Self-supporting nickel-iron hydrotalcite composite graphene, preparation method and application of self-supporting nickel-iron hydrotalcite composite graphene as oxygen evolution electrocatalyst
Self-supported nickel-ferrohydrotalc/graphene composite materials were prepared by one-step electrodeposition method, which solved the conductivity and stability of NiFe-LDH electrocatalysts in OER catalysis, and achieved efficient and long-life catalysts, which were suitable for industrial applications.
Patent Information
- Application Number
- CN202410714831.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-04
- Publication Date
- 2024-11-08
AI Technical Summary
The existing NiFe-LDH electrocatalysts have problems such as low conductivity, easy aggregation and limited active sites in OER catalysis, and powdered catalysts are prone to agglomeration on the electrodes, resulting in reduced activity and short service life, which limits its industrial application. .
A self-supported nickel-ferrohydrotalc/graphene composite material was prepared in alkaline solution by one-step electrodeposition method. The introduction of graphene enhances conductivity and constructs a porous structure to form a loose and open mesoporous structure to improve catalytic activity and stability.
It realizes a self-supported nickel-molecule hydrotalcite/graphene electrocatalyst with high activity and high stability, improves OER performance and efficiency, is suitable for industrial large-scale production, and extends the service life of the catalyst.
Smart Images

Figure CN118910653A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrocatalytic materials, and in particular relates to a self-supporting nickel-iron hydrotalcite / graphene oxygen evolution electrocatalyst and a preparation method thereof. Background Art
[0002] Electrochemical water splitting technology provides a promising way to solve energy shortage and environmental problems by decomposing water to produce hydrogen and oxygen. In this process, the oxygen evolution reaction (OER) at the anode has slow kinetics due to its involvement in the formation of oxygen-oxygen bonds and the coupled transfer of four electrons and protons, making it a key step in determining the overall efficiency. Although platinum group metal oxides are superior in OER catalysis, their high cost and resource scarcity limit the scope of their commercial application.
[0003] Therefore, the focus of scientific research has shifted to finding non-precious metals and their compounds as alternatives, especially transition metal-based materials such as sulfides, phosphides, and oxides / (oxy)hydroxides, which have attracted much attention due to their abundant reserves on Earth, adjustable nanostructures, and the existence of multiple intermediate states. Among them, layered double hydroxides (LDHs) are particularly prominent in OER electrocatalysis research due to their controllable structural properties.
[0004] Nickel-iron layered hydroxide (NiFe-LDH), also known as nickel-iron hydrotalcite, has been widely studied as a non-precious metal catalyst due to its excellent OER activity and cost-effectiveness in alkaline media. However, pure NiFe-LDH materials have limitations in OER performance, such as low electrical conductivity, easy aggregation, and a limited number of active sites. To address these issues, researchers have adopted various modification strategies, such as creating an intermediate layer between the 3D substrate and NiFe-LDH, which effectively enhanced the OER activity.
[0005] Graphene oxide (GO) is a material with excellent chemical and thermal stability, good conductivity and large specific surface area, and is widely used in electrocatalytic water decomposition. By constructing a composite electrocatalyst of GO and metal oxides or hydroxides, the charge transfer path can be significantly shortened, electron transfer can be improved, and the electronic structure can be adjusted through the interaction between interfaces, thereby improving the adsorption capacity of water molecules and reducing the oxidation state of Ni active sites, thereby improving the OER performance.
[0006] Traditionally prepared NiFe-LDH electrocatalysts are generally in powder form. When used as electrodes, the powder is usually first mixed with an organic binder to make a coating slurry, which is then evenly coated on a conductive substrate. However, this processing method easily leads to agglomeration of NiFe-LDH nanoparticles, increasing the possibility of active sites being shielded and reducing the effective internal mass transfer path, thereby weakening the activity of the catalyst. On the other hand, after long-term operation on the electrode, the powder catalyst may peel off from the electrode surface due to its poor stability, which not only reduces the service life of the catalyst itself, but also greatly limits the practicality of such catalysts in industrial-scale applications.
[0007] Electrodeposition is a method of directly depositing electrode materials on the surface of the current collector. This method can reduce system resistance and improve catalytic activity and stability. Electrocatalysts prepared by electrodeposition can easily adjust the amount of transferred charge, thereby accurately controlling the amount of material deposited. It is considered to be a simple and economical method. It can be easily expanded to large-scale applications, which is conducive to large-scale production.
