Method for preparing epoxy coating on surface of bonded magnet
By simplifying the preparation process of the magnet surface epoxy coating, using chamfering, baking soda solution ultrasonic cleaning and electrophoresis, the problems of complex processes and environmental pollution are solved, and efficient and environmentally friendly coating formation is achieved, which improves the magnet's Corrosion resistance.
Patent Information
- Application Number
- CN202410965923.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
AI Technical Summary
The preparation process of existing magnet surface epoxy coatings is complex and environmental pollution problems, especially the phosphorus-containing wastewater generated during phosphating needs to be strictly treated, which affects environmental protection benefits.
The method of chamfering → baking soda solution ultrasonic cleaning → deionized water washing → electrophoresis → curing is used to simplify the process steps and avoid the generation of phosphorus-containing wastewater. The epoxy coating is formed by electrophoresis and thermal deionized water washing in the segmented voltage method.
The preparation process of epoxy coating on the surface of the magnet is simplified, the process efficiency and environmental protection are improved, the generation of phosphorus-containing wastewater is avoided, and the corrosion resistance of the magnet is ensured.
Smart Images

Figure CN118910696A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparing epoxy coating on the surface of bonded magnets, and in particular to a method for preparing epoxy coating on the surface of bonded magnets. Background Art
[0002] The neodymium and iron elements in the bonded NdFeB magnet (hereinafter referred to as the magnet) are highly active and easily oxidized in humid air and easily corroded by acid. Therefore, it is necessary to find ways to improve the oxidation resistance or corrosion resistance of the magnet. To solve the above problems, the method of covering the surface with a layer of epoxy resin protective layer has become a widely adopted strategy in the industry. This protective layer can not only effectively isolate the direct effect of the external environment on the magnet, but also significantly improve the service life and stability of the magnet.
[0003] Magnets are usually made by compression molding, and the main shape is a ring. The unique feature is that the density in the middle of the ring is slightly sparser than at the two ends. This phenomenon is particularly significant in the thin-walled and high-height ring structure. This density difference directly affects the quality of the subsequent epoxy coating, which is manifested in the thin coating in the middle low-density area, and even the "exposed bottom" phenomenon where the coating is not fully covered, which seriously weakens the protective effect of the coating on the magnet.
[0004] To overcome this problem, the current industry generally adopts a series of complex pretreatment steps to optimize the coating quality. This process covers multiple key links from the initial processing of the magnet to the final coating curing. The corresponding typical preparation process includes: magnet → chamfering (grinding and polishing) → tap water ultrasonic cleaning → sealing → deionized water washing → curing → phosphating → deionized water washing → electrophoresis → deionized water washing → baking; the sealing process uses organic sealing agents to penetrate into the tiny pores of the magnet and solidify, forming an effective barrier to prevent the pretreatment liquid from penetrating into the interior of the magnet, while promoting the uniform adhesion of the subsequent resin coating, significantly improving the corrosion resistance; and the phosphating treatment constructs a protective phosphating film on the surface of the magnet, doubly guaranteeing the rust prevention ability of the magnet before electrophoresis and the overall corrosion resistance of the coating.
[0005] Although the above preparation process has achieved remarkable results in improving the protection effect of magnets, its complexity and environmental challenges cannot be ignored. In particular, the phosphorus-containing wastewater generated during the phosphating process must be strictly treated to meet the emission standards before it can be discharged, which puts higher requirements on environmental protection. Therefore, while continuously optimizing the magnet coating preparation process, exploring more environmentally friendly and efficient alternatives to achieve a win-win situation for magnet performance and environmental benefits will be an important direction for future research. Summary of the invention
[0006] In order to solve the above problems, the present invention provides a method for preparing an epoxy coating on the surface of a bonded magnet.
[0007] The present invention provides a method for preparing an epoxy coating on the surface of a bonded magnet, the method comprising the following steps:
[0008] The bonded magnet is chamfered, and then ultrasonically cleaned with a baking soda solution, washed with a first deionized water, and washed with hot deionized water to obtain a first bonded magnet;
[0009] Performing electrophoresis treatment on the first bonded magnet using electrophoretic paint containing epoxy resin, and then performing a second deionized water wash to obtain a second bonded magnet;
[0010] The second bonded magnet is cured to form an epoxy coating on the surface of the bonded magnet.
[0011] Furthermore, the working condition parameters of the chamfer include: the chamfer is C0.5.
