Ultrathin defect type oxide nanosheet catalyst, preparation method and application of ultrathin defect type oxide nanosheet catalyst in proton exchange membrane water electrolysis technology
The preparation of ultra-thin defective oxide nanosheet catalysts through solid phase synthesis and acid treatment solved the problems of slow transfer of four electrons at the anode end and poor stability of IrO2 catalysts in PEM electrolysis technology, achieving efficient and stable catalytic activity and low energy consumption. Have commercial application potential.
Patent Information
- Application Number
- CN202411055143.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-08
AI Technical Summary
The four-electron transfer process at the anode in the existing proton exchange membrane (PEM) electrolytic technology is slow, and commercial IrO2 catalysts have poor stability in strong acid and strong oxidation environments, resulting in high energy consumption and it is difficult to promote the large-scale application of the technology.
The two-dimensional iridium-based and ruthenium-based layered oxides/solid solution oxides containing defective structures were prepared by solid-phase synthesis method, and ultra-thin defective oxide nanosheet catalyst was obtained through acid treatment and liquid phase peeling, which utilized its excellent proton conduction ability. and abundant active sites are exposed to enhance catalytic activity and stability.
It achieves efficient and stable catalytic activity in acidic oxygen evolution catalysis, reduces the anode terminal overpotential, can achieve high current density under low Ir loading, and maintains catalytic activity for a long time, and has commercial application potential.
Smart Images

Figure CN118910670A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of inorganic functional materials, and specifically relates to an ultra-thin defective oxide nanosheet catalyst, a preparation method and application thereof in proton exchange membrane (PEM) water electrolysis technology. Background Art
[0002] With the growth of global energy demand and the increasingly serious environmental pollution problem, the development of renewable energy technology has become a hot topic in global research. The use of renewable energy power systems coupled with water electrolysis technology to produce hydrogen is an ideal way to achieve zero carbon emissions and high-purity green hydrogen. Among them, proton exchange membrane (PEM) water electrolysis technology has high efficiency, high purity hydrogen output and excellent dynamic response capability. It can couple the volatility of renewable energy sources such as wind, light, and electricity, and is currently the most promising green hydrogen production technology. However, the four-electron transfer process at the anode end of the PEM electrolyzer is slow, which significantly limits the efficiency of the water electrolysis reaction. In addition, in the extremely acidic and oxidizing corrosive environment of the anode, the oxygen evolution catalyst relies on commercial IrO2, but the activity of IrO2 is not ideal, resulting in the energy consumption of overcoming the anode end overpotential accounting for 30% to 50% of the total energy consumption of the electrolyzer. Therefore, it is urgent to develop new, efficient and stable acidic oxygen evolution catalysts to promote the large-scale application of PEM water electrolysis hydrogen production technology.
[0003] In recent years, iridium-based oxide catalysts represented by iridium salts have attracted extensive attention from researchers because they show catalytic activity that exceeds that of IrO2. However, since non-precious metal elements are easily soluble in acid, this type of material generally has stability problems such as disordered precipitation and amorphization that cannot be ignored during the catalytic process, making it difficult to apply in practice. Studies have found that iridium-based oxides with open skeleton structures can achieve orderly release of non-precious metal elements in acid solutions without causing amorphization of the iridium oxide skeleton, which has significant advantages in improving the stability of the catalyst structure. Among them, the most representative are layered oxides. This type of material has a periodically arranged layer structure and interlayer cation channels. In acidic solutions, cations can be controllably exchanged with protons without destroying the skeleton connection mode of the oxide layer, which is conducive to maintaining the stability of the material. At the same time, the protonated layered oxides have the potential to be further stripped into nanosheet catalysts. If defects are introduced into the structure on this basis, the exposure of active sites in the material can be maximized, and the dual optimization of catalyst activity and stability can be achieved, thereby obtaining an acidic oxygen evolution catalyst that can replace IrO2 in real application scenarios. Iridium- and ruthenium-based oxides are the most promising acidic oxygen evolution materials with rich layered structures. However, due to the various crystal forms of iridium- and ruthenium-based oxides and their close stoichiometric ratios, it is very difficult to synthesize pure-phase layered oxides. In addition, the synthesis of defects is highly uncontrollable, making the precise preparation of defective layered oxides challenging. In addition, the strong interaction between the layers and interlayer cations in the layered oxides also increases the difficulty of controlled exfoliation of the material. Therefore, it is of great significance to develop a universal method for preparing defective two-dimensional layered oxides and ultrathin defective oxide nanosheet catalysts. Summary of the invention
[0004] The present invention aims to provide an ultra-thin defective oxide nanosheet catalyst, a preparation method and application thereof in proton exchange membrane (PEM) water electrolysis technology.
