Graphite / metal hydroxide composite OER electrode and preparation and application thereof
Through the preparation method of graphite/metal hydroxide composite OER electrode, the existing catalysts have poor stability and chlorine resistance in seawater under large currents, and the high activity and chlorine resistance stability are achieved. It is suitable for seawater electrolysis process .
Patent Information
- Application Number
- CN202411156301.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-22
AI Technical Summary
The existing OER catalysts have poor stability under large currents, especially in seawater, and cannot withstand Cl-corrosion shock, making it difficult to take into account both high activity and chlorine resistance.
Using the preparation method of graphite/metal hydroxide composite OER electrode, the deep nucleation and growth of metal hydroxide are optimized and improved by thermally strengthening and electrostrengthening treatment of graphite substrate in aqueous metal solution and reaction in alkali solution. Its physical and chemical structure and defects improve catalytic activity and stability.
An OER catalyst with excellent activity and chlorine resistance under high current is achieved, and can be used stably in seawater, significantly improving the stability and performance of the catalyst.
Smart Images

Figure CN118910667A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of electrocatalysis, and in particular to the field of OER catalytic materials. Technical Background
[0002] The increasingly serious energy crisis and the deterioration of the living environment caused by pollutant emissions have led people to explore the use of greener and cleaner energy. The development and utilization of renewable energy such as wind energy and solar energy and the conversion into electrical energy for use, as well as the storage of electrical energy as clean hydrogen energy have become important links in energy conservation and emission reduction. Among them, the use of electricity obtained from renewable energy to electrolyze water to produce hydrogen, and the storage, transportation and use of hydrogen energy are the focus of researchers. The main reactions of water electrolysis are the anode oxygen evolution reaction (OER) and the cathode hydrogen evolution reaction (HER).
[0003] OER is not only an electrolyzer, but also an important module in energy conversion and storage devices such as rechargeable metal-air batteries and regenerative fuel cells. However, the four-electron reaction process of OER and the adsorption energy ratio between its reaction intermediates bring a large inherent overpotential and slow reaction kinetics to OER catalysts. The development of advanced electrocatalysts based on non-precious metal materials with high activity and stability remains a huge challenge. In addition, conventional water electrolysis requires the consumption of fresh water, and the lack of fresh water has seriously hindered the further development of water electrolysis to produce green hydrogen; but most of the earth is covered by seawater, and humans have abundant seawater resources. Therefore, the preparation of water electrolysis OER catalysts that can be used in seawater is of great significance to the development of the water electrolysis hydrogen production industry.
[0004] The alkaline water electrolysis OER catalysts currently studied and prepared by scholars have continuously made breakthroughs in performance and stability. The most eye-catching are the catalysts directly grown or sprayed on substrates with large specific surface areas such as nickel foam, copper foam, etc. Among them, NiFe-hydroxide, as a widely studied catalyst, has demonstrated unparalleled catalytic activity. However, with the higher requirements for the application current of catalysts, the in-situ grown catalysts have exposed the disadvantage of being easily detached by the impact of large bubbles and losing their activity, making the improvement of the stability of OER catalysts an important challenge.
[0005] In summary, how to prepare an OER catalyst that is both highly active and can work at high currents while maintaining high stability, especially one that can resist Cl - The corrosion impact of OER catalysts has great theoretical and practical significance. Summary of the invention
[0006] In view of the problems in the current field of hydrogen production by water electrolysis that OER catalysts have low activity and poor stability under high current, and most catalysts have the disadvantage of being unable to be used stably in seawater, the present invention provides a method for preparing a graphite / metal hydroxide composite OER electrode, aiming to prepare a new OER catalyst that has excellent OER activity, high current cycling stability and chlorine resistance stability.
[0007] The second object of the present invention is to provide a graphite / metal hydroxide composite OER electrode prepared by the preparation method.
[0008] The third object of the present invention is to provide application of the graphite / metal hydroxide composite OER electrode for water electrolysis.