[0008] In view of this, the present invention develops a simple one-step electrodeposition method to prepare a self-supporting nickel-iron hydrotalcite / graphene oxygen evolution electrocatalyst with high activity and high stability under alkaline solution conditions. Summary of the invention
[0009] In view of the problems existing in the above-mentioned prior art, the purpose of the present invention is to design and provide a self-supporting nickel-iron hydrotalcite / graphene oxygen evolution electrocatalyst. The preparation method of the present invention is simple, the requirements for experimental equipment are relatively basic, it has strong universality, and can be applied under industrial large-scale production conditions.
[0010] The present invention not only helps to enhance the conductivity of the composite nickel-iron hydrotalcite nanosheets with the graphene, but also changes the electronic structure of the nickel-iron hydrotalcite, increases the valence of nickel, and improves the intrinsic catalytic activity. At the same time, the composite nanosheets have a loose and open mesoporous structure, which avoids excessive stacking of the nickel-iron hydrotalcite nanosheets, thereby exposing more electrochemical active areas, promoting the electrocatalytic oxygen evolution reaction, and improving efficiency. The hierarchical porous structure of the porous nickel carrier and the graphene composite nickel-iron hydrotalcite and the low loading amount of the composite material ensure smooth gas escape channels, and can support the oxygen evolution reaction to be carried out continuously and stably. The hierarchical conductive network of the porous nickel carrier and the self-assembled graphene can make the current evenly distributed, which provides a guarantee for the catalyst to work continuously and stably.
[0011] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0012] In one aspect, the present invention provides a self-supporting nickel-iron hydrotalcite composite graphene, comprising a nickel-based carrier and the nickel-iron hydrotalcite composite graphene supported thereon.
[0013] The self-supporting nickel-iron hydrotalcite composite graphene, wherein the nickel-based carrier is a porous nickel material;
[0014] Preferably, the nickel-based carrier is one of nickel foam, nickel mesh or nickel mesh electroplated nickel.
[0015] In a second aspect, the present invention provides a method for preparing a self-supporting nickel-iron hydrotalcite composite graphene, comprising the following steps:
[0016] (1) taking a nickel-based carrier, ultrasonically cleaning it with acetone, ethanol and deionized water in sequence, then ultrasonically treating it with dilute hydrochloric acid, repeatedly washing it with water and drying it to remove surface oxides, thereby obtaining a pretreated nickel-based carrier;
[0017] (2) weighing graphene oxide, subjecting the obtained graphene oxide to alternating ultrasonic treatment and stirring treatment at room temperature, finely dispersing the obtained graphene oxide to ensure that it is fully and evenly dispersed in water to form a homogeneous graphene oxide dispersion, adding nickel nitrate hexahydrate and iron salt, and fully stirring at room temperature to obtain a mixed solution;
[0018] (3) In a three-electrode system, the pretreated nickel-based support obtained in step (1) is used as a working electrode, and the mixed solution obtained in step (2) is used as an electrolyte, and electrodeposition is performed at room temperature and constant potential. The working electrode is taken out, washed by shaking with water and ethanol solution, and dried to obtain a self-supporting nickel-iron hydrotalcite / graphene electrocatalyst.
[0019] In the preparation method, the ultrasonic cleaning time in step (1) is 30 to 90 minutes;
[0020] The ultrasonic treatment time is 3 to 5 minutes;
[0021] The concentration of the dilute hydrochloric acid is 5-10%;
[0022] The drying time is 3 to 4 hours.
[0023] The preparation method, the preparation method of graphene oxide in step (2) comprises: weighing graphite powder and reacting with a mixture of concentrated sulfuric acid and phosphoric acid under ice-water bath conditions, heating, adding potassium permanganate, stirring the reaction and then transferring to ice water, adding hydrogen peroxide, standing and stratifying, then acid washing, dialyzing, and freeze-drying to obtain graphene oxide.
[0024] In the preparation method, the graphite powder is in natural flake form and has a size of 10,000 to 20,000 meshes.
[0025] In the preparation method, the concentration of graphene oxide in step (2) is 0.4-1 mg / mL;
[0026] The ultrasonic treatment and stirring treatment are performed for 30 to 40 minutes and 5 to 10 minutes, respectively.
[0027] The iron salt is ferrous sulfate heptahydrate or ferric nitrate nonahydrate;
[0028] The concentration of the iron salt is 0.15-0.3 mol / L, and the concentration of the nickel nitrate hexahydrate is 0.15-0.3 mol / L;
[0029] The pH of the mixed solution is 4 to 5;
[0030] The sufficient stirring time is 5 to 10 hours.
[0031] The preparation method, in step (3), the three-electrode system uses a Pt sheet as an auxiliary electrode and a saturated calomel electrode as a reference electrode;
[0032] The constant potential is -1V, and the electrodeposition time is 60 to 120 seconds.