[0005] The present invention uses a solid phase synthesis method to prepare a series of two-dimensional iridium-based and ruthenium-based layered oxides / solid solution oxides (A x B y M z M' 1-z O2, where A and B are different alkali metals or alkaline earth metal elements; M is Ir; M' is Ru; 0≤z≤1), and ultrathin defective oxide nanosheet catalysts were obtained by acid treatment and liquid phase exfoliation. The nanosheet catalysts showed excellent catalytic activity and stability in acidic oxygen evolution catalysis. Thanks to the excellent proton conductivity and rich active site exposure of the nanosheet catalyst, the proton exchange membrane electrolyzer constructed with this material as the anode catalyst also showed excellent catalytic activity and stability.
[0006] The first object of the present invention is to provide a two-dimensional iridium-based, ruthenium-based layered oxide / solid solution oxide (A) containing a defect structure. x B y M z M' 1-z O2) preparation method, the steps are as follows:
[0007] An iridium source or a ruthenium source is mixed with an alkali metal or an alkaline earth metal compound, and ground in an agate mortar for 1 to 5 hours to obtain a uniformly mixed powder sample; the powder sample is placed in a muffle furnace, heated at a heating rate of 1 to 5°C / min, and then calcined at 500 to 1200°C for 1 to 36 hours, and the muffle furnace is naturally cooled to room temperature to obtain a two-dimensional iridium-based or ruthenium-based layered oxide / solid solution oxide (A) containing a defect structure. x B y M z M' 1-z O2) powder;
[0008] Note: During the calcination process, alkali metal / alkaline earth metal elements not only act as intercalation ions, but also dope into the oxide layer, thereby forming intrinsic iridium defects or ruthenium defects. When only iridium source or ruthenium source is added, the resulting product is an iridium-based or ruthenium-based layered oxide containing a defect structure; when iridium source and ruthenium source are added at the same time, the resulting product is an iridium-ruthenium layered solid solution oxide containing a defect structure in any proportion.
[0009] The second object of the present invention is to provide a method for preparing an ultra-thin defective oxide nanosheet catalyst, the steps of which are as follows:
[0010] (i) preparing the above-prepared two-dimensional iridium-based or ruthenium-based layered oxide / solid solution oxide containing defect structure (A) x B y M z M' 1-z The material is placed in an acid solution with a concentration of 0.1 to 2 M and immersed for 1 to 72 hours to allow the cations between the two-dimensional material layers and the cations soluble in the acid in the layer to fully react with H + exchange (protonation), then washed with water, ethanol several times and dried after centrifugation;
[0011] (ii) placing the solid powder obtained after the acid treatment in step (i) in deionized water, adding an organic intercalant thereto; and then stirring at room temperature for 3 to 10 days to allow the organic intercalant molecules to fully enter the interlayers of the two-dimensional iridium-based or ruthenium-based layered oxide / solid solution oxide containing defect structures;
[0012] (iii) subjecting the mixture obtained in step (ii) to ultrasonic treatment at 10 to 350 W for 0.5 to 3 h to obtain a suspended blue colloidal solution, and then subjecting the colloidal solution to high-speed centrifugation; washing and centrifuging the nanosheet precipitate obtained after centrifugation in sequence to remove residual organic intercalation agent; and freeze-drying to obtain the ultrathin defective oxide nanosheet catalyst.