[0012] Furthermore, the working condition parameters of the baking soda solution ultrasonic cleaning include: the pH of the baking soda solution is 7-8, the ultrasonic power is 10K-14KW, and the time is 1-1.5min.
[0013] Furthermore, the working condition parameters of the first deionized water washing and the second deionized water washing include: a temperature of 20° C. to 30° C., a time of 1 to 1.5 min, and a number of cleaning times of 2 to 3 times.
[0014] Furthermore, the working condition parameters of the hot deionized water washing include: temperature of 65° C. to 70° C. and time of 40 to 60 seconds.
[0015] Furthermore, the electrophoretic paint containing epoxy resin comprises a color paste, epoxy resin and deionized water in a weight ratio of 1:4:5.
[0016] Furthermore, the conductivity of the electrophoretic paint containing epoxy resin is 1400 μS / cm to 1600 μS / cm.
[0017] Furthermore, the step of electrophoresis treatment includes the following process:
[0018] The electrophoresis is performed by adopting a segmented voltage control method, wherein the segmented voltage control method is divided into six segments;
[0019] The first stage: the voltage rises from 0 to 130V at a constant speed, taking 100s;
[0020] The second stage: the voltage is maintained at 130V for 30 seconds;
[0021] The third stage: the voltage rises from 130V to 170V, which takes 30s;
[0022] The fourth stage: the voltage is maintained at 170V for 20s;
[0023] The fifth stage: the voltage rises from 170V to 210V at a constant speed, which takes 30s;
[0024] In the sixth section, the voltage is maintained at 210V for 10 seconds.
[0025] Furthermore, the curing step includes the following process:
[0026] The second bonded magnet is first kept at 80-90° C. for 15 min, then kept at 110-120° C. for 15 min, and finally kept at 165-170° C. for 30 min.
[0027] The above technical solution provided by the embodiment of the present invention has at least the following advantages compared with the prior art:
[0028] An embodiment of the present invention provides a method for preparing an epoxy coating on the surface of a bonded magnet. Compared with the prior art, the modified method for preparing an epoxy coating on the surface of a bonded magnet comprises: magnet → chamfering → ultrasonic cleaning with a baking soda solution → deionized water washing → hot deionized water washing → electrophoresis → deionized water washing → baking, which simplifies the existing epoxy coating preparation process steps and effectively avoids the generation of phosphorus-containing wastewater. The entire process is more efficient and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.
[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0031] Figure 1 A flow chart of a method for preparing an epoxy coating on the surface of a bonded magnet provided in an embodiment of the present invention.
[0032] Figure 2 This is a sample image before salt spray in Example 1 of the present invention;
[0033] Figure 3 This is a sample image after salt spray in Example 1 of the present invention;
[0034] Figure 4 This is a sample image before salt spray in Example 2 of the present invention;
[0035] Figure 5 This is a sample image after salt spray in Example 2 of the present invention;
[0036] Figure 6 This is a sample image before salt spray in Example 3 of the present invention;
[0037] Figure 7 This is a sample image after salt spray in Example 3 of the present invention;
[0038] Figure 8 This is a sample image before salt spray in Comparative Example 1 of the present invention;
[0039] Fig. 9 This is a sample diagram after salt spray in Comparative Example 1 of the present invention;
[0040] Fig.10 This is a sample image before salt spray in Comparative Example 2 of the present invention;
[0041] Fig.11 This is a sample diagram after salt spray in Comparative Example 2 of the present invention;
[0042] Fig.12 This is a sample image before salt spray in Comparative Example 3 of the present invention;
[0043] Fig.13 This is a sample picture before salt spray in Comparative Example 3 of the present invention. DETAILED DESCRIPTION
[0044] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0045] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0046] In a first aspect, the present invention provides a method for preparing an epoxy coating on the surface of a bonded magnet, such as Figure 1 As shown, the method comprises the following steps:
[0047] The bonded magnet is chamfered, and then ultrasonically cleaned with a baking soda solution, washed with a first deionized water, and washed with hot deionized water to obtain a first bonded magnet;
[0048] Performing electrophoresis treatment on the first bonded magnet using electrophoretic paint containing epoxy resin, and then performing a second deionized water wash to obtain a second bonded magnet;
[0049] The second bonded magnet is cured to form an epoxy coating on the surface of the bonded magnet.
[0050] Compared with the prior art, the modified method for preparing epoxy coating on the surface of a bonded magnet provided by the present invention comprises: magnet → chamfering → ultrasonic cleaning with baking soda solution → deionized water washing → hot deionized water washing → electrophoresis → deionized water washing → baking, which simplifies the existing epoxy coating preparation process steps and effectively avoids the generation of phosphorus-containing wastewater, making the entire process more efficient and environmentally friendly.