[0033] In the preparation method, during the electrodeposition process in step (3), the electrolyte is stirred at 200 to 320 rpm / min.
[0034] In a third aspect, the present invention provides the use of the self-supporting nickel-iron hydrotalcite composite graphene as an oxygen evolution electrocatalyst in the electrolysis of water in an alkaline solution.
[0035] Compared with the prior art, the present invention has the following beneficial effects:
[0036] 1. The one-step electrodeposition technology is used to quickly synthesize high-performance self-supporting composite electrocatalysts under constant voltage. The process is streamlined and efficient, suitable for large-scale industrial production, and meets the urgent needs of the industry for large-scale, low-cost and high-efficiency production.
[0037] 2. The present invention introduces graphene, which not only effectively regulates the electronic structure of nickel-iron hydrotalcite, promotes the increase of nickel valence, and enhances the intrinsic catalytic activity of nickel-iron hydrotalcite, but also constructs three-dimensional porous channels, forms loose and open mesopores, increases the electrochemical active area, and optimizes the catalytic performance.
[0038] 3. The design of the hierarchical porous conductive network of the porous nickel carrier and the graphene composite nickel-iron hydrotalcite and the low loading amount in the present invention enable the gas to escape quickly and the current to be evenly distributed during the catalytic oxygen evolution process, thereby ensuring the continuous and stable operation of the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is a SEM image of the self-supporting nickel-iron hydrotalcite / graphene oxygen evolution electrocatalyst obtained in Example 1 of the present invention, wherein a is a SEM image at a low magnification, and b is a SEM image at a high magnification;
[0040] Figure 2 This is an EDS analysis diagram of the surface of the self-supporting nickel-iron hydrotalcite / graphene oxygen evolution electrocatalyst obtained in Example 1 of the present invention, wherein a is a SEM image, b is a mapping diagram of the Ni element, c is a mapping diagram of the Fe element, e is a mapping diagram of the O element, f is a mapping diagram of the C element, and g is an energy dispersion total spectrum diagram;
[0041] Figure 3 TEM images of the self-supporting nickel-iron hydrotalcite / graphene oxygen evolution electrocatalyst obtained in Example 1 of the present invention, wherein a is the TEM image of NiFe-LDH, and b is the TEM image of NiFe-LDH / GO 20000-0.8mg / mL TEM images;
[0042] Figure 4 This is the XRD pattern of the self-supporting nickel-iron hydrotalcite / graphene oxygen evolution electrocatalyst obtained in Example 1 of the present invention;
[0043] Figure 5 This is the Raman image of the self-supporting nickel-iron hydrotalcite / graphene oxygen evolution electrocatalyst obtained in Example 1 of the present invention;
[0044] Figure 6 This is an XPS graph of the self-supporting nickel-iron hydrotalcite / graphene oxygen evolution electrocatalyst obtained in Example 1 of the present invention, wherein a is the overall XPS spectrum, b is the Ni 2P orbital, c is the Fe 2P orbital, d is the C1s orbital, and e is the O1s orbital;
[0045] Figure 7 This is a SEM image of the self-supporting nickel-iron hydrotalcite / graphene oxygen evolution electrocatalyst obtained in Example 2 of the present invention, wherein a is a SEM image at a low magnification, and b is a SEM image at a high magnification;
[0046] Figure 8 This is a SEM image of the self-supporting nickel-iron hydrotalcite / graphene oxygen evolution electrocatalyst obtained in Example 3 of the present invention, wherein a is a SEM image at a low magnification, and b is a SEM image at a high magnification;
[0047] Fig. 9 This is a SEM image of the self-supporting nickel-iron hydrotalcite / graphene oxygen evolution electrocatalyst obtained in Example 4 of the present invention;
[0048] Fig.10 This is a SEM image of the self-supporting nickel-iron hydrotalcite / graphene oxygen evolution electrocatalyst obtained in the comparative example;
[0049] Fig.11This is a test diagram of polarization curves of the self-supporting nickel-iron hydrotalcite / graphene electrocatalyst obtained in Examples 1-5 of the present invention and the comparative example;
[0050] Fig.12 The Tafel curve test diagram of the self-supporting nickel-iron hydrotalcite / graphene electrocatalyst obtained in Examples 1-5 of the present invention and the comparative example;
[0051] Fig.13 The electrochemical impedance test graph of the self-supporting nickel-iron hydrotalcite / graphene electrocatalyst obtained in Examples 1-5 of the present invention and the comparative example;
[0052] Fig.14 It is a fitting diagram of the double-layer capacitance of the self-supporting nickel-iron hydrotalcite / graphene electrocatalyst obtained in Examples 1-5 of the present invention and the comparative example;
[0053] Fig.15 This is a stability test chart of the self-supporting nickel-iron hydrotalcite / graphene electrocatalyst obtained in Example 1 of the present invention. DETAILED DESCRIPTION
[0054] The embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings and examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0055] Embodiment 1:
[0056] This embodiment provides a self-supporting nickel-iron hydrotalcite composite graphene oxygen evolution electrocatalyst, and the preparation method thereof includes:
[0057] (1) Cut the commercial NF into 1×1 cm 2 The samples were ultrasonically washed with acetone, ethanol and deionized water for 30 min in sequence, and then ultrasonically treated with 5% dilute hydrochloric acid for 5 min to remove surface oxides. Finally, they were repeatedly washed with deionized water and vacuum dried for 4 h and put into sample bags for later use.