[0013] In the preparation method of the above-mentioned two-dimensional iridium-based or ruthenium-based layered oxide / solid solution oxide containing defective structure, the iridium source or ruthenium source includes but is not limited to one or a mixture of two or more of iridium or ruthenium chloride, sulfide, hydroxide, oxide, and acetate acetonate;
[0014] In the preparation method of the above-mentioned two-dimensional iridium-based and ruthenium-based layered oxide / solid solution oxide containing defect structures, the alkali metal or alkaline earth metal compound includes but is not limited to one or a mixture of two or more of carbonates, bicarbonates, phosphates, nitrates, chlorides, and hydroxides of Li, Na, K, Rb, Cs, Mg, Ca, Sr, Ba, etc.;
[0015] In the method for preparing the above-mentioned two-dimensional iridium-based or ruthenium-based layered oxide / solid solution oxide containing a defect structure, the molar ratio of the iridium source or ruthenium source to the alkali metal or alkaline earth metal compound is 1:1 to 10;
[0016] In step (i) of the above-mentioned method for preparing the ultra-thin defective oxide nanosheet catalyst, the acid solution for acid treatment (proton exchange) of the two-dimensional iridium-based or ruthenium-based layered oxide / solid solution oxide material containing defective structure includes but is not limited to one or a mixture of two or more of hydrochloric acid solution, sulfuric acid solution, acetic acid solution or perchloric acid solution; the two-dimensional iridium-based or ruthenium-based layered oxide / solid solution oxide powder and H in the acid are reacted. + The molar ratio is 1:1 to 100;
[0017] In step (ii) of the above-mentioned method for preparing ultra-thin defective oxide nanosheet catalysts, the organic intercalation agent includes but is not limited to one or a mixture of two or more of formamide, acetamide, N-methylformamide, diethanolamine, and dimethyl sulfoxide, wherein the two-dimensional iridium-based or ruthenium-based layered oxide / solid solution oxide (A x B y M z M' 1-z The molar ratio of O2 powder to organic intercalant is 1:1-10;
[0018] The third object of the present invention is to provide a two-dimensional iridium-based, ruthenium-based layered oxide / solid solution oxide (A) containing a defect structure. x B y M z M'1-z O2) and its corresponding ultra-thin defective oxide nanosheet catalyst, which are prepared by the above method.
[0019] The fourth object of the present invention is to provide the above-mentioned two-dimensional iridium-based, ruthenium-based layered oxide / solid solution oxide (A) containing defective structure x B y M z M' 1-z O2) and its corresponding ultrathin defective oxide nanosheet catalysts in proton exchange membrane water electrolysis technology.
