Preparation method of high-hardness corrosion-resistant high-entropy alloy coating and valve

By using laser cladding technology with high-entropy alloy stranded welding wire to prepare coatings, the welding compatibility and cracking problems of high-entropy alloy coatings on the sealing surface of high-parameter valves were solved. High-hardness and corrosion-resistant coatings were obtained while reducing energy consumption, thus achieving energy saving and cost reduction.

CN118910612APending Publication Date: 2024-11-08ZHEJIANG UNIV OF TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411103978.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

High-entropy alloy coatings have problems such as poor welding compatibility and easy cracking in high-parameter valve sealing surface applications, and traditional welding processes are time-consuming and energy-intensive.

Method used

A coating is prepared by laser cladding using high-entropy alloy stranded welding wire. The wire arrangement is 1×6+1 or 1×7 structure, the twist angle is 50°~70°, the wire feed speed is 17.5mm/s, the laser parameters are 2000~2200W, and the cladding speed is 3~5mm/s. This method avoids welding cracks and improves the bonding strength.

Benefits of technology

A uniform, crack-free, high-hardness, corrosion-resistant coating was obtained, which has high hardness and good corrosion resistance, and no substrate preheating is required, thus achieving energy saving and cost reduction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910612A_ABST
    Figure CN118910612A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of metal material surface modification, and particularly relates to a preparation method of a high-hardness corrosion-resistant high-entropy alloy coating and a valve, and the preparation method comprises the following steps: preparing a high-entropy alloy stranded welding wire material, preparing a high-entropy alloy stranded welding wire, pretreating a base plate and performing laser cladding. In order to solve the problem that cracks are prone to being generated during welding of the high-entropy alloy coating, a stranded welding wire structure is designed, an Al wire is adopted as a center wire of a 1 * 7 or 1 * 6 + 1 structure, meanwhile, the wire feeding speed in laser cladding process parameters is regulated and controlled, the FCC / BCC two-phase distribution proportion in the coating is regulated, the coating deposition effect is improved, and the high-hardness and corrosion-resistant high-entropy alloy coating is prepared. The prepared high-entropy alloy coating can be applied to a sealing surface of a high-parameter valve.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal material surface modification, and in particular relates to a preparation method of a high-hardness, corrosion-resistant high-entropy alloy coating and a valve. Background Art

[0002] The main circulating media of high-parameter valves usually include different types of fluids such as high-pressure gas, high-pressure liquid, high-temperature medium, corrosive medium, high-viscosity medium, pollutants and solid particles. The valve sealing surface needs to have greater mechanical strength, wear resistance, corrosion resistance, etc. than the conventional valve sealing surface to ensure the sealing and reliability of the valve under extreme working conditions. At present, the sealing surface of high-parameter valves mainly uses some traditional coating materials, such as 316 stainless steel, tungsten carbide, cobalt-based alloys, etc. High entropy alloy is a new material that breaks through the traditional alloy concept. It has high entropy effect in thermodynamics, lattice distortion effect in structure, hysteresis diffusion effect in dynamics and "cocktail" effect in performance, which makes it have many properties superior to traditional alloys, such as high hardness, high strength, good wear resistance, corrosion resistance and radiation resistance.

[0003] The factors that limit the application of high entropy alloy coatings are that the expansion coefficient, thermal conductivity and other properties of high entropy alloys are quite different from those of traditional metals. The welding between high entropy alloys still has good compatibility, while the welding of high entropy alloys with other metals is prone to cracks, and the welding process design is difficult. In the prior art, Chinese patent application CN117535574 A proposes a preparation method of Al-Co-Cr-Fe-Ni coating, wherein single powders of Al, Co, Cr, Fe and Ni are mixed and smelted and then cooled to obtain high-purity high entropy alloy powder, and the high-purity high entropy alloy powder is melted and sprayed onto the surface of the substrate by supersonic flame spraying technology, and the resulting coating has good anti-mechanical friction performance. Summary of the invention

[0004] In order to overcome the obstacles to the application of high entropy alloy coatings, the present invention proposes the following technical solutions: A method for preparing a high-hardness, corrosion-resistant Al-Co-Cr-Fe-Ni high-entropy alloy coating, characterized in that: S1, taking Ni-Cr wire, Fe-Ni-Cr wire, Co wire, and Al wire as wire materials; S2, twisting the wire material to obtain a high entropy alloy stranded welding wire; S3, pre-treating the surface to be treated; S4. Using a laser cladding process, the high entropy alloy stranded welding wire is clad onto the surface to be processed.

[0005] Preferably, the wire arrangement during twisting is a 1×6+1 structure or a 1×7 structure.

[0006] Further preferably, the wire arrangement during twisting is a 1×6+1 structure, and the ratio of the diameters of the central wire to the peripheral wire is greater than or equal to 5:3.

[0007] Preferably, during twisting, the central wire is an Al wire, and the peripheral wires are Ni-Cr wires, Fe-Ni-Cr wires, or Co wires.

