Impregnation system for fiber surface treatment and fiber and preparation method thereof

By using a one-bath treatment with water-soluble epoxy resin and blocked isocyanate, and a two-bath treatment with hydroxyl acrylic resin and amino resin, the environmental pollution problem during fiber-rubber composite is solved, achieving efficient and environmentally friendly interfacial bonding and simplifying the production process.

CN118910890APending Publication Date: 2024-11-08BEIJING UNIV OF CHEM TECH
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202310504623.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-06
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing technologies for fiber-rubber composites require harsh reaction conditions and complex equipment, causing significant damage to the fibers. Furthermore, the accelerators used are harmful to the environment, making it difficult to achieve efficient and environmentally friendly interfacial bonding.

Method used

The first-bath impregnation solution consists of deionized water, water-soluble epoxy resin, and blocked isocyanate, while the second-bath impregnation solution consists of deionized water, hydroxyl acrylic dispersion resin, amino resin, and rubber latex. The use of resorcinol, formaldehyde, and accelerators is avoided. A stable three-dimensional resin network is formed through simple room temperature treatment to enhance interfacial adhesion.

Benefits of technology

It achieves efficient interfacial bonding between fibers and rubber, simplifies the production process, reduces environmental pollution, and the impregnation solution remains stable at room temperature for a long time, making it suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004215257860000021
    Figure BDA0004215257860000021
  • Figure BDA0004215257860000031
    Figure BDA0004215257860000031
  • Figure BDA0004215257860000151
    Figure BDA0004215257860000151
Patent Text Reader

Abstract

The invention discloses a gum dipping system for fiber surface treatment, a fiber and a preparation method, the gum dipping system comprises a first-bath gum dipping solution and a second-bath gum dipping solution, and the first-bath gum dipping solution is prepared from the following raw materials: deionized water, water-soluble epoxy resin and blocked isocyanate; the two-bath impregnation liquid is prepared from the following raw materials: deionized water, hydroxy acrylic dispersion resin, amino resin and rubber latex; and the amino resin is one of CYMEL-325 and CYMEL-327 (CYMEL-325). According to the gum dipping system, under the condition that an accelerant is not adopted, the environmental problem caused by using the accelerant is solved, meanwhile, the performance of the bonding strength between fibers dipped with the gum dipping system and a rubber interface meets the requirement, and the gum dipping system is suitable for industrial application.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Field

[0002] The invention relates to the technical field of high-performance fiber-reinforced rubber composite materials, and in particular to a fiber surface treatment impregnation system and a preparation method thereof; the invention also relates to a fiber and a preparation method thereof. Background Art

[0003] High-performance fibers have excellent performance characteristics such as low density, light weight, puncture resistance and fatigue resistance. In recent years, they have been used in tire skeleton materials and tire belt layers. Due to the inertness of the surface functional groups of high-performance fibers, when compounding with rubber, the fibers need to be pretreated so that they can form chemical bonds with the rubber for better interfacial bonding. The one-bath treatment activates the fiber surface and produces active groups. The second bath uses RFL solution to dip the fibers to enhance the interfacial bonding between the fibers and the rubber compound. However, the traditional one-bath treatment methods such as plasma, ultraviolet-induced grafting, and fluorination have the disadvantages of harsh reaction conditions, complex equipment, and great damage to the fibers. The traditional two-bath resorcinol-formaldehyde-latex (RFL) dipping system contains resorcinol, formaldehyde, etc., which are highly harmful to the human body and the environment.

[0004] CN115748256A discloses an environmentally friendly impregnation system for fiber surface treatment, a preparation method thereof and an impregnation treatment method. The environmentally friendly impregnation system for fiber surface treatment comprises hydroxy acrylic resin, amino resin, epoxy resin, blocked isocyanate, accelerator, rubber latex and deionized water. The accelerator is selected from at least one of amine-blocked dinonylnaphthalene disulfonic acid, amine-blocked dinonylnaphthalene sulfonic acid, amine-blocked dodecylbenzene sulfonic acid or amine-blocked p-toluene sulfonic acid. The accelerator has a direct effect on the adhesion performance of the cord and rubber after the dipping treatment, so the accelerator is used in the prior art. And in order to facilitate long-term storage, the aforementioned amine-blocked accelerator is generally used. However, some accelerators, such as p-toluene sulfonic acid, are harmful to the environment and can cause pollution to water bodies and the atmosphere.