[0009] In order to obtain ideal OER catalytic activity, the conventional idea is to composite hydroxide active ingredients on the surface of graphite. Although this can achieve ideal OER performance, the stability of the material, especially the OER catalytic stability under high current and high chlorine systems, is not ideal. In response to this problem, the present invention previously attempted to fill the metal hydroxide active ingredients into the pore structure and interlayers of graphite to improve the idea, but early research and development showed that this idea was difficult to achieve the expected effect. The main difficulties are: (1) It is difficult to highly selectively nucleate metal hydroxides in the pores and interlayers of graphite; (2) The activity of metal hydroxides in the pores and interlayers of graphite is limited, which will greatly affect the OER catalytic activity, and it is difficult to obtain the expected material that takes into account both activity and stability. In response to the problems faced in the implementation of this new idea, the present invention has conducted in-depth research and provides the following improvement scheme:
[0010] A method for preparing a graphite / metal hydroxide composite OER electrode comprises immersing a graphite substrate in a metal aqueous solution and pre-treating it under thermal strengthening and / or electrical strengthening to obtain a pre-treated graphite substrate; and then reacting the pre-treated graphite substrate in an alkaline solution with a solute concentration of more than 1M to obtain the graphite / metal hydroxide composite OER electrode.
[0011] The temperature of the heat treatment is above 50°C;
[0012] The metal aqueous solution is an aqueous solution in which metal ions are dissolved, wherein the metal ions are at least one of Ni, Fe, Co, Mn, Cr, and Cu.
[0013] The present invention innovatively heat-strengthens and / or electrically strengthens the graphite substrate in the aqueous metal solution, and then reacts in an alkali, and further cooperates with the joint control of the alkali concentration, so that the deep nucleation and growth of the metal hydroxide on the graphite substrate can be unexpectedly induced, and its physicochemical structure, defects and orientation can be optimized. The method described in the present invention can solve the negative impact of deep nucleation of metal hydroxide on OER activity, and in addition, it can also significantly improve its OER catalytic stability under high current and chlorine resistance, and can obtain an OER catalytic material that takes into account excellent OER activity, high current cycle stability and chlorine resistance stability.
[0014] In the present invention, the graphite substrate is a porous graphite plate; for example, it can be a conventional graphite electrode (graphite current collector).
[0015] In the present invention, the graphite substrate density is 1.65-1.85 g cm -3 .
[0016] Preferably, the graphite substrate is subjected to surface oxidation treatment in advance. The surface oxidation process can be conventional. For example, the graphite substrate can be placed in a mixed acid containing sulfuric acid and nitric acid for surface oxidation treatment.
[0017] In the present invention, the metal ions include divalent metal ions and trivalent metal ions. The present invention has shown that by combining the composite ions, in combination with the strengthening and alkaline reaction process of the present invention, the physicochemical structure of the metal hydroxide grown in the deep graphite layer, such as morphology, orientation and defects, can be optimized. For example, a layered double metal hydroxide with controllable defects can be obtained, which can further improve the OER activity of the prepared material and the OER catalytic stability under high current and chlorine.
[0018] In the present invention, the divalent metal ions include Ni 2+ , Fe 2+ 、Co 2+ , Mn 2+ Cr 2+ , Cu 2+ At least one of; the trivalent metal ions include Fe 3+ 、Co 3+ Cr 3+ At least one of; and the divalent metal and the trivalent metal are different metal elements.
[0019] Preferably, the molar ratio of the divalent metal ions to the trivalent metal ions is 1 to 5:1, and may further be 2 to 4:1.
[0020] Preferably, in the aqueous metal solution, the concentration of the solute may be above 0.1M, further 0.5-5M, further 3-5M.
[0021] Preferably, acid is also added to the aqueous metal solution.
[0022] Preferably, the acid includes at least one of hydrochloric acid and sulfuric acid.
[0023] In the present invention, the concentration of the acid in the aqueous metal solution may be 0.1 to 0.5M.
[0024] In the present invention, the graphite substrate is immersed in the metal aqueous solution, heated and kept warm, and subjected to thermal strengthening treatment. The present invention has shown that through the thermal strengthening treatment, combined with the temperature and the concentration of the alkali reaction, the growth behavior and orientation of the metal hydroxide in the pores and interlayers of the graphite can be optimized, so that the OER activity of the material and the stability under high current and high chloride ion concentration can be further enhanced.