[0051] In some specific embodiments, the working condition parameters of the chamfer include: the chamfer is C0.5.
[0052] In some specific embodiments, the working condition parameters of the baking soda solution ultrasonic cleaning include: the pH of the baking soda solution is 7-8, the ultrasonic power is 10K-14KW, the time is 1-1.5min, and the room temperature.
[0053] In some specific embodiments, the working condition parameters of the first deionized water washing and the second deionized water washing include: temperature of 20° C. to 30° C., time of 1 to 1.5 min, and number of cleaning times of 1 to 3 times.
[0054] In some specific embodiments, the working condition parameters of the hot deionized water washing include: a temperature of 65° C. to 70° C. and a time of 40 to 60 seconds.
[0055] In some specific embodiments, the electrophoretic paint containing epoxy resin includes a color paste, epoxy resin and deionized water in a weight ratio of 1:4:5.
[0056] In some specific embodiments, the conductivity of the electrophoretic paint containing epoxy resin is 1400 μS / cm to 1600 μS / cm.
[0057] In some specific embodiments, the preparation of the electrophoretic paint containing epoxy resin includes the following process: PPG electrophoretic paint is used, and the mass ratio of color paste: resin: deionized water is 1:4:5. The solid content of the prepared electrophoretic paint is 18% to 20%, and the ash content is between 0.99 and 1.02. When the temperature of the electrophoretic liquid is 29°C to 31°C, the conductivity of the electrophoretic paint is 1400μS / cm to 1600μS / cm. The prepared electrophoretic paint should be fully mixed and matured for at least 24 to 48 hours.
[0058] In some specific embodiments, the step of electrophoresis treatment includes the following process:
[0059] The electrophoresis is performed by adopting a segmented voltage control method, wherein the segmented voltage control method is divided into six segments;
[0060] The first stage: the voltage rises from 0 to 130V at a constant speed, taking 100s;
[0061] The second stage: the voltage is maintained at 130V for 30 seconds;
[0062] The third stage: the voltage rises from 130V to 170V, which takes 30s;
[0063] The fourth stage: the voltage is maintained at 170V for 20s;
[0064] The fifth stage: the voltage rises from 170V to 210V at a constant speed, which takes 30s;
[0065] In the sixth section, the voltage is maintained at 210V for 10 seconds.
[0066] In some specific embodiments, the curing step includes the following process:
[0067] The second bonded magnet is first kept at 80-90° C. for 15 min, then kept at 110-120° C. for 15 min, and finally kept at 165-170° C. for 30 min.
[0068] It should be noted that the components and raw materials involved in the method for preparing the epoxy coating on the surface of the bonded magnet provided in the embodiment of the present invention can be directly commercially available unless otherwise specified or described. At the same time, the operation steps involved can be performed with reference to the existing technology or using existing equipment unless otherwise specified.
[0069] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are intended only to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples that do not specify specific conditions are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.
[0070] Example 1
[0071] This example provides a method for preparing an epoxy coating on the surface of a bonded magnet, comprising the following steps:
[0072] Preparation of electrophoretic paint: PPG electrophoretic paint is used, and its mass ratio is color paste: epoxy resin: deionized water = 1:4:5. The solid content of the prepared electrophoretic paint is 18% to 20%, and the ash content is between 0.99 and 1.02. When the temperature of the electrophoretic liquid is 29℃ to 31℃, the conductivity of the electrophoretic paint is 1400μS / cm to 1600μS / cm. The prepared electrophoretic paint should be fully mixed and matured for 36 hours.