[0005] Therefore, developing a fiber surface treatment dipping system without using an accelerator, which can not only ensure that the performance of the interfacial bonding strength between the fiber and rubber after dipping meets the requirements, but also solve the environmental problems caused by the use of accelerators, has become an urgent problem to be solved by technical personnel in this field. Summary of the invention

[0006] In order to solve the technical problems existing in the prior art, the present invention provides a fiber surface treatment impregnation system and a preparation method thereof, and also provides a fiber treated by the aforementioned impregnation system and a preparation method of the fiber. The present invention uses a two-bath method for the surface treatment of the fiber, wherein the first-bath impregnation solution is prepared with blocked isocyanate, water-soluble epoxy resin, and deionized water. Compared with treatment methods such as plasma, ultraviolet-induced grafting, and fluorination, the one-bath treatment of the present invention has the advantages of not harsh reaction conditions, simple equipment, and little damage to the fiber. The second-bath impregnation solution uses hydroxyl acrylic resin dispersion resin, amino resin, and rubber latex as main raw materials. Compared with the two-bath impregnation solution of the prior art, the present invention does not use substances harmful to the human body and the environment such as resorcinol, formaldehyde, and accelerators, and the bonding performance is close to that of the fiber treated by the RFL impregnation system, which is suitable for industrial application. At the same time, the impregnation solution of the present application is stable, and has the advantages of long-term storage, long-term use, and convenience for industrial continuous production.

[0007] One of the objects of the present invention is to provide a dipping system for fiber surface treatment, the dipping system comprising a first-bath dipping solution and a second-bath dipping solution;

[0008] The one-bath dipping solution is prepared from deionized water, a water-soluble epoxy resin and a blocked isocyanate; based on 100 parts by weight of deionized water,

[0009] Deionized water 100 parts by weight

[0010] 1-3 parts by weight of water-soluble epoxy resin

[0011] Blocked isocyanate 8-10 parts by weight

[0012] The second bath dipping solution is prepared from deionized water, hydroxyl acrylic acid dispersion resin, amino resin and rubber latex; based on 100 parts by weight of deionized water,

[0013]

[0014] Wherein, the amino resin is at least one of CYMEL-325, CYMEL-327, and XT-303.

[0015] Furthermore, the one-bath dipping solution is calculated based on 100 parts by weight of deionized water.

[0016] Deionized water 100 parts by weight

[0017] 1-2 parts by weight of water-soluble epoxy resin

[0018] Blocked isocyanate 8-9 parts by weight

[0019] and / or

[0020] The second bath dipping solution is calculated based on 100 parts by weight of deionized water.

[0021]

[0022] Furthermore, the weight ratio of the amino resin to the hydroxylated acrylic dispersion resin is 0.36-0.42:1; and / or

[0023] The weight ratio of the rubber latex to the hydroxylated acrylic dispersion resin is 1:0.65-0.75; and / or

[0024] The mass ratio of the first bath dipping solution to the second bath dipping solution is 1:2-2.5.

[0025] Furthermore, the solid content of the rubber latex is 20% to 40%; the solid content of the hydroxylated acrylic dispersion resin is 40% to 50%, preferably 41% to 45%.

[0026] Furthermore, the hydroxyl value of the hydroxylated acrylic dispersion resin is at least one of 2.0 and 4.2.

[0027] Further, the water-soluble epoxy resin can be selected from sorbitol glycidyl ether, diphenol propane type epoxy resin, bisphenol A type liquid epoxy resin, trimethylolpropane glycidyl ether, tetraphenol ethane tetraglycidyl ether epoxy resin. The water-soluble epoxy resin can be selected from one or a combination of multiple types, and the technician can select according to the actual situation.