[0025] Preferably, the temperature of heat strengthening is 50-150°C; further preferably, 80-100°C.
[0026] Preferably, the thermal strengthening time is more than 5 hours, and considering the processing efficiency, it can be further 5 to 10 hours.
[0027] In the present invention, the step of electrical strengthening is: using Hg / HgO electrode as reference electrode, platinum sheet as counter electrode, and the graphite substrate as working electrode, placing each electrode in the metal aqueous solution, and performing electrical strengthening treatment, wherein the current on the working electrode is set to -10mAcm -2 ~-20mAcm -2 .
[0028] In the present invention, the electrical strengthening can further improve the growth efficiency and behavior of metal hydroxides in the deep layers of graphite, and can better balance the preparation efficiency and the OER performance of the material.
[0029] In the present invention, the time of electrical strengthening is 1 to 2 minutes.
[0030] In the present invention, thermal strengthening may be performed in advance, and then electrical strengthening treatment may be performed.
[0031] In the present invention, under the aforementioned enhanced treatment, further combined with the alkaline reaction solute, the growth behavior of the metal hydroxide in the pores and interlayers of the graphite substrate as well as the exposure orientation and defects can be optimized, so that the prepared material can have both excellent OER activity and high current stability and chlorine resistance stability.
[0032] In the present invention, the solute in the alkali solution includes at least one of sodium hydroxide, potassium hydroxide, and lithium hydroxide;
[0033] In the present invention, the concentration of the solute in the alkali solution is 1 to 6 M, preferably 3 to 5 M. Studies have shown that under the enhanced process, combined with the optimized control of the alkali concentration, the growth behavior and physicochemical morphology of the metal hydroxide can be optimized, and its OER activity, high current stability and chlorine resistance stability can be further optimized.
[0034] In the present invention, the temperature in the reaction stage is 20-90°C, and can be further room temperature, for example, 20-40°C, in consideration of energy consumption and operation.
[0035] In the present invention, the reaction time is 0.5 h or longer, preferably 0.5 to 1.5 h.
[0036] The present invention also includes a graphite / metal hydroxide composite OER electrode prepared by the preparation method; the composite electrode includes a graphite substrate, and metal hydroxide with defects filled in the pore structure and interlayers of the graphite substrate.
[0037] The preparation method of the present invention can give the prepared material special physical and chemical characteristics, and the material with special characteristics prepared by the preparation method can take into account excellent OER activity as well as high current stability and chlorine resistance stability.
[0038] In the present invention, in the graphite / metal hydroxide composite OER electrode, the loading amount of metal hydroxide in each square centimeter of graphite is 10 to 20 mg.
[0039] The present invention also provides the application of the graphite / metal hydroxide composite OER electrode prepared by the preparation method, which is used as an OER catalyst for water electrolysis.
[0040] The application of the present invention is to use it as an anode for electrolysis of alkaline aqueous solution and / or alkaline brine.
[0041] In the application of the present invention, the concentration of the alkaline component of the alkaline aqueous solution is above 0.1M, preferably 1-6M.
[0042] In the application of the present invention, the brine is an aqueous solution containing metal chlorides. For example, the metal chlorides include at least one of sodium chloride, potassium chloride and lithium chloride.
[0043] In the application of the present invention, the concentration of the metal chloride in the brine is above 0.1M, further can be 0.1-5M, further can be 0.5-3M.
[0044] In the application of the present invention, the brine is seawater.
[0045] Beneficial Effects
[0046] The present invention innovatively subjects the graphite substrate to thermal and / or electrical strengthening treatment in the metal aqueous solution, further reacts in an alkali, and coordinates with the joint control of the alkali concentration, thereby unexpectedly growing the metal hydroxide in the pores and interlayers of the graphite substrate, and optimizing its physicochemical structure and defects, thereby improving the OER activity of the material, and not only that, but also improving its OER catalytic stability under high current and chlorine resistance.