[0073] Setting of electrophoresis curve: electrophoresis was performed by controlled voltage method, which was divided into six sections; the first section: the voltage increased from 0 to 130V at a constant speed for 100s, the second section: the voltage was kept at 130V for 30s, the third section: the voltage increased from 130V to 170V for 30s, the fourth section: the voltage was kept at 170V for 20s, the fifth section: the voltage increased from 170V to 210V at a constant speed for 30s, the sixth section: the voltage was kept at 210V for 10s;
[0074] Magnet chamfering: Chamfer the inner and outer arc edges of the bonding magnet with a size of φ22.1*φ12*36, and the chamfer is C0.5;
[0075] Magnet cleaning: First, rinse the dust on the chamfered magnet surface with tap water, then put the magnet into a 1% sodium bicarbonate deionized water solution (pH 7.5), and ultrasonically clean the magnet for 1.5 minutes at an ultrasonic power of 14KW, and then rinse the magnet three times with deionized water; then: clamp the magnet with a hanger, and then soak it in deionized water at a temperature of 65°C for 60 seconds, take it out, and cool it for 1.5 minutes;
[0076] Electrophoresis treatment: The cleaned magnet is electrophoresed using the prepared electrophoresis paint and according to the setting of the electrophoresis curve. After the electrophoresis is completed, the magnet is rinsed three times with deionized water;
[0077] Curing treatment: The magnet after electrophoresis treatment and cleaning is first kept at 85°C for 15 minutes, then kept at 105°C for 15 minutes, and finally kept at 168°C for 30 minutes to form an epoxy coating on the surface of the bonded magnet.
[0078] Example 2
[0079] This example provides a method for preparing an epoxy coating on the surface of a bonded magnet, comprising the following steps:
[0080] Preparation of electrophoretic paint: PPG electrophoretic paint is used, and its mass ratio is color paste: epoxy resin: deionized water = 1:4:5. The solid content of the prepared electrophoretic paint is 18% to 20%, and the ash content is between 0.99 and 1.02. When the temperature of the electrophoretic liquid is 29℃ to 31℃, the conductivity of the electrophoretic paint is 1400μS / cm to 1600μS / cm. The prepared electrophoretic paint should be fully mixed and matured for 36 hours.
[0081] Setting of electrophoresis curve: electrophoresis was performed by controlled voltage method, which was divided into six sections; the first section: the voltage increased from 0 to 130V at a constant speed for 100s, the second section: the voltage was kept at 130V for 30s, the third section: the voltage increased from 130V to 170V for 30s, the fourth section: the voltage was kept at 170V for 20s, the fifth section: the voltage increased from 170V to 210V at a constant speed for 30s, the sixth section: the voltage was kept at 210V for 10s;
[0082] Magnet chamfering: Chamfer the inner and outer arc edges of the bonding magnet with a size of φ22.1*φ12*36, and the chamfer is C0.5;
[0083] Magnet cleaning: First, rinse the dust on the chamfered magnet surface with tap water, then put the magnet into a 3% sodium bicarbonate deionized water solution (pH 7.8), and ultrasonically clean the magnet for 1 minute at an ultrasonic power of 12KW, and then rinse the magnet three times with deionized water; then: clamp the magnet with a hanger, and then soak it in deionized water at a temperature of 70°C for 40 seconds, take it out, and cool it for 1.5 minutes;
[0084] Electrophoresis treatment: The cleaned magnet is electrophoresed using the prepared electrophoresis paint and according to the setting of the electrophoresis curve. After the electrophoresis is completed, the magnet is rinsed three times with deionized water;
[0085] Curing treatment: The magnet after electrophoresis treatment and cleaning is first kept at 80°C for 15 minutes, then kept at 110°C for 15 minutes, and finally kept at 170°C for 30 minutes to form an epoxy coating on the surface of the bonded magnet.
[0086] Example 3
[0087] This example provides a method for preparing an epoxy coating on the surface of a bonded magnet, comprising the following steps:
[0088] Preparation of electrophoretic paint: PPG electrophoretic paint is used, and its mass ratio is color paste: epoxy resin: deionized water = 1:4:5. The solid content of the prepared electrophoretic paint is 18% to 20%, and the ash content is between 0.99 and 1.02. When the temperature of the electrophoretic liquid is 29℃ to 31℃, the conductivity of the electrophoretic paint is 1400μS / cm to 1600μS / cm. The prepared electrophoretic paint should be fully mixed and matured for 36 hours.
