 4 mL of reducing agent replenisher (10 g / L sodium hypophosphite solution), stop stirring after no bubbles are generated in the plating solution for 10 minutes, filter, wash with deionized water to neutral, and dry at 60°C to obtain nickel-plated conductive microspheres.
[0061] Example 3
[0062] This embodiment provides a method for preparing nickel-plated conductive microspheres, which specifically comprises the following steps:
[0063] Step 1: Roughening of polystyrene microspheres
[0064] Mix 20 mL of 50 wt% sulfuric acid and 2 mL of 3 M 2-mercaptoethanesulfonic acid solution as a roughening agent; add 1 g of polystyrene microspheres to 20 mL of the roughening agent at a ratio of 1 g:20 mL, stir at 50°C for 1.5 h, filter, wash with deionized water until neutral, and dry at 60°C to obtain roughened microspheres.
[0065] Step 2: Polystyrene microsphere sensitization
[0066] 1 g of roughened microspheres was added to 40 mL of 40 g / L stannous chloride solution at a ratio of 1 g:40 mL, stirred in a 60° C. constant temperature water bath for 40 min, filtered, washed with deionized water until neutral, and dried at 60° C. to obtain sensitized microspheres.
[0067] Step 3: Activation of polystyrene microspheres
[0068] 1 g of sensitized microspheres was added to 40 mL of 4 g / L palladium nitrate solution at a ratio of 1 g:40 mL, stirred in a constant temperature water bath at 45°C for 1 h, filtered, washed with deionized water until neutral, and dried at 60°C to obtain activated polystyrene microspheres.
[0069] Step 4: Preparation of microsphere dispersion
[0070] 1 g of activated polystyrene microspheres was dispersed in 20 mL of deionized water, and the pH value was adjusted to 11 with a pH adjuster (4 g / L of sodium hydroxide) to obtain a microsphere dispersion.
[0071] Step 5: Chemical Plating Process
[0072] The chemical plating solution includes the following components by mass: nickel salt (nickel sulfate and nickel chloride are mixed in a mass ratio of 1:1) 20g, complexing agent (sodium citrate) 6g, buffer (sodium acetate) 25g, reducing agent (sodium hypophosphite) 12g, stabilizer (zinc phytate and lanthanum acetate are mixed in a mass ratio of 1:3) 0.015g, low eutectic solvent (betaine and lauryl alcohol are mixed in a mass ratio of 1:1) 20g, deionized water 1000g;
[0073] Heat the chemical plating solution to 40°C, add all the microsphere dispersion prepared in step 4, stir for 15 minutes, add a pH adjuster (4 g / L sodium hydroxide) to adjust the pH to 10, and add 2 mL of reducing agent replenisher (10 g / L sodium hypophosphite solution), continue stirring for 15 minutes, then adjust the pH to 10 with a pH adjuster (4 g / L sodium hydroxide), continue to add 4 mL of reducing agent replenisher (10 g / L sodium hypophosphite solution), stop stirring after no bubbles are generated in the plating solution for 5 minutes, filter, wash with deionized water to neutral, and dry at 60°C to obtain nickel-plated conductive microspheres.
[0074] Comparative Example 1
[0075] This comparative example provides a method for preparing nickel-plated conductive microspheres. The specific steps are referred to Example 1, except that no stabilizer is added to the chemical plating solution.
[0076] Comparative Example 2
[0077] This comparative example provides a method for preparing nickel-plated conductive microspheres. The specific steps are referred to Example 1, except that the stabilizer is only zinc phytate.
[0078] Comparative Example 3
[0079] This comparative example provides a method for preparing nickel-plated conductive microspheres. The specific steps are referred to Example 1, except that the stabilizer is only lanthanum acetate.
[0080] Comparative Example 4
[0081] This comparative example provides a method for preparing nickel-plated conductive microspheres. The specific steps are referred to Example 1, except that no low eutectic solvent is added to the chemical plating solution.
[0082] Comparative Example 5
[0083] This comparative example provides a method for preparing nickel-plated conductive microspheres. The specific steps refer to Example 1, except that the roughening agent is 15 mL of 50 wt % sulfuric acid.
[0084] Comparative Example 6
[0085] This comparative example provides a method for preparing nickel-plated conductive microspheres. The specific steps refer to Example 1, except that the roughening agent is 15 mL of 3M 2-mercaptoethanesulfonic acid solution.
[0086] Figure 1-3 They are SEM images of nickel-plated conductive microspheres prepared in Examples 1-3, from which it can be seen that the surface of the conductive microsphere coating is smooth, uniform and dense, and the grain accumulation is greatly reduced.