[0047] For example, the OER catalyst prepared by the preparation method of the present invention can be used for large current operation under alkaline conditions and has high stability. It can also be used in the electrolysis process of seawater and has high stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 SEM image of OER polarization obtained in Example 1
[0049] Figure 2 It is a comparison of polarization curves of the OER prepared in Example 1 and the pure graphite plate electrode used as the substrate.
[0050] Figure 3 The OER prepared in Example 1 was carried out in 1 M KOH at 1 A cm -2 The curve of the constant current test.
[0051] Figure 4 The OER prepared in Example 1 was carried out in 1M KOH at 0.5Acm -2 Constant current test
[0052] Figure 5 It is the OER polarization curve of the OER prepared in Example 1 in 1M KOH and in a simulated alkaline seawater environment of 1M KOH+0.5M NaCl.
[0053] Figure 6 The OER prepared in Example 1 was carried out in a simulated alkaline seawater environment of 1M KOH+0.5M NaCl at 1Acm -2 The curve of the constant current test.
[0054] Figure 7 The OER prepared in Example 1 was subjected to 1Acm in a simulated alkaline seawater environment of 1M KOH + 0.5M NaCl. -2 OER polarization curves before and after constant current test.
[0055] Figure 8 This is the polarization curve diagram of the OER electrode obtained under various conditions in Example 2.
[0056] Fig. 9 This is the polarization curve diagram of the OER electrode obtained under various conditions in Example 3.
[0057] Fig.10 This is the polarization curve of the OER electrode obtained in Example 4.
[0058] Fig.11 The OER electrodes of Example 1 and Comparative Example 1 were subjected to 1Acm in 1M KOH+3M NaCl electrolyte. -2 The curve of the constant current test.
[0059] Fig.12 It is the OER polarization curve of the OER electrodes of Example 1 and Comparative Example 2 in 1M KOH+3M NaCl electrolyte. DETAILED DESCRIPTION
[0060] In the present invention, unless otherwise specified, the required raw materials for preparation are all commercially available products well known to those skilled in the art. The present invention provides the application of the OER catalyst described in the above technical scheme in electrolysis of water. The present invention has no special limitation on the method of application, and it can be applied according to methods well known in the art. The present invention is further described below in conjunction with specific examples, and the embodiments described are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present invention.
[0061] Embodiment 1:
[0062] The method for preparing a catalyst that works efficiently and stably in seawater and at industrial current density comprises the following steps:
[0063] Step 1:
[0064] A mixed solution of nickel nitrate and ferric nitrate is prepared and the ratio is controlled, wherein the concentration of nickel nitrate is controlled at 3M, the molar ratio of nickel to iron is 3:1, and 0.2M sulfuric acid solution is added dropwise, and the pH of the system is controlled at 1-2 to obtain a metal solution.
[0065] Step 2:
[0066] Prepare a concentrated acid solution with a volume ratio of concentrated sulfuric acid to concentrated nitric acid of 3:1. Soak a 10*10*2 mm graphite sheet in the concentrated acid solution of step 2 for 5 to 10 seconds. Clean and dry the graphite sheet to obtain surface-treated graphite.
[0067] Step 3: immerse the surface treated graphite of step 2 in the metal solution of step 1, and heat-strengthen at 80° C. (marked as T) under normal pressure for 5 to 6 hours; then take out the graphite and dry it to obtain a modified graphite sheet (also called Graphite-M(NO3)x);
[0068] Step 4: The modified graphite sheet obtained in step 3 was immersed in a 4M sodium hydroxide solution (alkaline solution) at 30°C for 1 hour, and then the electrode was taken out and rinsed to obtain the graphite / metal hydroxide composite OER electrode (also known as Graphite-M(OH)x). The cross-sectional SEM image is shown in Figure 1 .
[0069] Step 5: OER Testing:
[0070] Step 5-1: Test 1: 1M KOH electrolysis test:
[0071] Directly used for OER testing in alkaline solution conditions, for measuring LSV curves or constant current testing.