[0028] The blocked isocyanate is an isocyanate blocked by a blocking agent. Under the action of the blocking agent, the isocyanate is stable. When the subsequent cord is placed in a bath dipping solution for dipping, the isocyanate is unblocked. The isocyanate can be selected from trimethyl-1,6-hexamethylene diisocyanate, tetramethylene diisocyanate, tetramethyl diisocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate. The selection of isocyanate can be one or a combination of multiple, and the technician can choose according to the actual situation. The blocking agent is caprolactam, butanone oxime, and phenol. The selection of the blocking agent can be one or a combination of multiple, and the technician can choose according to the actual situation.

[0029] The rubber latex is selected from butyl pyridine latex, styrene butadiene latex, styrene butadiene pyridine latex, chloroprene latex, nitrile latex. The rubber latex can be selected from one or a combination of multiple types, and the technician can select according to the actual situation.

[0030] The second object of the present invention is to provide a method for preparing the impregnation system for fiber surface treatment according to the first object of the present invention, the method comprising:

[0031] The water-soluble epoxy resin and the blocked isocyanate are added into the deionized water to obtain a first-bath dipping solution; and the hydroxylated acrylic dispersion resin, the amino resin and rubber latex are added into the deionized water to obtain a second-bath dipping solution.

[0032] The present invention can specifically adopt the following technical solutions:

[0033] The preparation method comprises the following steps:

[0034] Preparation of one-bath dipping solution: Add water-soluble epoxy resin to deionized water and stir at room temperature for 5 to 10 minutes to obtain a uniform aqueous solution, then add blocked isocyanate and stir at room temperature for 1.5 to 2 hours to obtain a one-bath dipping solution.

[0035] Preparation of the second-bath dipping solution: Add hydroxy acrylic dispersion resin and amino resin into deionized water, then add rubber latex and stir at room temperature for 1.5 to 2 hours to obtain the second-bath dipping solution.

[0036] The amino resin is CYMEL-325 or CYMEL-327. The mass ratio of the first bath dipping solution to the second bath dipping solution is 1:2-2.5.

[0037] In the actual preparation process, the water-soluble epoxy resin can be selected from sorbitol glycidyl ether, diphenol propane type epoxy resin, bisphenol A type liquid epoxy resin, trimethylolpropane glycidyl ether, tetraphenol ethane tetraglycidyl ether epoxy resin. The water-soluble epoxy resin can be selected from one or a combination of multiple types, and the technician can select according to the actual situation. However, this does not constitute a limitation on the water-soluble epoxy resin.

[0038] In the actual preparation process, the isocyanate can be selected from trimethyl-1,6-hexamethylene diisocyanate, tetramethylene diisocyanate, tetramethyl diisocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate. The selection of isocyanate can be one or a combination of multiple, and the technician can choose according to the actual situation. The blocking agent is caprolactam, butanone oxime, and phenol. The selection of the blocking agent can be one or a combination of multiple, and the technician can choose according to the actual situation. But this does not constitute a limitation on blocked isocyanates.

[0039] In the actual preparation process, the rubber latex is selected from butyl pyridine latex, styrene butadiene latex, styrene butadiene pyridine latex, chloroprene latex, butadiene nitrile latex. The selection of rubber latex can be one or a combination of multiple types, and the technician can select according to the actual situation. However, this does not constitute a limitation on the rubber latex.

[0040] In the actual preparation process, the stirring time can be adjusted according to the specific types and amounts of the water-soluble epoxy resin, blocked isocyanate, hydroxylated acrylic dispersion resin, amino resin and rubber latex.

[0041] The third object of the present invention is to provide a fiber dipped in the dipping system for fiber surface treatment according to one of the objects of the present invention, wherein the fiber is obtained by dipping in the dipping system described in any one of claims 1 to 6.