[0089] Setting of electrophoresis curve: electrophoresis was performed by controlled voltage method, which was divided into six sections; the first section: the voltage increased from 0 to 130V at a constant speed for 100s, the second section: the voltage was kept at 130V for 30s, the third section: the voltage increased from 130V to 170V for 30s, the fourth section: the voltage was kept at 170V for 20s, the fifth section: the voltage increased from 170V to 210V at a constant speed for 30s, the sixth section: the voltage was kept at 210V for 10s;
[0090] Magnet chamfering: Chamfer the inner and outer arc edges of the bonding magnet with a size of φ22.1*φ12*36, and the chamfer is C0.5;
[0091] Magnet cleaning: First, rinse the dust on the chamfered magnet surface with tap water, then put the magnet into a 6% sodium bicarbonate deionized water solution (pH 8), and ultrasonically clean the magnet for 1 minute at an ultrasonic power of 10KW, and then rinse the magnet three times with deionized water; then: clamp the magnet with a hanger, and then soak it in deionized water at a temperature of 68°C for 50 seconds, take it out, and cool it for 1.5 minutes;
[0092] Electrophoresis treatment: The cleaned magnet is electrophoresed using the prepared electrophoresis paint and according to the setting of the electrophoresis curve. After the electrophoresis is completed, the magnet is rinsed three times with deionized water;
[0093] Curing treatment: The magnet after electrophoresis treatment and cleaning is first kept at 90°C for 15 minutes, then kept at 120°C for 15 minutes, and finally kept at 165°C for 30 minutes to form an epoxy coating on the surface of the bonded magnet.
[0094] Comparative Example 1
[0095] This example provides a typical existing method for preparing epoxy coating on the surface of bonded magnets, including: magnet → chamfering (grinding and polishing) → tap water ultrasonic cleaning → sealing → deionized water washing → curing → phosphating → deionized water washing → electrophoresis → deionized water washing → baking, specifically including the following steps: preparing electrophoretic paint: using PPG electrophoretic paint, the mass ratio of which is color paste: epoxy resin: deionized water = 1:4:5, the prepared electrophoretic paint has a solid content of 18% to 20%, and an ash content of 0.99 to 1.02; when the temperature of the electrophoretic liquid is 29°C to 31°C, the conductivity of the electrophoretic paint is 1400μS / cm to 1600μS / cm; the prepared electrophoretic paint should be fully mixed and aged for 36 hours;
[0096] Setting of electrophoresis curve: electrophoresis was performed by controlled voltage method, which was divided into six sections; the first section: the voltage increased from 0 to 130V at a constant speed for 100s, the second section: the voltage was kept at 130V for 30s, the third section: the voltage increased from 130V to 170V for 30s, the fourth section: the voltage was kept at 170V for 20s, the fifth section: the voltage increased from 170V to 210V at a constant speed for 30s, the sixth section: the voltage was kept at 210V for 10s;
[0097] Magnet chamfering: Chamfer the inner and outer arc edges of the bonding magnet with a size of φ22.1*φ12*36, and the chamfer is C0.5;
[0098] Magnet cleaning: First, rinse the dust on the surface of the chamfered magnet with tap water until the rinse water is no longer turbid, then use tap water ultrasonic cleaning at 14KW for 1.5 minutes. Then rinse the magnet twice with deionized water. Then immerse the magnet in a 5% sealing agent for 1 minute, take it out and rinse it twice with deionized water, and cure it at 80°C for 10 minutes. After curing, immerse the magnet in a 5% phosphating solution for 1 minute, take it out and rinse it twice with deionized water. Clamp the magnet with a hanger.
[0099] Electrophoresis treatment: The cleaned magnet is electrophoresed using the prepared electrophoresis paint and according to the setting of the electrophoresis curve. After the electrophoresis is completed, the magnet is rinsed three times with deionized water;
[0100] Curing treatment: The magnet after electrophoresis treatment and cleaning is first kept at 85°C for 15 minutes, then kept at 105°C for 15 minutes, and finally kept at 168°C for 30 minutes to form an epoxy coating on the surface of the bonded magnet.
[0101] Comparative Example 2
[0102] This example provides a method for preparing an epoxy coating on the surface of a bonded magnet, which differs from Example 1 only in that: Pretreatment: First, rinse the dust on the surface of the magnet after chamfering with tap water until the rinse water is no longer turbid, and then use tap water for ultrasonic cleaning at a power of 14KW for 1.5 minutes. Then rinse the magnet twice with deionized water. Then immerse the magnet in a sealing agent with a mass fraction of 5% for 1 minute, take it out and rinse it with deionized water twice, and cure it at 80°C for 10 minutes. The cured magnet is immersed in a phosphating solution with a mass fraction of 10% for 1 minute, and then rinse it with deionized water twice after taking it out; the remaining steps and parameters are the same.