[0020] Beneficial Effects
[0021] 1. The present invention provides a two-dimensional iridium-based or ruthenium-based layered oxide / solid solution oxide (A) containing a defect structure. x B y M z M' 1-z O2) and its corresponding ultra-thin defective oxide nanosheet catalyst and preparation method thereof, the method is simple to operate, has good repeatability, can be mass-produced, and has strong scalability;
[0022] 2. The present invention is to prepare a two-dimensional iridium-based or ruthenium-based layered oxide / solid solution oxide (A) containing a defect structure. x B y M z M' 1-z O2) was subjected to acid treatment and mechanical exfoliation to obtain an ultra-thin defective oxide nanosheet catalyst with a thickness of about 1 nm. Due to the existence of defective structure and ultra-thin morphology, the nanosheet catalyst achieves maximum exposure of iridium active sites. It exists in the form of a stable colloidal solution in aqueous solution. The prepared catalyst slurry has high dispersibility, which is conducive to electrocatalytic testing;
[0023] 3. The ultra-thin defective oxide nanosheet catalyst prepared by the present invention has good catalytic activity and stability. Taking the ultra-thin defective iridium oxide nanosheet catalyst as an example, it can reach 10mA / cm at an overpotential of 250mV. 2 Current density, and can maintain catalytic activity for more than 1800 hours;
[0024] 4.Ultra-thin defective iridium oxide nanosheet catalyst is used as anode catalyst for PEM electrolyzer, which has a high 2 2.0V@3.92A / cm can be achieved with ultra-low Ir loading 2 @80℃ current density, with commercial application potential. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1: The defective layered iridium salt K prepared in Example 1 0.5 Na 0.2 Ir 0.8 X-ray diffraction (XRD) pattern of O2 Figure 1 a); K 0.5 Na 0.2 Ir 0.8 Schematic diagram of the crystal structure of O2 ( Figure 1 b left) and the protonated sample IrO x H y Schematic diagram of the crystal structure ( Figure 1 b, right panel);
[0026] Figure 2 : The defective layered iridium salt K prepared in Example 1 0.5 Na 0.2 Ir 0.8 Scanning electron microscope (SEM) image of O2 Figure 2 a) and SEM images of the ultra-thin defective iridium oxide nanosheet catalyst obtained after peeling ( Figure 2 b);
[0027] Figure 3 : Transmission electron microscope (TEM) photo of the ultra-thin defective iridium oxide nanosheet catalyst prepared in Example 1 after peeling ( Figure 3 a) and high-resolution photos ( Figure 3 b);
[0028] Figure 4 : Polarization curve of electrocatalytic oxygen evolution of the ultrathin defective iridium oxide nanosheet catalyst prepared in Example 1;
[0029] Figure 5 : Three-electrode oxygen evolution catalytic stability curve of the ultrathin defective iridium oxide nanosheet catalyst prepared in Example 1;
[0030] Figure 6 : Membrane electrode polarization curve of the ultrathin defective iridium oxide nanosheet catalyst prepared in Example 1. DETAILED DESCRIPTION
[0031] The present invention is further explained and illustrated by specific embodiments in combination with the accompanying drawings. It should be noted that the scope of protection of the present invention includes but is not limited to the following embodiments, and all adjustments and changes made to the present invention using some common means and techniques without departing from the subject matter and scope of the present invention should also be included in the scope of protection of the present invention.
[0032] Example 1
[0033] This example prepares a defective layered iridium salt K 0.5 Na0.2 Ir 0.8 O2, and using this material as a precursor, an ultra-thin defective oxide nanosheet catalyst with a thickness of about 1 nm was obtained through acid treatment and liquid phase exfoliation. The specific operation steps are as follows:
[0034] (1) Weigh 0.5 mmol of K2CO3, 0.2 mmol of Na2CO3 and 1.6 mmol of IrO2 into an agate mortar and grind for 1 h to mix them evenly. Place the mixture in a muffle furnace, heat it at a heating rate of 5 °C / min, and then calcine it at 900 °C for 10 h. After the muffle furnace is naturally cooled to room temperature, defective layered iridium salt K 0.5 Na 0.2 Ir 0.8 O2 solid powder, the product mass is about 0.33g.
[0035] (2) Add 0.33 g of K 0.5 Na 0.2 Ir 0.8 O2 powder was placed in 50 ml of 0.5M HCl solution and stirred for 24 h to allow K 0.5 Na 0.2 Ir 0.8 K in O2 + and Na + The ions were completely exchanged with hydrogen ions (protonated), and then the above samples were washed with water and ethanol for 4 times, centrifuged and dried. The obtained sample was a protonated defective two-dimensional layered iridium oxide solid powder, which we named IrO x H y .
[0036] (3) Take 1 mmol of IrO obtained in (2) x H y The sample was placed in a solution containing 100 mL of deionized water and 2 mmol of formamide and stirred at room temperature for 5 days to allow the organic intercalant molecules to fully enter the interlayers of the protonated two-dimensional layered material.
