Preparation method of TiAl coating of high-temperature composite metal material
The preparation of TiAl coating through laser cladding technology solves the problem of insufficient uniformity and bonding strength in traditional coating methods, and achieves uniformity and stability of high-temperature materials, which is suitable for high-performance needs in high friction scenarios.
Patent Information
- Application Number
- CN202410999499.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-08
AI Technical Summary
Traditional coating methods such as spraying and electroplating are difficult to ensure the uniformity of TiAl coating, resulting in unstable local performance, low bond strength and toughness between the coating and the substrate, and cannot effectively adapt to high friction scenarios.
Using laser cladding technology, TiAl titanium aluminum alloy high-temperature material is pretreated and sprayed according to specific components. The alloy powder is heated and melted by laser beam to form a metallurgical bond with the substrate surface. The binding steps include cleaning, ball milling and slow cooling to ensure Uniformity and quality.
The structure uniformity and performance stability of TiAl high-temperature materials are achieved, the bonding strength and toughness of the coating are improved, and they are suitable for high-temperature environments and high friction scenarios, meeting the high-performance needs of aerospace, automobiles and other fields.
Smart Images

Figure CN118910608A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite material preparation, and in particular to a method for preparing a high-temperature composite metal material TiAl coating. Background Art
[0002] TiAl material has the characteristics of low density, high specific strength and excellent high temperature performance, making it a lightweight high temperature structural material with great development potential in the aerospace field.
[0003] For example, the patent with publication number CN115074686B discloses a method for preparing a TiAl-based composite material that resists cracking. The method for preparing the composite material includes using two titanium-aluminum targets of different compositions, using continuous SiC fibers as reinforcement, and using a physical vapor deposition method to deposit a TiAl alloy coating with similar compositions and alternating staggered arrangements on the fiber surface, and then using hot isostatic pressing or hot pressing to achieve diffusion fusion between TiAl of different compositions, forming a gradient TiAl coating with continuously changing compositions, thereby achieving the preparation of a crack-resistant TiAl-based composite material. Under the premise of ensuring that the composite matrix is a TiAl intermetallic compound, the invention can effectively alleviate the thermal residual stress generated by a single TiAl coating during the molding process, prevent the initiation and expansion of cracks in the matrix, and give full play to the high-temperature mechanical properties of the TiAl matrix.
[0004] Although the above scheme has the above advantages, traditional coating methods such as spraying and electroplating, including the above scheme, are difficult to ensure the uniformity of the coating, resulting in unstable local performance. The bonding between the coating and the substrate mainly relies on physical adsorption and chemical bonding, and the bonding strength is relatively low. In addition, the coating strength and toughness are low, and it cannot effectively adapt to high friction scenarios. Summary of the invention
[0005] In view of the shortcomings of the prior art, the present invention provides a method for preparing a TiAl coating of a high-temperature composite metal material, which solves the problem that the spraying and electroplating methods in the prior art are difficult to ensure the uniformity of the coating, resulting in unstable local performance, and the bonding between the coating and the substrate mainly relies on physical adsorption and chemical bonding, and the bonding strength is relatively low. In addition, the coating strength and toughness are low, and it cannot effectively adapt to high friction scenarios.
[0006] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0007] The present invention provides a method for preparing a high-temperature composite metal material TiAl coating, which is prepared by spraying a TiAl titanium-aluminum alloy high-temperature material on a substrate by laser cladding. The mass percentage of alloy components in the TiAl titanium-aluminum alloy high-temperature material is:
[0008] Al: 43% to 48%, Nb: 1% to 2%, Cr: 1% to 2%, Ce: 0% to 2.5%, of which Ce is not 0, and the rest are Ti and unavoidable impurity elements;
[0009] The laser cladding preparation process steps include:
[0010] Step 1. Prepare corresponding metal raw materials and non-metal raw materials according to the alloy component ratio, and pre-treat the TiAl titanium aluminum alloy high temperature material, including cleaning, crushing and drying;
[0011] Step 2. Use titanium alloy as the substrate and perform cleaning, degreasing and rust removal pretreatment;
[0012] Step 3. Use high-precision laser cladding equipment to evenly spray the pretreated raw material powder on the surface of the substrate, heat and melt the spray layer through the laser beam, so that the molten alloy powder forms a metallurgical bond with the surface of the substrate;
[0013] Step 4: The laser clad TiAl alloy is allowed to stand at 800-150° C. for 2-4 hours, and then slowly cooled to room temperature.