[0103] Comparative Example 3
[0104] This example provides a method for preparing an epoxy coating on the surface of a bonded magnet, which differs from Example 1 only in that: Pretreatment: First, rinse the dust on the surface of the magnet after chamfering with tap water until the rinse water is no longer turbid, and then use tap water for ultrasonic cleaning at a power of 14KW for 1.5 minutes. Then rinse the magnet twice with deionized water. Then immerse the magnet in a sealing agent with a mass fraction of 10% for 30 seconds, take it out, rinse it with deionized water twice, and cure it at 80°C for 10 minutes. The cured magnet is immersed in a phosphating solution with a mass fraction of 10% for 1 minute, and then rinse it with deionized water twice after taking it out; the remaining steps and parameters are the same.
[0105] Test Case
[0106] In this example, the corrosion resistance of the bonded magnets with epoxy coating on the surface obtained in the above-mentioned embodiments and comparative examples was tested.
[0107] Test method: The salt spray test was performed on the embodiments and comparative examples using the GBT10125-2021 artificial atmosphere corrosion test. The salt spray time was 600 hours.
[0108] The test results are shown in Table 1 and Figure 2-Figure 13 shown.
[0109] Table 1
[0110]
[0111] The test results show that after 600 hours of salt spray, the samples of the embodiment and the comparative example only have rust on the inner arc edge (because there are hanging points on the inner arc edge, the coating at the hanging points is very thin and easily corroded), and there is no rust visible to the naked eye on the outer arc surface. Therefore, the embodiment and the comparative example achieve the same effect, indicating that the method used in the embodiment of the present invention can replace the method of the comparative example. The difference between the two before and after the test is the inner ring edge of the end face. The samples after the test all have rust on the inner ring edge.
[0112] Various embodiments of the present invention may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present invention; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0113] The foregoing is merely a specific embodiment of the present invention, which enables those skilled in the art to understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features claimed herein.
Claims
1. A method for preparing an epoxy coating on the surface of a bonded magnet, characterized in that: The method comprises the following steps: The bonded magnet is chamfered, and then ultrasonically cleaned with a baking soda solution, washed with a first deionized water, and washed with hot deionized water to obtain a first bonded magnet; Performing electrophoresis treatment on the first bonded magnet using electrophoretic paint containing epoxy resin, and then performing a second deionized water wash to obtain a second bonded magnet; The second bonded magnet is cured to form an epoxy coating on the surface of the bonded magnet.
2. The method for preparing an epoxy coating on the surface of a bonded magnet according to claim 1, characterized in that: The working condition parameters of the chamfer include: the chamfer is C0.
5.
3. The method for preparing an epoxy coating on the surface of a bonded magnet according to claim 1, characterized in that: The working condition parameters of the baking soda solution ultrasonic cleaning include: the pH of the baking soda solution is 7-8, the ultrasonic power is 10K-14KW, and the time is 1-1.5min.
4. The method for preparing an epoxy coating on the surface of a bonded magnet according to claim 1, characterized in that: The working condition parameters of the first deionized water washing and the second deionized water washing include: temperature of 20° C. to 30° C., time of 1 to 1.5 minutes, and number of washings of 2 to 3 times.
5. The method for preparing an epoxy coating on the surface of a bonded magnet according to claim 1, characterized in that: The working condition parameters of the hot deionized water washing include: temperature of 65° C. to 70° C., and time of 40 to 60 seconds.
6. The method for preparing an epoxy coating on the surface of a bonded magnet according to claim 1, characterized in that: The epoxy resin-containing electrophoretic paint comprises a color paste, an epoxy resin and deionized water in a weight ratio of 1:4:
5.
7. The method for preparing an epoxy coating on the surface of a bonded magnet according to claim 6, characterized in that: The conductivity of the electrophoretic paint containing epoxy resin is 1400 μS / cm to 1600 μS / cm.
8. The method for preparing an epoxy coating on the surface of a bonded magnet according to claim 1, characterized in that: The electrophoresis treatment step includes the following process: The electrophoresis is performed by adopting a segmented voltage control method, wherein the segmented voltage control method is divided into six segments; The first stage: the voltage rises from 0 to 130V at a constant speed, taking 100s; The second stage: the voltage is maintained at 130V for 30 seconds; The third stage: the voltage rises from 130V to 170V, which takes 30s; The fourth stage: the voltage is maintained at 170V for 20s; The fifth stage: the voltage rises from 170V to 210V at a constant speed, which takes 30s; In the sixth section, the voltage is maintained at 210V for 10 seconds.
9. The method for preparing an epoxy coating on the surface of a bonded magnet according to claim 1, characterized in that: The curing process comprises the following steps: The second bonded magnet is first kept at 80-90° C. for 15 min, then kept at 110-120° C. for 15 min, and finally kept at 165-170° C. for 30 min.