[0058] (2) Preparation of graphene oxide by modified Hummers method: In an ice-water bath, 1.5 g of graphite powder was mixed with 180 mL of concentrated sulfuric acid and 20 mL of phosphoric acid for reaction, and then 9 g of potassium permanganate was slowly added and stirred for 2 h. Next, the temperature was raised to 35 °C and stirring was continued for 30 min; finally, the temperature was raised to 50 °C and stirring was continued for 8 h. After the reaction was completed, the mixture was poured into 250 mL of ice water prepared in advance, and after the ice melted, it was poured into a large beaker and stirred. While stirring, 30% hydrogen peroxide solution (H 2 O2 ) until the solution turns golden yellow. After standing for 24 hours to allow the solution to separate, pour off the supernatant, add 5% HCl to pickle and stir, stand for another 24 hours to separate, and then pour off the supernatant, repeat this step three times. Then, dialyze the solution, change the distilled water in the beaker every half a day, and use pH test paper to test until the water in the beaker is neutral. Finally, freeze-dry to obtain graphene oxide.
[0059] (3) Weigh the graphene oxide prepared by the modified Hummers method with 20000 mesh graphite powder, add it into 30 mL ultrapure water, the graphene oxide concentration is 0.8 mg / mL, ultrasonicate it for 30 min at room temperature, stir it for 5 min, and repeat the above alternating ultrasonication and stirring process to ensure that it is fully and evenly dispersed, and finally form a stable homogeneous dispersion. Add 0.15 mol / L nickel nitrate hexahydrate and iron nitrate nonahydrate into the graphene oxide dispersion, stir it for 5 hours at room temperature, and the solution formed is the electrolyte.
[0060] (4) A three-electrode system was used, i.e., a Pt sheet was used as an auxiliary electrode, a saturated calomel electrode (SCE) was used as a reference electrode, and a pretreated nickel-based support was used as a working electrode. The deposition was carried out at room temperature (25°C) and a constant potential of -1 V (vs. SCE) at a magnetic stirring speed of 200 rpm / min for 60 s. After the deposition, the prepared catalyst (working electrode) was taken out, washed with deionized water and ethanol solution for multiple shaking, and dried at 60°C for 4 h to obtain a self-supporting nickel-iron hydrotalcite / graphene electrocatalyst, denoted as NiFe-LDH / GO. 20000-0.8mg / mL .
[0061] We used a SUPRA 55 field emission scanning electron microscope (SEM) manufactured by Zeiss, Germany, to study the microscopic morphology of the material at a depth of about 1 micron. Figure 1 As shown in the figure, the amount of catalyst loaded on the NF skeleton is very uniform at low rate. As the rate increases, the NiFe-LDH / GO 20000-0.8mg / mL The nanosheets are cross-linked with each other, and the phenomenon of easy stacking of hydrotalcite is almost non-existent. This is because the introduction of graphene into the middle layer of the hydrotalcite nanosheets not only plays a role in opening the interlayer of the hydrotalcite, but also increases the conductivity of the foam nickel matrix and the contact area with the electrolyte, allowing the nickel-iron hydrotalcite to be deposited on the matrix more quickly and evenly.
[0062] Further application of energy dispersive spectroscopy (EDS) technology results such as Figure 2As shown in the figure, the elemental composition and ratio of the sample were analyzed in depth, and the results showed that the four elements Ni, Fe, C and O were evenly distributed on the catalyst surface, which indirectly verified the effective composite process of nickel-iron hydrotalcite and graphene. In addition, the material was microscopically tested using a transmission electron microscope (TEM) of Hitachi, Japan, and the results are shown in the figure. Figure 3 As shown, the TEM observation results are consistent with the SEM observation results.