[0014] The present invention is further configured that the pretreatment step includes mixing the five elements Ti, Al, Cr, Nb and Ce into powder and ball milling them in a ball mill;
[0015] The present invention is further configured that, during the ball milling process, the ball milling speed is 100-300 r / min, and the ball milling time is 2-4 h;
[0016] The present invention is further configured such that the substrate is made of TC4 alloy;
[0017] The present invention is further configured such that, in step 4, the clad alloy is allowed to stand at 800-150° C. for 2-4 hours.
[0018] Compared with the prior art, the present invention has the following beneficial effects: the TiAl high-temperature material obtained by the preparation process provided by the present application has uniform structure and stable performance, and can still maintain excellent mechanical properties and chemical stability in a high-temperature environment;
[0019] The present invention provides precise control over alloy composition and laser cladding process parameters during the processing process, thereby achieving precise control over the uniformity and quality of the cladding layer; and the laser cladding technology has the advantages of high precision and high efficiency, and is suitable for large-scale production;
[0020] The TiAl high-temperature material prepared by the present invention has excellent high-temperature performance and chemical stability, and can effectively meet the high-performance requirements of the aerospace, automotive and chemical industries.
[0021] The invention solves the problem that the spraying and electroplating methods in the prior art are difficult to ensure the uniformity of the coating, resulting in unstable local performance. The bonding between the coating and the substrate mainly relies on physical adsorption and chemical bonding, and the bonding strength is relatively low. In addition, the coating strength and toughness are low, and it cannot effectively adapt to high friction scenarios. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The XRD crystal structure ray diffraction diagram of the coating prepared by the method provided by the present invention;
[0023] Figure 2 The metallographic diagram of the high temperature composite metal material TiAl coating with Ce element added thereto of the present invention;
[0024] Figure 3 The metallographic diagram of the high temperature composite metal material TiAl coating without adding Ce element of the present invention;
[0025] Figure 4 This is the Nb element distribution diagram after ball milling in the preparation method of the high-temperature composite metal material TiAl coating of the present invention;
[0026] Figure 5 This is the distribution diagram of Ti element after ball milling in the preparation method of the high temperature composite metal material TiAl coating of the present invention;
[0027] Figure 6 This is the Al element distribution diagram after ball milling in the preparation method of the high temperature composite metal material TiAl coating of the present invention;
[0028] Figure 7 This is the distribution diagram of CeO2 elements after ball milling in the preparation method of the high temperature composite metal material TiAl coating of the present invention;
[0029] Figure 8 This is the distribution diagram of Cr element after ball milling in the preparation method of the high-temperature composite metal material TiAl coating of the present invention. DETAILED DESCRIPTION
[0030] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0031] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0032] The present invention is further described in detail below in conjunction with the accompanying drawings:
[0033] Example 1
[0034] See also Figure 1-Figure 8 The present invention provides a method for preparing a TiAl coating of a high-temperature composite metal material, wherein the alloy composition mass percentage is: Al: 48%, Nb: 2%, Cr: 2%, Ce: 0.5%, and the rest is Ti and unavoidable impurity elements; wherein the impurity elements include: oxygen (O), nitrogen (N), hydrogen (H), carbon (C), and iron (Fe), and the preparation steps include:
[0035] 1) Raw material preparation and substrate treatment: Prepare raw materials according to the above alloy composition ratio and perform pretreatment; select titanium alloy as the substrate and perform pretreatment such as cleaning, degreasing, and rust removal;
[0036] 2) Laser cladding: Use high-precision laser cladding equipment to evenly spray the pre-treated raw material powder on the surface of the substrate, heat and melt the spray layer through the laser beam, so that the molten alloy powder forms a metallurgical bond with the substrate surface;
[0037] During the laser cladding process, the laser power is 1400W, the scanning speed is 4mm / s, and the powder feeding speed is 10g / min. The laser power directly affects the melting depth and width of the cladding layer.
[0038] After multiple processing verifications, the metallurgical bonding effect of the substrate is best at 1400W, so in this embodiment, the laser power is selected to be 1400W, and the cladding layer can be fully melted and form a metallurgical bond with the substrate;
[0039] The scanning speed in the cladding stage determines the moving speed of the laser beam on the substrate surface. In this embodiment, the scanning speed is selected to be 4 mm / s to obtain a more uniform and dense cladding layer, effectively eliminate the residual stress and structural defects inside the material, and improve the mechanical properties and chemical stability of the material.