[0008] Further preferably, the Ni-Cr wire model is Cr20Ni80, the Fe-Ni-Cr wire model is Fe55-Cr20-Ni25, the Co wire purity is greater than or equal to 99.5wt.%, the Al wire purity is greater than or equal to 99.7wt.%, and the quantity ratio of Ni-Cr wire, Fe-Ni-Cr wire and Co wire is 3:2:1.

[0009] Preferably, the twist angle is 50° to 70° when twisting the stranded welding wire.

[0010] Preferably, the surface to be processed is polished and wiped clean before step S4.

[0011] Preferably, the parameters of the laser cladding process are: laser power 2000-2200 W, cladding speed 3-5 mm / s, wire feeding speed 15-25 mm / s, laser focal length 300-400 mm, laser rotation diameter 3-7 mm, and laser rotation speed 3400-3800 r / min.

[0012] Further preferably, the wire feeding speed of the laser cladding process is 17.5 mm / s.

[0013] The present invention also includes a valve, the valve sealing surface of which has a coating prepared by the above-mentioned high entropy alloy coating preparation method.

[0014] Based on the thermodynamics and kinetics of high entropy alloy formation, the present invention proposes a method for preparing a high-hardness, corrosion-resistant Al-Co-Cr-Fe-Ni high entropy alloy coating based on a laser cladding process. The obtained coating is uniform and crack-free, has high hardness and is corrosion-resistant. When twisted, the wire arrangement is a 1×7 structure or a 1×6+1 structure, and the twist angle is set to 50°~70°. The welding speed is accelerated while the weld penetration is controlled within a reasonable range to avoid cracking caused by excessive penetration. Among the wires, the addition of Al wire can improve the hardness of the high entropy alloy coating, but it is easy to break during the wire feeding process, and a hard oxide film is easy to form at the weld point to reduce the interface bonding force; setting it as the central wire of a 1×7 structure or a 1×6+1 structure can not only make it subjected to the pressure of the outer wire winding to improve the tensile strength, but also reduce the formation of the hard oxide film. When the wire diameter of Al wire and the outer wire is greater than or equal to 5:3, the ratio of Al element in the high entropy alloy can be guaranteed. From the perspective of microstructure, by adjusting the wire feeding rate, the metallographic phase of the high-entropy alloy coating can be made more inclined to the FCC phase, the proportion of the BCC phase can be reduced, and a coating with higher hardness and better corrosion resistance can be obtained.

[0015] In addition, the preparation method proposed in the present invention also has commercial advantages. The raw materials for preparation are all commercially available alloy welding wires, the products are easily available and the purity of each component is stable. The traditional process requires preheating the substrate to improve coating deposition and prevent welding cracks, but this step is time-consuming and energy-intensive. The preparation method of the present invention can obtain a high-entropy alloy coating with the same performance or even slightly better than the traditional process without preheating the substrate, achieving the effect of energy saving, cost reduction and speed increase. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 Schematic diagram of 1×6+1 structure and 1×7 structure when twisted, the left side is 1×6+1 structure, and the right side is 1×7 structure; Figure 2 Metallographic images of the Al-Co-Cr-Fe-Ni high entropy alloy coatings prepared in Examples 1 to 5; Figure 3 This is a comparison chart of the average hardness of the Al-Co-Cr-Fe-Ni high entropy alloy coatings prepared in Examples 1 to 5; Figure 4 Electrochemical polarization curves of Al-Co-Cr-Fe-Ni high entropy alloy coatings prepared in Examples 1 to 5; Figure 5 Electrochemical impedance Nyquist diagram of the Al-Co-Cr-Fe-Ni high entropy alloy coating prepared in Examples 1 to 5. DETAILED DESCRIPTION

[0017] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments of the specification. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.

[0018] Example 1 S1. Prepare high entropy alloy twisted welding wires: 3 Ni-Cr wires (model Cr20Ni80, wire diameter 0.6 mm), 2 Fe-Ni-Cr wires (model Fe55-Cr20-Ni25, wire diameter 0.6 mm), 1 Co wire (purity 99.9 wt.%, wire diameter 0.6 mm), and 1 Al wire (purity 99.9 wt.%, wire diameter 1.0 mm).

[0019] S2. Preparation of high entropy alloy stranded welding wire: 3 Ni-Cr wires, 2 Fe-Ni-Cr wires, 1 Co wire and 1 Al wire are prepared as follows: Figure 1 The 1×6+1 structural arrangement shown is twisted using a high entropy alloy welding wire machine with a twist angle of 60°.

[0020] S3. Substrate pretreatment: Use a handheld grinding wheel to polish the surface of the substrate (Q235), then use absorbent cotton dipped in acetone to wipe the polished substrate clean, and preheat the substrate to 300°C.

[0021] S4. Laser cladding: HK30 laser was used to clad the high entropy alloy stranded wire. Process parameters: laser power 2100W, cladding speed 4mm / s, laser focal length 350mm, laser rotation speed 3600r / min, laser rotation diameter 5mm, wire feeding speed 25mm / s.