[0087] Figure 4-6They are SEM images of nickel-plated conductive microspheres prepared in Comparative Examples 1-3, Figure 4 It can be seen from the figure that the nickel-plated conductive microsphere coating has obvious large-scale grain accumulation; the main reason for this phenomenon is that the stabilizer in the chemical plating can control the reaction rate and inhibit the spontaneous decomposition of the plating solution, so that the metal deposition can proceed in an orderly manner; Figure 5 and 6 It can be seen that the use of zinc phytate or lanthanum acetate as a stabilizer alone does not have a significant effect on the grain accumulation of the coating. The nickel-plated conductive microsphere coating is uneven, the surface grains are chaotic and disordered, and the nickel-plated conductive microsphere coating has obvious large-scale grain accumulation.
[0088] Figure 7 This is the SEM image of nickel-plated conductive microspheres prepared in Comparative Example 4, without adding a low eutectic solvent. Figure 7 It can be seen that the coating of the prepared nickel-plated conductive microspheres is relatively smooth, with a small amount of grain accumulation, and the coating of some microspheres tends to fall off, and the coating effect is not as good as that of Example 1.
[0089] Figure 8 This is the SEM image of the nickel-plated conductive microspheres prepared in Comparative Example 5. Figure 8 It can be seen that some microspheres did not obtain a complete coating and were only etched with sulfuric acid. Although the specific surface area of the polystyrene microspheres was increased, polystyrene is a hydrophobic material. After being roughened with sulfuric acid, there are still fewer hydrophilic groups, which makes it difficult for the roughened microspheres to disperse in water. During the chemical plating process, some microspheres will not undergo chemical plating reaction. It can also be seen from the SEM image that the fewer hydrophilic groups cause agglomeration problems.
[0090] Fig. 9 This is a SEM image of the conductive microspheres prepared in Comparative Example 6. Fig. 9 It can be seen that the conductive microsphere coating is incomplete. This is because the etching effect of 2-mercaptoethanesulfonic acid on the microsphere surface is lower than that of sulfuric acid. The specific surface area is small and the adsorption of divalent tin ions is small, which leads to a low number of activated centers in the activated microspheres. The coating formed during the chemical plating process is uneven and irregular. Figure 8 , 9 It can be seen that the combined effect of sulfuric acid and 2-mercaptoethanesulfonic acid can improve the coarsening effect of polystyrene microspheres, which can not only increase the hydrophilicity of the microspheres, but also increase the specific surface area of the microspheres.
[0091] A self-made rectangular mold was used to press the nickel-plated conductive microspheres into a sheet with a cross-sectional area of 6 cm using an infrared tablet press. 2, a sample with a length of 3 cm, and then a four-probe surface impedance analyzer is used to measure the surface resistance value of the nickel-plated conductive microspheres prepared in Examples 1-3 and Comparative Examples 1-6, and then the conductivity is calculated; the nickel-plated conductive microspheres prepared in Examples 1-3 and Comparative Examples 1-6 are added with anisotropic conductive adhesive (ACP, Dexerials Corporation, model: SA5920HN) to make anisotropic conductive adhesive films, which are placed on ITO, and the polyimide film flexible circuit is aligned with the ITO circuit using a digital camera on a hot press, and then hot pressed using a hot press: first, pre-pressed at 80°C for 1 min, and then at a bonding temperature of 150°C, a bonding pressure of 0.3 MPa, and a bonding time of 20 s. After hot pressing, the sample is post-treated in an oven at 100°C for 1 h to form a device for resistance testing, and the resistance is tested by a Uni-T UT620B DC low resistance tester, and each group is measured 5 times to take the average value. The specific test results are shown in Table 1.
[0092] Table 1
[0093] Serial number Conductivity (S / m) Resistance / Ω Example 1 <![CDATA[2.8×10 3 ]]> 1.83 Example 2 <![CDATA[2.5×10 3 ]]> 1.75 Example 3 <![CDATA[2.6×10 3 ]]> 1.79 Comparative Example 1 <![CDATA[5.2×10 2 ]]> 4.88 Comparative Example 2 <![CDATA[7.5×10 2 ]]> 3.13 Comparative Example 3 <![CDATA[8.1×10 2 ]]> 3.05 Comparative Example 4 <![CDATA[6.3×10 2 ]]> 4.02 Comparative Example 5 <![CDATA[1.8×10 3 ]]> 2.49 Comparative Example 6 <![CDATA[1.2×10 3 ]]> 2.81
[0094] It can be seen from the test data in Table 1 that the surface resistance of the nickel-plated conductive microspheres prepared in Examples 1-3 is small, and when applied to anisotropic conductive films, the connection resistance is significantly reduced, the conductive reliability is high, and the stability is good, which fully demonstrates that the nickel-plated conductive microspheres obtained by the preparation method of the nickel-plated conductive microspheres of the present invention have excellent conductive properties, which are better than the nickel-plated conductive microspheres prepared in Comparative Examples 1-6, and have broad application prospects.