[0040] 3) Post-treatment: The laser clad TiAl alloy was kept at 1200°C for 2 hours and then slowly cooled to room temperature;
[0041] Example 2
[0042] The only difference from Example 1 is that the Ce content in the alloy composition mass percentage is 1.0%;
[0043] Example 3
[0044] The only difference from Example 1 is that the Ce content in the alloy composition mass percentage is 1.5%;
[0045] Example 4
[0046] The only difference from Example 1 is that the Ce content in the alloy composition mass percentage is 2.0%;
[0047] Example 5
[0048] The only difference from Example 1 is that the Ce content in the alloy composition is 2.5% by mass.
[0049] Figure 1 The crystal structure X-ray diffraction shown is the effect of different Ce contents (from 0 to 2.5%) on the Ti4822 alloy in Examples 1-5; from bottom to top in the figure, pure Ti4822 and Ti4822 alloy samples with 0.5%, 1.0%, 1.5%, 2.0% and 2.5% Ce added are respectively;
[0050] From the figure, we can see the structural changes in different embodiments. With the increase of Ce content, the position and intensity of the diffraction peaks of each sample at different 2θ angles change. CeO2 diffraction peaks appear in 2.5%, 2.0%, 1.5%, and 1.0% Ce samples, indicating that Ce exists mainly in the form of CeO2 in the samples, while the diffraction peaks of Ti3Al and TiAl phases change in intensity and position with Ce content in all samples, indicating that the addition of Ce changes the grain size and relative content of the phase.
[0051] Then based on Figure 1 The analysis results, combined with Figure 2-Figure 3, the improvement of mechanical properties can be clearly seen from the metallographic phase. The strength of the sample with Ce added is improved, and the finer grain boundaries can effectively hinder the movement of dislocations, thereby improving the strength of the material; the fine grain structure helps to increase the impact toughness and ductility of the material and reduce the possibility of brittle fracture; at the same time, grain refinement increases the hardness of the material and increases wear resistance; in summary, in terms of processing methods, this application uses laser cladding technology to effectively enhance the uniformity and density of the coating by precisely controlling the laser power, scanning speed and powder feeding speed, and forms a metallurgical bond with the surface of the substrate by melting the alloy powder, thereby greatly improving the bonding strength of the coating;
[0052] In terms of coating, the addition of Ce element significantly improves the strength and toughness of the coating. The fine grain structure effectively hinders dislocation movement, reduces the possibility of brittle fracture, and improves wear resistance.
[0053] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A method for preparing a high-temperature composite metal material TiAl coating, characterized in that: The TiAl titanium aluminum alloy high temperature material is prepared by spraying it on the substrate by laser cladding. The mass percentage of the alloy components in the TiAl titanium aluminum alloy high temperature material is: Al: 43% to 48%, Nb: 1% to 2%, Cr: 1% to 2%, Ce: 0% to 2.5%; The laser cladding preparation process steps include: Step 1. Prepare corresponding metal raw materials and non-metal raw materials according to the alloy component ratio, and pre-treat the TiAl titanium aluminum alloy high temperature material, including cleaning, crushing and drying; Step 2. Use titanium alloy as the substrate and perform cleaning, degreasing and rust removal pretreatment; Step 3. Use high-precision laser cladding equipment to evenly spray the pretreated raw material powder on the surface of the substrate, heat and melt the spray layer through the laser beam, so that the molten alloy powder forms a metallurgical bond with the surface of the substrate; Step 4: Let the laser clad TiAl stand still and then slowly cool to room temperature.
2. The method for preparing a high temperature composite metal material TiAl coating according to claim 1, characterized in that: The pretreatment step includes mixing the five elements Ti, Al, Cr, Nb and Ce into powder and then ball milling them in a ball mill.
3. The method for preparing a high temperature composite metal material TiAl coating according to claim 2, characterized in that: During the ball milling process, the ball milling speed is 100-300r / min and the ball milling time is 2-4h.
4. The method for preparing a high temperature composite metal material TiAl coating according to claim 3, characterized in that: The substrate is made of TC4 alloy.