[0072] The conditions for the OER test are as follows: a platinum sheet is used as a counter electrode, a Hg / HgO electrode is used as a reference electrode, the graphite / metal hydroxide composite OER electrode obtained in the present invention is used as a working electrode, 1M KOH is used as an electrolyte, and a three-electrode system is used for testing. The scanning speed for measuring the polarization curve is 5mV / s, and the scanning window is 0.1 to 1V relative to the reference electrode.
[0073] The polarization curve of Example 1 is as follows Figure 2 As shown in 1. At 1Acm -2 and 0.5Acm -2 The constant current test results under industrial current are as follows Figure 3 as well as Figure 4 shown.
[0074] Step 5-2: Test 2: 1M KOH+0.5M NaCl solution electrolysis test:
[0075] Based on the OER test in step 5-1, the electrolyte was replaced with 1M KOH+0.5M NaCl to simulate alkaline seawater electrolysis. Figure 5 , Figure 6 as well as Figure 7 The performance of the catalyst prepared by this method in simulated alkaline seawater electrolysis is provided.
[0076] Example 2
[0077] Compared with Example 1, the only difference is that the temperature T of step 3 is changed to 25°C, 50°C, 90°C or 120°C, and the other operations and parameters are the same as those of Example 1.
[0078] The polarization results of OER electrodes prepared at different strengthening temperatures are shown in Figure 8 (Test according to step 5-1).
[0079] Figure 8 It can be seen that better results can be obtained above 80°C.
[0080] Example 3
[0081] Compared with Example 1, the only difference is that the concentration of the base in step 4 is changed to 0.1 M or 1 M respectively; other operations and parameters are the same as in Example 1.
[0082] The polarization effect of the OER electrode with different alkali concentrations was tested according to step 5-1 of Example 1. The results are shown in Fig. 9 . Fig. 9 It can be seen that a higher concentration of alkali gives better results, while a too low concentration of alkali gives a poorer effect.
[0083] Example 4
[0084] Compared with Example 1, the only difference is that after thermal strengthening in step 3, electrical strengthening treatment is performed, wherein the electrical strengthening step is: directly using the thermally strengthened graphite plate as the working electrode, using the thermally strengthened solution system as the electrolyte, and inserting a Hg / HgO electrode (reference electrode) and a platinum sheet (counter electrode) into the system to form a three-electrode system, applying a constant current of -10 to -20 mA cm -2 The current is applied and the electric strengthening is performed for 90±10s. Then the graphite is taken out and dried to obtain a modified graphite sheet, and then the subsequent steps 4 and 5 are performed.
[0085] The polarization effect of the OER electrode was tested according to step 5-1 of Example 1. The results are shown in Fig.10 , showing that it has higher activity than Example 1.
[0086] Comparative Example 1
[0087] NiFe hydroxide loaded on nickel foam was prepared by hydrothermal method for OER test. The specific method is: weigh 3mmol nickel nitrate + 1mmol iron nitrate + 15mmol urea + 5mmol ammonium fluoride and dissolve them in 60mL deionized water, stir evenly, transfer to a 100mL hydrothermal kettle, immerse a 3×4cm nickel foam in the solution, put the hydrothermal kettle in an oven, and maintain it at 140℃ for 12h. After the reaction is completed, take it out and rinse it, and test it under the conditions of step 5 of Example 1. Then at 1Acm -2 Perform a constant current stability test.
[0088] The constant current test effect of the OER electrodes of Example 1 and Comparative Example 1 was tested according to step 5-1 of Example 1 (the electrolyte in the electrolysis stage was 1M KOH+3M NaCl aqueous solution). The effect is shown in Fig.11 .
[0089] Comparative Example 2
[0090] Different from Comparative Example 1, the nickel foam is replaced by a graphite plate as a substrate.
[0091] According to the test method of step 5-1 of Example 1, a polarization test was performed in 1M KOH+3M NaCl simulated alkaline seawater. The test results are shown in Fig.12 It can be seen that the method of the present invention can show excellent stability under high chlorine conditions.