[0037] (4) The mixture obtained above is ultrasonicated in an ultrasonic machine with a power of 350 W for 0.5 h to obtain a suspended blue colloidal solution, which is then centrifuged at high speed; the nanosheet precipitate obtained after centrifugation is washed with water and centrifuged in sequence to remove the residual organic intercalant; and finally, the ultrathin defective iridium oxide nanosheet catalyst with a thickness of about 1 nm is obtained by freeze drying (-50°C).
[0038] The material in Example 1 was structurally characterized. Figure 1 a is a defective layered iridium salt K 0.5 Na 0.2 Ir0.8 X-ray diffraction (XRD) pattern of O2. The XRD pattern combined with the refined data shows that the synthesized material is a pure phase sample. Figure 1 b is K 0.5 Na 0.2 Ir 0.8 Schematic diagram of the crystal structure of O2 obtained by refinement and fitting (left) and the crystal structure of the sample after acid treatment (right). 0.5 Na 0.2 Ir 0.8 O2 K + Mainly located in the interlayer position, Na + It is mainly located in the layer plate and presents a disordered distribution state. + and Na + All ions are replaced by hydrogen ions, and the layer plate shows a state of disordered iridium defects. Figure 2 a is K 0.5 Na 0.2 Ir 0.8 Scanning electron microscope (SEM) photo of O2 shows K 0.5 Na 0.2 Ir 0.8 The plane size of O2 is about 3 to 10 μm, the thickness is about 2 μm, and it has a hexagonal morphology with characteristic layered structure on the sides. Figure 2 b is a SEM photograph of a defective iridium oxide nanosheet catalyst with a thickness of about 1 nm obtained after exfoliation, which shows that the bulk material was successfully exfoliated into an ultra-thin nanosheet catalyst. Figure 3 a is a transmission electron microscope (TEM) photograph of an ultrathin defective iridium oxide nanosheet catalyst with a thickness of about 1 nm obtained after peeling. Figure 3 b is a high-resolution photograph of the ultra-thin defective iridium oxide nanosheet catalyst. It can be clearly seen that the nanosheet catalyst layer has a variety of defect structures.
[0039] The acidic oxygen evolution activity of the iridium oxide nanosheet catalyst was evaluated. The specific operation steps are as follows: weigh 8 mg of freeze-dried nanosheet catalyst solid powder, disperse it in 800 μL of isopropanol solution with a mass fraction of 10% naphthol, and disperse it by ultrasonic machine to obtain a uniform catalyst slurry. Take 2 μL of catalyst slurry and drop it on the surface of a glassy carbon electrode (3 mm in diameter) as the working electrode. The reference electrode and the counter electrode are saturated calomel electrode and platinum wire, respectively, and the electrolyte is 0.1M HClO4 solution. Subsequently, the electrochemical activity test at the three-electrode level was carried out. For comparison, the commercial IrO2 catalyst was tested together using the same slurry configuration method.
[0040] Figure 4This is the polarization curve of the electrocatalytic oxygen evolution of ultra-thin defective iridium oxide nanosheet catalyst and commercial IrO2 catalyst. It can be seen from the figure that the current density is 10mA / cm 2 The overpotential of the nanosheet catalyst is 250 mV, which is 100 mV lower than the overpotential of the commercial IrO2 catalyst at the same loading amount. Figure 5 The three-electrode oxygen evolution catalytic stability curve of the ultra-thin defective iridium oxide nanosheet catalyst. It can be seen that the nanosheet catalyst is 10mA / cm 2 The catalytic activity can be maintained for more than 1800 hours under the current density without obvious change in potential, demonstrating excellent catalytic stability.
[0041] The defective iridium oxide nanosheet catalyst was tested for PEM electrolyzer activity, and the specific process is as follows:
[0042] Preparation of cathode membrane electrode: 18.4 mg Pt / C (40%) was weighed into a centrifuge tube, 13 mL deionized water was added, and ultrasonic dispersion was performed using a cell crusher for 45 min. Then, 17 mL isopropanol and 200 μL 5 wt% naphthol solution were added, and ultrasonic dispersion was performed in the cell crusher for 60 min. The ultrasonic cathode slurry was evenly sprayed on the N115 membrane (area 5 cm) using an ultrasonic sprayer. 2 )superior.