[0022] This embodiment is used as a comparative example, and a high entropy alloy coating is prepared using traditional pretreatment operations and the endpoint parameters of the present technical solution as a performance numerical reference.

[0023] Example 2 The steps are the same as those in Example 1, except that the substrate preheating operation is omitted in step S3. Obvious cracking sound is heard during the cladding process. This example is used as a comparative example to illustrate the effect of the substrate preheating process on preventing cracking.

[0024] Example 3 The steps are the same as those in Example 2, except that the wire feeding speed is set to 20 mm / s during S4 laser cladding. An obvious cracking sound is heard during the cladding process. This example is used as a comparative example to illustrate the effect of the wire feeding speed on the coating effect.

[0025] Example 4 The steps are the same as those in Example 2, except that the wire feeding speed is set to 17.5 mm / s during S4 laser cladding. This example is a preferred example.

[0026] Example 5 The steps are the same as those in Example 2, except that the wire feeding speed is set to 15 mm / s during S4 laser cladding.

[0027] Figure 1 The metallographic images of the coatings obtained in various embodiments are used to reveal the microstructure. As shown in the figure, the metallographic structure obtained in the present invention is a FCC / BCC two-phase structure, and as the wire feeding speed decreases, the BCC phase structure decreases.

[0028] Figure 2 The hardness test results of the coatings obtained in each example are used to demonstrate the effect of process parameter changes on the coating hardness. As shown in the figure, the hardness of the coatings obtained in Examples 1 to 4 all reached above 450 HV, among which the hardness of Examples 3 and 4 reached above 500 HV, while the hardness of Example 5 was only about 220 HV due to the low wire feeding speed and large dilution rate.

[0029] Since cracks occurred in Example 2 and Example 3, the corrosion resistance of the coatings obtained under these parameters was no longer measured.

[0030] Figure 3 The electrochemical polarization curves of the coatings obtained in Examples 1, 4, and 5 are used to demonstrate the corrosion resistance of the coatings. As shown in the figure, the high entropy alloy coatings generally have a passivation phenomenon and good corrosion resistance. Different process parameters have no obvious effect on the corrosion potential. The self-corrosion current density of Examples 1, 4, and 5 increases successively, which are 3.351×10 -6 / A·cm -2 , 1.478×10 -5 / A·cm -2 ,9.671×10 -5 / A·cm -2 .

[0031] Figure 4 The Nyquist plots of the coatings obtained in Examples 1, 4, and 5. According to the test principle of impedance spectroscopy, the larger the radius of the arc in the Nyquist plot, the higher the impedance of the coating and the better the corrosion resistance. As shown in the figure, Example 4 has the largest arc radius and better corrosion resistance than other examples.

[0032] Based on the comprehensive results of various parameters, setting the wire feeding speed to 17.5 mm / s during S4 laser cladding can obtain a coating with optimal hardness and corrosion resistance.

[0033] Example 6 A valve, wherein a high entropy alloy coating is prepared on a valve sealing surface using the method of Example 4.

Claims

1. A method for preparing a high-hardness, corrosion-resistant, high-entropy alloy coating, characterized in that: The preparation method comprises the following steps: S1, taking Ni-Cr wire, Fe-Ni-Cr wire, Co wire and Al wire as wire materials; S2, twisting the wire material to obtain a high entropy alloy stranded welding wire; S3, pretreating the surface to be treated; S4, using a laser cladding process to clad the high entropy alloy stranded welding wire onto the surface to be treated.

2. The preparation method according to claim 1, characterized in that: Among the wire materials, the model of Ni-Cr wire is Cr20Ni80, the model of Fe-Ni-Cr wire is Fe55-Cr20-Ni25, the purity of Co wire is greater than or equal to 99.5wt.%, and the purity of Al wire is greater than or equal to 99.7wt.%.

3. The preparation method according to claim 1, characterized in that: During twisting in S2, the wires are arranged in a 1×7 structure or a 1×6+1 structure.

4. The preparation method according to any one of claims 1 to 3, characterized in that: During twisting in S2, the wires are arranged in a manner that the Al wire is the central wire.

5. The preparation method according to claim 3, characterized in that: In the 1×6+1 structure, the wire diameter ratio of the central wire to the peripheral wire is greater than or equal to 5:

3.

6. The preparation method according to claim 1, characterized in that: The twist angle during twisting in S2 is 50° to 70°.

7. The preparation method according to claim 1, characterized in that: The pretreatment in S3 includes polishing and cleaning.

8. The preparation method according to claim 1, characterized in that: The parameters of the laser cladding process are: laser power 2000~2200W, cladding speed 3~5mm / s, wire feeding speed 15~25mm / s, laser focal length 300~400mm, laser rotation diameter 3~7mm, and laser rotation speed 3400~3800r / min.

9. The preparation method according to claim 1 or claim 8, characterized in that: The wire feeding speed of the laser cladding process is 17.5 mm / s.

10. A valve, characterized in that: The sealing surface has a coating prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Electrochemical pretreatment method for improving corrosion resistance of surfacing layer of high-entropy alloy

    CN122466535A