Claims
1. A method for preparing a graphite / metal hydroxide composite OER electrode, characterized in that: Immersing the graphite substrate in a metal aqueous solution and pre-treating it under thermal strengthening and / or electrical strengthening to obtain a pre-treated graphite substrate; The pretreated graphite substrate is then reacted in an alkaline solution with a solute concentration of more than 1M to obtain the graphite / metal hydroxide composite OER electrode; The temperature of the heat treatment is above 50°C; The metal aqueous solution is an aqueous solution in which metal ions are dissolved, wherein the metal ions are at least one of Ni, Fe, Co, Mn, Cr, and Cu.
2. The preparation method according to claim 1, characterized in that The graphite substrate is a porous graphite plate; Preferably, the graphite substrate density is between 1.65 and 1.85 g cm -3 ; Preferably, the graphite substrate is pre-treated by surface oxidation.
3. The preparation method according to claim 1, characterized in that: The metal ions include divalent metal ions and trivalent metal ions; The divalent metal ions include Ni 2+ , Fe 2+ 、Co 2+ , Mn 2+ Cr 2+ , Cu 2+ At least one of; the trivalent metal ions include Fe 3+ 、Co 3+ Cr 3+ At least one of; and the divalent metal and the trivalent metal are different metal elements; Preferably, the molar ratio of the divalent metal ion to the trivalent metal ion is 1 to 5:1; Preferably, in the aqueous metal solution, the concentration of the solute is above 0.1M, further 0.5 to 5M; Preferably, an acid is also added to the aqueous metal solution; Preferably, the acid includes at least one of hydrochloric acid and sulfuric acid.
4. The preparation method according to claim 1, characterized in that: The temperature of heat strengthening is 50-150°C; further 80-100°C; Preferably, the thermal strengthening time is more than 5 hours.
5. The preparation method according to claim 1, characterized in that: The steps of electrical strengthening are: using Hg / HgO electrode as reference electrode, platinum sheet as counter electrode, and the graphite substrate as working electrode, placing each electrode in the metal aqueous solution, and performing electrical strengthening treatment, wherein the current on the working electrode is set to -10mAcm -2 ~-20mAcm -2 ; Preferably, the electrical strengthening time is 1-2 minutes.
6. The preparation method according to claim 1, characterized in that: The solute in the alkali solution includes at least one of sodium hydroxide, potassium hydroxide, and lithium hydroxide; Preferably, the concentration of the solute in the alkali solution is 1 to 6 M, preferably 3 to 5 M; Preferably, the temperature during the reaction stage is 20-90°C; Preferably, the reaction time is more than 0.5 h, preferably 0.5-1.5 h.
7. A graphite / metal hydroxide composite OER electrode prepared by the preparation method according to any one of claims 1 to 6; characterized in that: It includes a graphite substrate, and metal hydroxide with defects filled in the pore structure and interlayer of the graphite substrate; Preferably, in the graphite / metal hydroxide composite OER electrode, the loading amount of metal hydroxide in each square centimeter of graphite is 10 to 20 mg.
8. An application of a graphite / metal hydroxide composite OER electrode prepared by the preparation method according to any one of claims 1 to 6, characterized in that: It is used as an OER catalyst for water electrolysis.
9. The use according to claim 8, characterized in that It is used as an anode for electrolysis of alkaline aqueous solution and / or alkaline brine.
10. The use according to claim 9, characterized in that The concentration of the alkaline component of the alkaline aqueous solution is above 0.1M, preferably 0.5 to 6M; Preferably, the brine is an aqueous solution containing metal chloride; preferably, the metal chloride includes at least one of sodium chloride, potassium chloride and lithium chloride; Preferably, the concentration of metal chloride in the brine is above 0.1M; Preferably, the brine is seawater.
Citation Information
Patent Citations
Composite material of nickel hydroxide / graphene or graphite and preparation method for composite material
CN104616908A
Preparation method of metal hydroxide composite electrocatalyst and product thereof
CN114196983A
Self-supporting bifunctional electrolyzed water catalyst as well as preparation and application thereof
CN116180119A
High-entropy Ni-Co-Fe-N-M hydroxide composite material as well as preparation and application thereof in electro-catalysis
CN117230458A
Alkaline electrolyzed water catalyst as well as preparation method and application thereof
CN118127547A