[0043] Preparation of anode membrane electrode: Weigh 15 mg of vacuum freeze-dried nanosheet catalyst powder into a centrifuge tube, add 13 mL of deionized water, and ultrasonically disperse for 20 min. Then add 120 μL of 5 wt% naphthol solution and 187 mL of isopropanol. Continue ultrasonicating for 20 min to obtain a uniform anode slurry. Use an ultrasonic sprayer to evenly spray it on the N115 membrane (area 5 cm) sprayed with the cathode slurry. 2 )’s other side.
[0044] The membrane electrode obtained after spraying was assembled into a PEM electrolyzer for performance evaluation. Note: The gas diffusion layer is titanium felt, the test temperature is 80°C, and the active area is 5cm 2 , iridium loading is 0.3 mg / cm 2 .
[0045] Figure 6 This is the polarization curve of the membrane electrode prepared with defective iridium oxide nanosheet catalyst as the anode catalyst. It can be seen that the nanosheet catalyst has a high conductivity at 0.3 mg / cm 2 2.0V@3.92A / cm can be achieved with Ir loading 2 @80℃ current density, showing excellent catalytic activity.
[0046] Example 2
[0047] As in Example 1, only iridium oxide is replaced with iridium chloride, iridium sulfide, iridium oxyhydroxyl and iridium acetylacetonate, and other synthesis conditions and the amount of reactants remain unchanged, and ultra-thin defective iridium oxide nanosheet catalysts with a thickness of 1 nm can be obtained. They are 2 The acidic oxygen production overpotentials at the current densities are 248mV, 250mV, 249mV and 247mV, respectively.
[0048] Example 3
[0049] As in Example 1, only iridium oxide needs to be replaced by ruthenium oxide, ruthenium chloride, ruthenium oxyhydroxide, ruthenium sulfide, or ruthenium acetylacetonate, and other synthesis conditions and the amount of reactants remain unchanged to obtain ultrathin defective ruthenium oxide nanosheet catalysts with a thickness of 0.7 nm. They are 2 The corresponding acidic oxygen production overpotentials under current density are 228mV, 220mV, 222mV, 224mV and 223mV respectively.
[0050] Example 4
[0051] As in Example 1, only the iridium oxide is changed to a mixture of iridium oxide and ruthenium-based oxide, chloride, sulfide, hydroxide and acetylacetonate in a molar ratio of 1:1, and other synthesis conditions and the amount of reactants remain unchanged to obtain ultra-thin defective iridium oxide ruthenium nanosheet catalysts with a thickness of 0.7 to 1 nm. They are 10 mA / cm 2 The corresponding acidic oxygen production overpotentials under current density are 230mV, 232mV, 228mV, 235mV and 231mV respectively.
[0052] Example 5
[0053] As in Example 1, only sodium carbonate needs to be replaced with the corresponding carbonates of the same molar amounts of Li, K, Rb, Cs, Mg, Ca, Sr, Ba and other elements, and other synthesis conditions and the amounts of reactants remain unchanged to obtain ultra-thin defective iridium oxide nanosheet catalysts with a thickness of 1 nm. They are 2 The corresponding acidic oxygen production overpotentials under current density are 249mV, 241mV, 243mV, 242mV, 243mV, 245mV, 250mV and 251mV respectively.
[0054] Example 6
[0055] As in Example 1, only potassium carbonate needs to be replaced with the corresponding carbonates of the same molar amounts of Li, Na, Rb, Cs, Mg, Ca, Sr, Ba and other elements, and other synthesis conditions and the amounts of reactants remain unchanged to obtain ultra-thin defective iridium oxide nanosheet catalysts with a thickness of 1 nm. They are 2The corresponding acidic oxygen production overpotentials under current density are 242mV, 247mV, 243mV, 245mV, 244mV, 245mV, 252mV and 251mV respectively.