[0095] Those skilled in the art should understand that the above are only some specific embodiments of the present invention, rather than all embodiments. It should be noted that for those of ordinary skill in the art, many modifications and improvements can be made, and all modifications or improvements that do not exceed the scope of protection of the present invention should be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing nickel-plated conductive microspheres, It is characterized in that The following steps are involved: S1, subjecting the polystyrene microspheres to a coarsening treatment, a sensitization treatment and an activation treatment in sequence, and then dispersing them in deionized water, adjusting the pH value to 9-11, to obtain a microsphere dispersion; S2. Heat the chemical plating solution to 40-60°C, add the microsphere dispersion and stir for 10-15 minutes, adjust the pH to 9-10 and add the reducing agent replenisher, continue stirring for 10-15 minutes and adjust the pH to 9-10 again and add the reducing agent replenisher, stop stirring after no bubbles are generated in the plating solution for 5-10 minutes, filter, wash with deionized water until neutral and then dry to obtain nickel-plated conductive microspheres.
2. The method for preparing nickel-plated conductive microspheres according to claim 1, It is characterized in that The specific process of the roughening treatment is as follows: 50wt% sulfuric acid and 3M 2-mercaptoethanesulfonic acid solution are mixed in a volume ratio of 10:(1-5) as a roughening agent; polystyrene microspheres are added to the roughening agent in a ratio of 1g:(10-20)mL, stirred at 55-65°C for 1-2h, filtered, washed with deionized water until neutral, and then dried to obtain roughened microspheres.
3. The method for preparing nickel-plated conductive microspheres according to claim 2, It is characterized in that The specific process of sensitization treatment is as follows: the roughened microspheres are added to a 40g / L stannous chloride solution at a ratio of 1g:(30-40)mL, stirred in a constant temperature water bath at 55-60°C for 30-45min, filtered, washed with deionized water until neutral, and then dried to obtain sensitized microspheres.
4. The method for preparing nickel-plated conductive microspheres according to claim 3, It is characterized in that The specific process of activation treatment is as follows: add the sensitized microspheres into 4g / L palladium nitrate solution at a ratio of 1g:(30-40)mL, stir for 1-2h in a constant temperature water bath at 45-55°C, filter, wash with deionized water until neutral, and then dry to obtain activated polystyrene microspheres.
5. The method for preparing nickel-plated conductive microspheres according to claim 1, It is characterized in that The dispersion concentration of the activated polystyrene microspheres in deionized water in step S1 is 0.02-0.05 g / mL, and the addition amount of the microsphere dispersion in the chemical plating solution in step S2 is 1.5-2.5 wt %.
6. The method for preparing nickel-plated conductive microspheres according to claim 1 or 5, It is characterized in that The chemical plating solution includes the following components by weight: 10-20 g of nickel salt, 5-20 g of complexing agent, 15-40 g of buffer, 5-15 g of reducing agent, 0.01-0.02 g of stabilizer, 10-20 g of low eutectic solvent, and 1000 g of deionized water.
7. The method for preparing nickel-plated conductive microspheres according to claim 6, It is characterized in that The nickel salt is one or a combination of two or more of nickel sulfate, nickel chloride, nickel hypophosphite, and nickel carbonate; or, the complexing agent is one or a combination of two or more of EDTA, citric acid, citrate, ammonium chloride, succinic acid, succinate, triethanolamine, ethylenediamine, and lactic acid; or, the buffer is sodium acetate; or, the reducing agent is sodium hypophosphite.
8. The method for preparing nickel-plated conductive microspheres according to claim 6, It is characterized in that The stabilizer is formed by mixing zinc phytate and lanthanum acetate in a mass ratio of 1:3; or, the low eutectic solvent is formed by mixing betaine and lauryl alcohol in a mass ratio of 1:(1-3).
9. The method for preparing nickel-plated conductive microspheres according to claim 1, It is characterized in that In steps S1 and S2, 4 g / L sodium hydroxide is used to adjust the pH; the reducing agent supplement solution is 8-15 g / L sodium hypophosphite solution.
10. Nickel-plated conductive microspheres prepared by the method for preparing nickel-plated conductive microspheres according to any one of claims 1 to 9.
Citation Information
Cited By
Double-layer nickel-plated conductive microspheres and a preparation method thereof
CN122791358A