[0063] The sample was then tested (XRD) using a D-max-2500 / PC X-ray diffractometer from Rigaku Corporation. The experimental conditions were as follows: Cu target material was selected, tube current was adjusted to 200 microamperes, tube voltage was set to 40 kilovolts; diffraction slits DS and SS were both 1°, receiving slit RS was set to 0.3 mm; 2θ angle scanning range was 5° to 80°, and data was collected at a speed of 5° / min. The results are shown in Figure 2. Figure 4 As shown in the figure, only the (111), (200), and (220) crystal plane diffraction peaks corresponding to the substrate Ni were detected in the XRD spectrum. No other diffraction peaks were observed, indicating that the amount of catalyst deposited on the NF may be small or the degree of crystallization is low.
[0064] Therefore, the Raman test was performed using the Xplora series imaging spectrometer of HORIBA, France, to verify the successful preparation of the catalyst in Example 1. Figure 5 As shown in the figure, we observed the characteristic peaks of metal bond MOM and the characteristic peaks of graphene D and G, which can indirectly prove the successful synthesis of the catalyst and clarify the change in the degree of graphene reduction before and after the composite. Finally, the ESCALAB 250 X-ray photoelectron spectroscopy (XPS) equipment produced by Thermo Fisher Scientific was used for testing, and the charge correction was performed using the 284.8eV binding energy of C1s as the benchmark. Figure 6 XPS analysis results show that the introduction of graphene changes the chemical environment of nickel-iron hydrotalcite and generates Ni 3+ ions, confirming the interaction between graphene and nickel-iron hydrotalcite.
[0065] Embodiment 2:
[0066] This embodiment provides a self-supporting nickel-iron hydrotalcite / graphene oxygen evolution electrocatalyst, and the preparation method thereof includes:
[0067] (1) Cut the commercial NF into 1×1 cm 2 The samples were ultrasonically washed with acetone, ethanol and deionized water for 30 min in sequence, and then ultrasonically treated with 5% dilute hydrochloric acid for 5 min to remove surface oxides. Finally, they were repeatedly washed with deionized water and vacuum dried for 4 h and placed in sample bags for later use.
[0068] (2) Weigh the graphene oxide prepared by the modified Hummers method with 10000 mesh graphite powder, add it into 30 mL ultrapure water, the graphene oxide concentration is 0.8 mg / mL, ultrasonicate it for 30 min at room temperature, stir it for 5 min, and repeat the above alternating ultrasonication and stirring process to ensure that it is fully and evenly dispersed, and finally form a stable homogeneous dispersion. Add 0.15 mol / L nickel nitrate hexahydrate and iron nitrate nonahydrate into the graphene oxide dispersion, stir it for 5 hours at room temperature, and the solution formed is the electrolyte.
[0069] (3) A three-electrode system was used, i.e., a Pt sheet was used as an auxiliary electrode, a saturated calomel electrode (SCE) was used as a reference electrode, and a pre-treated nickel-based support was used as a working electrode. The catalyst was deposited at a constant potential of -1 V (vs. SCE) at room temperature (25°C) for 60 seconds at a magnetic stirring speed of 200 rpm / min. After the deposition, the prepared catalyst (working electrode) was taken out and washed with deionized water and ethanol solution for multiple shaking, and dried at 60°C for 4 hours to obtain a self-supporting nickel-iron hydrotalcite / graphene electrocatalyst. The morphology was shown in SEM. Figure 7 shown.
[0070] Embodiment 3:
[0071] This embodiment provides a self-supporting nickel-iron hydrotalcite / graphene oxygen evolution electrocatalyst, and the preparation method thereof includes:
[0072] (1) Cut the commercial NF into 1×1 cm 2 The samples were ultrasonically washed with acetone, ethanol and deionized water for 30 min in sequence, and then ultrasonically treated with 5% dilute hydrochloric acid for 5 min to remove surface oxides. Finally, they were repeatedly washed with deionized water and vacuum dried for 4 h and put into sample bags for later use.
[0073] (2) Weigh the graphene oxide prepared by the modified Hummers method with 20000 mesh graphite powder as in Example 1, add 30 mL of ultrapure water, the graphene oxide concentration is 1.0 mg / mL, ultrasonicate for 30 min at room temperature, stir for 5 min, and repeat the above alternating ultrasonication and stirring process to ensure that it is fully and evenly dispersed, and finally form a stable homogeneous dispersion. Add 0.15 mol / L of nickel nitrate hexahydrate and ferric nitrate nonahydrate to the graphene oxide dispersion, stir for 5 hours at room temperature, and the solution formed is the electrolyte.