[0056] Example 7
[0057] As in Example 1, only the sodium carbonate is replaced by the same molar amount of sodium bicarbonate, phosphate, nitrate, chloride, and hydroxide, and other synthesis conditions and the amount of reactants remain unchanged to obtain an ultra-thin defective iridium oxide nanosheet catalyst with a thickness of 1 nm. 2 The corresponding acidic oxygen production overpotentials under current density are 241mV, 242mV, 245mV, 246mV and 250mV respectively.
[0058] Example 8
[0059] As in Example 1, only potassium carbonate needs to be replaced with bicarbonate, phosphate, nitrate, chloride, and hydroxide of potassium element of the same molar amount, and other synthesis conditions and the amount of reactants remain unchanged to obtain an ultra-thin defective iridium oxide nanosheet catalyst with a thickness of 1 nm. 2 The corresponding acidic oxygen production overpotentials under current density are 249mV, 243mV, 245mV, 244mV and 251mV respectively.
[0060] Example 9
[0061] As in Example 1, only the calcination time was changed to 1h and 36h, and other synthesis conditions and the amount of reactants remained unchanged, and the same ultra-thin defective iridium oxide nanosheet catalyst with a thickness of 1nm as in Example 1 was obtained. This shows that the defective iridium oxide nanosheet catalyst can be successfully prepared within the calcination time range of 1h to 36h. They are 2 The corresponding acidic oxygen production overpotentials at the current density are 250mV and 255mV respectively.
[0062] Example 10
[0063] As in Example 1, only the calcination temperature is changed to 500°C and 1100°C, and other reaction conditions and the amount of reactants remain unchanged, and the same ultra-thin defective iridium oxide nanosheet catalyst with a thickness of 1 nm as in Example 1 can still be obtained. This shows that the defective iridium oxide nanosheet catalyst can be successfully prepared within the calcination temperature range of 500°C to 1100°C, and they are 2 The corresponding acidic oxygen production overpotentials at the current density are 245mV and 255mV respectively.
[0064] Embodiment 11
[0065] As in Example 1, only the 0.5 M HCl solution is replaced with 0.5 M sulfuric acid solution, acetic acid solution and perchloric acid solution, and other synthesis conditions and the amount of reactants remain unchanged, and the same ultra-thin defective iridium oxide nanosheet catalyst with a thickness of 1 nm as in Example 1 can still be obtained. They are 2 The corresponding acidic oxygen production overpotentials at the current density are 251mV, 250mV and 244mV respectively.
[0066] Example 12
[0067] As in Example 1, only the acid treatment time was changed to 1 h and 72 h, and other synthesis conditions and the amount of reactants remained unchanged, and the same ultra-thin defective iridium oxide nanosheet catalyst with a thickness of 1 nm as in Example 1 was obtained. 2 The corresponding acidic oxygen production overpotentials at the current density are 250mV and 251mV.
[0068] Embodiment 13
[0069] As in Example 1, only the type of organic intercalant is changed to acetamide, N-methylformamide, diethanolamine or dimethyl sulfoxide, and other synthesis conditions and the amount of reactants remain unchanged, and the same ultra-thin defective iridium oxide nanosheet catalyst with a thickness of 1 nm as in Example 1 can still be obtained. 2 The corresponding acidic oxygen production overpotentials under current density are 255mV, 250mV, 244mV and 251mV respectively.
Claims
1. A method for preparing a two-dimensional iridium-based or ruthenium-based layered oxide / solid solution oxide containing a defect structure, characterized in that: An iridium source or a ruthenium source is mixed with an alkali metal or an alkaline earth metal compound, and ground in an agate mortar for 1 to 5 hours to obtain a uniformly mixed powder sample; the powder sample is placed in a muffle furnace, heated at a heating rate of 1 to 5°C / min, and then calcined at 500 to 1200°C for 1 to 36 hours, and after the muffle furnace is naturally cooled to room temperature, a two-dimensional iridium-based or ruthenium-based layered oxide / solid solution oxide powder containing a defect structure is obtained.