[0042] Furthermore, the fiber is one of nylon fiber cords, aramid cords, and polyarylate fiber cords, or a mixed cord of two or more thereof.

[0043] The fourth object of the present invention is to provide a method for preparing the third fiber of the present invention, the method comprising

[0044] The cord is placed in a first-bath dipping solution for dipping, drying and curing, and then placed in a second-bath dipping solution for dipping, drying and curing to obtain the cord.

[0045] The present invention can specifically adopt the following technical solutions:

[0046] The preparation method comprises the following steps:

[0047] The cord is first placed in a bath of dipping solution for dipping, and is dipped at room temperature for 4 to 6 seconds; then the dipped cord is placed in an oven at 130 to 150°C for drying for 70 to 73 seconds, and cured at 230 to 250°C for 70 to 73 seconds. The first bath reaction is the reaction of isocyanate with fiber, and then the water-soluble epoxy resin reacts with isocyanate to activate the fiber surface, which is convenient for reaction with the subsequent second bath dipping solution.

[0048] The aramid cord impregnated with glue is then placed in the second bath impregnation solution for impregnation, and is impregnated for 4 to 6 seconds at room temperature; the impregnated cord is then placed in an oven at 130 to 150°C for drying for 70 to 73 seconds, and cured at 230 to 250°C for 70 to 73 seconds, so that the impregnation solution adheres to the surface of the cord, and the impregnated cord is obtained. The second bath reaction forms a cross-linked network structure of hydroxyl acrylic dispersion resin and amino resin in the formed interface layer, which can react with the fiber surface treated in the first bath to form a three-dimensional resin, and the formed three-dimensional resin can wrap the latex inside, and the latex particles can be co-vulcanized with the rubber.

[0049] During the dipping process, the dipping time, drying temperature, drying time, curing temperature and curing time can be adjusted according to the specific types and amounts of water-soluble epoxy resin, blocked isocyanate, hydroxy acrylic dispersion resin, amino resin and rubber latex, and the final cord adhesive content is 4-7%.

[0050] Compared with the prior art, the present invention has the following beneficial effects:

[0051] 1. The dipping system of the present invention does not contain substances harmful to human body and environment such as resorcinol, formaldehyde and accelerator, and the whole system is water-soluble substances and does not contain harmful organic solvents.

[0052] 2. After the fiber is dipped in the two-bath dipping system composed of the hydroxyl acrylic dispersion resin and the amino resin latex of the present invention, its bonding effect is equivalent to that of the RFL system, meeting the needs of industrial production.

[0053] 3. The preparation process of the dipping system of the present invention is simpler, the production process is simplified, and the production cost is saved.

[0054] 4. After the dipping system of the present invention is placed at room temperature for three days, the components of the dipping solution remain unchanged, the bonding effect is equivalent to that of the initial formulation, and it can be used continuously, which is conducive to the industrial production of fibers. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] Figure 1 This is a rubber attachment diagram of the polyarylate cord of Example 1 of the present invention after H sampling;

[0056] Figure 2 This is a rubber attachment diagram of the polyarylate cord of Example 2 of the present invention after H sampling;

[0057] Figure 3 This is a rubber attachment diagram of the polyarylate cord of Example 3 of the present invention after H sampling;

[0058] Figure 4 This is a rubber attachment diagram of the polyarylate cord of Comparative Example 1 of the present invention after H sampling;

[0059] Figure 5 This is a rubber attachment diagram of the polyarylate cord of comparative example 2 of the present invention after H sampling;

[0060] Figure 6 This is a rubber attachment diagram of the polyarylate cord of comparative example 3 of the present invention after H sampling;

[0061] Figure 7 This is a rubber attachment diagram of the polyarylate cord of comparative example 4 of the present invention after H sampling;

[0062] Figure 8This is an AFM image of the hydroxy acrylic dispersion resin-amino resin-latex dipping solution after freeze drying treatment in Example 2 of the present invention;

[0063] Fig. 9 It is the H extraction force diagram of the dipping solution of Example 2 of the present invention after being placed for 24h, 48h and 72h. DETAILED DESCRIPTION

[0064] The present invention is described in detail below in conjunction with specific drawings and embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the content of the present invention still fall within the scope of protection of the present invention.