[0074] (3) A three-electrode system was used, i.e., a Pt sheet was used as an auxiliary electrode, a saturated calomel electrode (SCE) was used as a reference electrode, and a pre-treated nickel-based support was used as a working electrode. The catalyst was deposited at a constant potential of -1 V (vs. SCE) at room temperature (25°C) for 60 seconds at a magnetic stirring speed of 200 rpm / min. After the deposition, the prepared catalyst (working electrode) was taken out and washed with deionized water and ethanol solution for multiple shaking, and dried at 60°C for 4 hours to obtain a self-supporting nickel-iron hydrotalcite / graphene electrocatalyst. The morphology was shown in SEM. Figure 8 shown.
[0075] Embodiment 4:
[0076] This embodiment provides a self-supporting nickel-iron hydrotalcite / graphene oxygen evolution electrocatalyst, and the preparation method thereof includes:
[0077] (1) Cut the commercial NF into 1×1 cm 2 The samples were ultrasonically washed with acetone, ethanol and deionized water for 30 min in sequence, and then ultrasonically treated with 5% dilute hydrochloric acid for 5 min to remove surface oxides. Finally, they were repeatedly washed with deionized water and vacuum dried for 4 h and put into sample bags for later use.
[0078] (2) Weigh the graphene oxide prepared by the modified Hummers method with 20000 mesh graphite powder as in Example 1, add 30 mL of ultrapure water, the graphene oxide concentration is 0.8 mg / mL, ultrasonicate for 30 min at room temperature, stir for 5 min, and repeat the above alternating ultrasonication and stirring process to ensure that it is fully and evenly dispersed, and finally form a stable homogeneous dispersion. Add 0.15 mol / L of nickel nitrate hexahydrate and ferric nitrate nonahydrate to the graphene oxide dispersion, stir for 5 hours at room temperature, and the solution formed is the electrolyte.
[0079] (3) A three-electrode system was used, i.e., a Pt sheet was used as an auxiliary electrode, a saturated calomel electrode (SCE) was used as a reference electrode, and a pre-treated nickel-based support was used as a working electrode. The deposition was carried out at room temperature (25°C) at a constant potential of -1 V (vs. SCE) without magnetic stirring for 60 s. After the deposition, the prepared catalyst (working electrode) was taken out and washed with deionized water and ethanol solution for multiple oscillations. The self-supporting nickel-iron hydrotalcite / graphene electrocatalyst was obtained by drying at 60°C for 4 h. The SEM morphology is shown in FIG. Fig. 9 shown.
[0080] Embodiment 5:
[0081] This embodiment provides a self-supporting nickel-iron hydrotalcite / graphene oxygen evolution electrocatalyst, and the preparation method thereof includes:
[0082] (1) Cut the commercial NF into 1×1 cm 2The samples were ultrasonically washed with acetone, ethanol and deionized water for 30 min in sequence, and then ultrasonically treated with 5% dilute hydrochloric acid for 5 min to remove surface oxides. Finally, they were repeatedly washed with deionized water and vacuum dried for 4 h and put into sample bags for later use.
[0083] (2) Weigh the graphene oxide prepared by the modified Hummers method with 20000 mesh graphite powder as in Example 1, add 30 mL of ultrapure water, the graphene oxide concentration is 0.8 mg / mL, ultrasonicate for 30 min at room temperature, stir for 5 min, and repeat the above alternating ultrasonication and stirring process to ensure that it is fully and evenly dispersed, and finally form a stable homogeneous dispersion. Add 0.15 mol / L of nickel nitrate hexahydrate and ferric nitrate nonahydrate to the graphene oxide dispersion, stir for 5 hours at room temperature, and the solution formed is the electrolyte.
[0084] (3) A three-electrode system was used, i.e., a Pt sheet was used as an auxiliary electrode, a saturated calomel electrode (SCE) was used as a reference electrode, and a pretreated nickel-based support was used as a working electrode. The deposition was performed at room temperature (25°C) and a constant potential of -1 V (vs. SCE) with a magnetic stirring speed of 200 rpm / min for 120 s. After the deposition, the prepared catalyst (working electrode) was taken out, washed with deionized water and ethanol solution by multiple shaking, and dried at 60°C for 4 h to obtain a self-supporting nickel-iron hydrotalcite / graphene electrocatalyst.