2. The method for preparing a two-dimensional iridium-based or ruthenium-based layered oxide / solid solution oxide containing a defect structure as claimed in claim 1, characterized in that: The iridium source or ruthenium source is one or a mixture of two or more of the chloride, sulfide, hydroxide, oxide, and acetate of iridium or ruthenium; the alkali metal or alkaline earth metal compound is one or a mixture of two or more of the carbonate, bicarbonate, phosphate, nitrate, chloride, and hydroxide of Li, Na, K, Rb, Cs, Mg, Ca, Sr, and Ba.
3. The method for preparing a two-dimensional iridium-based or ruthenium-based layered oxide / solid solution oxide containing a defect structure as claimed in claim 1, characterized in that: The molar ratio of the iridium source or ruthenium source to the alkali metal or alkaline earth metal compound is 1:1-10.
4. A two-dimensional iridium-based or ruthenium-based layered oxide / solid solution oxide containing a defect structure, characterized in that: The invention is prepared by the method according to any one of claims 1 to 3.
5. Application of a two-dimensional iridium-based or ruthenium-based layered oxide / solid solution oxide containing a defect structure as described in claim 4 in proton exchange membrane water electrolysis technology.
6. A method for preparing an ultrathin defective oxide nanosheet catalyst, the steps of which are as follows: (i) soaking the two-dimensional iridium-based or ruthenium-based layered oxide / solid solution oxide powder material containing defect structures as claimed in claim 1 in an acid solution with a concentration of 0.1 to 2 M for 1 to 72 hours, so that the cations between the two-dimensional material layers and the cations soluble in the acid in the layer plates are fully reacted with H + The cells were exchanged, then washed with water and ethanol several times and dried after centrifugation. (ii) placing the solid powder obtained after the acid treatment in step (i) in deionized water, adding an organic intercalant thereto; and then stirring at room temperature for 3 to 10 days to allow the organic intercalant molecules to fully enter the interlayers of the two-dimensional iridium-based or ruthenium-based layered oxide / solid solution oxide containing defect structures; (iii) subjecting the mixture obtained in step (ii) to ultrasonic treatment at 10 to 350 W for 0.5 to 3 h to obtain a suspended blue colloidal solution, and then subjecting the colloidal solution to high-speed centrifugation; washing and centrifuging the nanosheet precipitate obtained after centrifugation in sequence to remove residual organic intercalation agent; and freeze-drying to obtain the ultrathin defective oxide nanosheet catalyst.
7. The method for preparing an ultra-thin defective oxide nanosheet catalyst according to claim 6, characterized in that: In step (i), the acid solution is one or a mixture of two or more of a hydrochloric acid solution, a sulfuric acid solution, an acetic acid solution or a perchloric acid solution; in step (i), the two-dimensional iridium-based, ruthenium-based layered oxide / solid solution oxide powder material and H in the acid are mixed. + The molar ratio of dosage is 1:1~100.
8. The method for preparing an ultra-thin defective oxide nanosheet catalyst according to claim 6, characterized in that: In step (ii), the organic intercalant is one or a mixture of two or more of formamide, acetamide, N-methylformamide, diethanolamine, and dimethyl sulfoxide, and the molar ratio of the two-dimensional iridium-based or ruthenium-based layered oxide / solid solution oxide containing a defect structure to the organic intercalant is 1:1 to 10.
9. An ultra-thin defective oxide nanosheet catalyst, characterized in that: The invention is prepared by the method according to any one of claims 6 to 8.
10. Use of the ultra-thin defective oxide nanosheet catalyst according to claim 9 in proton exchange membrane water electrolysis technology.