[0085] Comparative Example:
[0086] This comparative example provides a self-supporting nickel-iron hydrotalcite / graphene oxygen evolution electrocatalyst, and its preparation method comprises:
[0087] (1) Cut the commercial NF into 2×4cm 2 The samples were ultrasonically washed with acetone, ethanol and deionized water for 30 min in sequence, and then ultrasonically treated with 5% dilute hydrochloric acid for 5 min to remove surface oxides. Finally, they were repeatedly washed with deionized water and vacuum dried for 4 h and put into sample bags for later use.
[0088] (2) Weigh the graphene oxide prepared by the modified Hummers method with 20000 mesh graphite powder as in Example 1, add 30 mL of ultrapure water, the graphene oxide concentration is 0.8 mg / mL, ultrasonicate for 30 min at room temperature, stir for 5 min, and repeat the above alternating ultrasonication and stirring process to ensure that it is fully and evenly dispersed, and finally form a stable homogeneous dispersion. Add 0.15 mol / L of nickel nitrate hexahydrate and ferrous sulfate heptahydrate to the graphene oxide dispersion, stir for 5 hours at room temperature, and the solution formed is the electrolyte.
[0089] (3) A dual anode deposition method was used: nickel foam was used as the counter electrode, the dual working electrodes were two Pt sheet electrodes, and the reference electrode was a saturated calomel electrode (SCE). The working parameters were selected as constant voltage charging at 1V, and deposition was performed for 60s at room temperature (25°C) and under magnetic stirring. After the deposition, the prepared catalyst electrode was taken out and washed with deionized water and ethanol solution for multiple oscillations, and dried at 60°C for 4h to obtain a self-supporting nickel-iron hydrotalcite / graphene electrocatalyst. The SEM morphology is shown in Figure 1. Fig.10 shown.
[0090] The self-supporting nickel-iron hydrotalcite / graphene prepared according to Examples 1 to 5 and the comparative example was used for electrocatalytic oxygen evolution test.
[0091] 1. Electrochemical test:
[0092] A 100 mL non-sealed electrolytic cell was used on a CHI660E electrochemical workstation. The electrolyte was a 1 mol / L KOH solution. The test system was a three-electrode system with a Hg / HgO electrode as the reference electrode and a 1×1 cm 2 The platinum sheet was used as the counter electrode, and the size of the prepared self-supporting nickel-iron hydrotalcite / graphene electrocatalyst was 1×1 cm 2 The electrode sheet is used as the working electrode, and it is necessary to ensure that the working ends of the three electrodes are located at the same level and are completely immersed in the electrolyte.
[0093] Before testing the polarization curve (LSV), it is necessary to perform CV activation at a potential of 0-1V (vs. Hg / HgO) at 10mV / s and 50 cycles. Then the test is performed at a scan rate of 5mV / s and a voltage scan range of 0-1V vs. Hg / HgO. The cyclic voltammetry (CV) test scan rate is 20 to 120mV / s, and the scan is performed in the non-Faraday region voltage range. The test graph is obtained by using the scan rate (v) as the horizontal axis and the current density (i) as the vertical axis to make a scatter plot to fit the double layer capacitance value (C dl ) to evaluate the electrochemical active area (ECSA) of the material. Electrochemical impedance spectroscopy (EIS) analysis chart, frequency range 0.01Hz to 10 5 Hz, with an amplitude of 5mV. Chronopotentiometry is the process of observing the change in potential over time at two current densities (20mA / cm 2 , 500mA / cm 2 ) and observe the curve of potential changing with running time.
[0094] 2. Test results:
[0095] The experimental data of Examples 1-5 and Comparative Examples are shown in Table 1 below. 2Under the current density condition, the electrocatalyst prepared in Example 1 exhibited better performance characteristics than other control group samples: its overpotential reached the minimum value, and the Tafel slope was also the lowest. The small overpotential means that the catalyst needs to overcome a smaller energy barrier when driving a specific electrochemical reaction, so its catalytic activity is relatively higher. On the other hand, the lower Tafel slope directly confirms that the catalyst enhances the reaction efficiency in the key rate-determining step, indicating that it can more effectively accelerate the electrochemical reaction process, reflecting excellent catalytic performance. The specific test results are as follows: Fig.11 and Fig.12 shown.
[0096] The diameter of the semicircle corresponding to the catalyst in Example 1 is the smallest in the chart, which indirectly verifies that it has the smallest charge transfer kinetic resistance. In other words, the charge transfer process between the surface and the reactants of the catalyst is extremely fast, thus showing a particularly outstanding electrocatalytic activity for the oxygen evolution reaction (OER). Fig.13 As for the double-layer capacitance value, the larger the value, the larger the electrochemical active area of the catalyst. The double-layer capacitance value of the catalyst in Example 1 is the largest, indicating that the electrochemical active area is the largest, which greatly improves the electrocatalytic oxygen evolution performance. The test results are as follows Fig.14 shown.
[0097] For stability testing, such as Fig.15 As shown, at a low current density of 20 mA / cm 2 Under the condition of continuous operation for 3100 hours, the voltage of the electrocatalyst of Example 1 remained stable without significant change; 2 Under the harsh conditions of , its stable working time can reach 400 hours, and all electrochemical performances are better than those of the comparative examples. These strongly prove that this self-supporting nickel-iron hydrotalcite / graphene composite material not only has efficient catalytic reaction ability in practical applications, but also has excellent long-term stability under low current density, and its potential application value in the field of catalysis cannot be ignored.
[0098] Table 1 Oxygen evolution performance test of electrocatalysts of Examples 1-5 and Comparative Examples
[0099]
[0100] Finally, it should be noted that the above-described embodiments are only used to illustrate the technical solution of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solution described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solution to deviate from the scope of the technical solution of the embodiments of the present invention.
Claims
1. A self-supporting nickel-iron hydrotalcite composite graphene, characterized in that: It comprises a nickel-based carrier and nickel-iron hydrotalcite composite graphene loaded thereon.
2. A self-supporting nickel-iron hydrotalcite composite graphene according to claim 1, characterized in that: The nickel-based carrier is a porous nickel material; Preferably, the nickel-based carrier is one of nickel foam, nickel mesh or nickel mesh electroplated nickel.
3. A method for preparing a self-supporting nickel-iron hydrotalcite composite graphene according to claim 1 or 2, characterized in that: The following steps are involved: (1) taking a nickel-based carrier, ultrasonically cleaning it with acetone, ethanol and deionized water in sequence, then ultrasonically treating it with dilute hydrochloric acid, repeatedly washing it with water and drying it to obtain a pretreated nickel-based carrier; (2) weighing graphene oxide, subjecting it to alternating ultrasonic treatment and stirring treatment at room temperature to form a homogeneous graphene oxide dispersion, adding nickel nitrate hexahydrate and iron salt, and stirring them sufficiently at room temperature to obtain a mixed solution; (3) In a three-electrode system, the pretreated nickel-based support obtained in step (1) is used as a working electrode, and the mixed solution obtained in step (2) is used as an electrolyte, and electrodeposition is performed at room temperature and constant potential. The working electrode is taken out, washed by shaking with water and ethanol solution, and dried to obtain a self-supporting nickel-iron hydrotalcite / graphene electrocatalyst.
4. The preparation method according to claim 3, characterized in that: The ultrasonic cleaning time in step (1) is 30 to 90 minutes; The ultrasonic treatment time is 3 to 5 minutes; The concentration of the dilute hydrochloric acid is 5-10%; The drying time is 3 to 4 hours.
5. The preparation method according to claim 3, characterized in that: The preparation method of graphene oxide described in step (2) comprises: weighing graphite powder and reacting with a mixture of concentrated sulfuric acid and phosphoric acid under ice-water bath conditions, heating, adding potassium permanganate, stirring the reaction and transferring to ice water, adding hydrogen peroxide, standing and stratifying, acid washing, dialyzing, and freeze-drying to obtain graphene oxide.
6. The preparation method according to claim 5, characterized in that: The graphite powder is in natural flake form and has a size of 10000 mesh to 20000 mesh.
7. The preparation method according to claim 3, characterized in that: The concentration of graphene oxide in the mixed solution in step (2) is 0.4-1 mg / mL; The ultrasonic treatment and stirring treatment are performed for 30 to 40 minutes and 5 to 10 minutes, respectively. The iron salt is ferrous sulfate heptahydrate or ferric nitrate nonahydrate; The concentration of the iron salt is 0.15-0.3 mol / L, and the concentration of the nickel nitrate hexahydrate is 0.15-0.3 mol / L; The pH of the mixed solution is 4 to 5; The sufficient stirring time is 5 to 10 hours.
8. The preparation method according to claim 3, characterized in that: In the three-electrode system described in step (3), a Pt sheet is used as an auxiliary electrode and a saturated calomel electrode is used as a reference electrode; The constant potential is -1V, and the electrodeposition time is 60 to 120 seconds.
9. The preparation method according to claim 3, characterized in that: During the electrodeposition process in step (3), the electrolyte is stirred at 200 to 320 rpm / min.
10. Use of the self-supporting nickel-iron hydrotalcite composite graphene as claimed in claim 1 or 2 as an oxygen evolution electrocatalyst in the electrolysis of water in an alkaline solution.