[0065] The raw materials used in the examples are all conventional commercially available raw materials. It should be noted that the hydroxylated acrylic dispersion resin of the present invention is in the form of an emulsion, purchased from Foshan Dongjie New Material Technology Co., Ltd., and is not in a solid form. The percentage of the butylpyrrolidone latex of the present invention is 40wt%.

[0066] The equipment used in the examples are all conventional production equipment.

[0067] Example 1

[0068] A two-bath dipping system of hydroxylated acrylic dispersion resin-amino resin-latex for surface treatment of polyarylate cord, the production steps of which are as follows:

[0069] (1) Preparation of a one-bath dipping solution: 1.48 parts by weight of sorbitol glycidyl ether was added to 100 parts by weight of deionized water and stirred at room temperature for 5 minutes to obtain a uniform aqueous solution, and then 9.86 parts by weight of caprolactam-blocked 4,4'-diphenylmethane diisocyanate was added and stirred at room temperature for 2 hours to obtain a one-bath dipping solution.

[0070] (2) Preparation of the second-bath dipping solution: 21.34 parts by weight of a hydroxyl acrylic dispersion resin having a hydroxyl value of 2.0 and 8.89 parts by weight of CYMEL-325 amino resin were added to 100 parts by weight of deionized water, and then 108 parts by weight of butylpyrrolidone latex was added and stirred at room temperature for 2 hours to obtain the second-bath dipping solution.

[0071] (3) Dipping treatment: The polyarylate cord is first dipped in a first-bath dipping solution for dipping, and is dipped at room temperature for 5 seconds; the dipped cord is then placed in an oven at 150°C for drying for 72 seconds and cured at 230°C for 72 seconds, and then the dipped aramid cord is dipped in a second-bath dipping solution for dipping, and is dipped at room temperature for 5 seconds; the dipped cord is then placed in an oven at 150°C for drying for 72 seconds and cured at 230°C for 72 seconds, so that the dipping solution adheres to the surface of the aramid cord, thereby obtaining the dipped polyarylate cord.

[0072] Example 2

[0073] A two-bath dipping system of hydroxylated acrylic dispersion resin-amino resin-latex for surface treatment of polyarylate cord, the production steps of which are as follows:

[0074] (1) Preparation of a one-bath dipping solution: 1.48 parts by weight of sorbitol glycidyl ether was added to 100 parts by weight of deionized water and stirred at room temperature for 5 minutes to obtain a uniform aqueous solution, and then 9.86 parts by weight of caprolactam-blocked 4,4'-diphenylmethane diisocyanate was added and stirred at room temperature for 2 hours to obtain a one-bath dipping solution.

[0075] (2) Preparation of the second-bath dipping solution: 21.34 parts by weight of a hydroxyl acrylic dispersion resin having a hydroxyl value of 4.2 and 8.89 parts by weight of CYMEL-325 amino resin were added to 100 parts by weight of deionized water, and then 108 parts by weight of butylpyrrolidone latex was added and stirred at room temperature for 2 hours to obtain the second-bath dipping solution.

[0076] (3) Dipping treatment: The polyarylate cord is first dipped in a first-bath dipping solution for dipping, and is dipped at room temperature for 5 seconds; the dipped cord is then placed in an oven at 150°C for drying for 72 seconds and cured at 230°C for 72 seconds, and then the dipped aramid cord is dipped in a second-bath dipping solution for dipping, and is dipped at room temperature for 5 seconds; the dipped cord is then placed in an oven at 150°C for drying for 72 seconds and cured at 230°C for 72 seconds, so that the dipping solution adheres to the surface of the aramid cord, thereby obtaining the dipped polyarylate cord.

[0077] Example 3

[0078] A two-bath dipping system of hydroxylated acrylic dispersion resin-amino resin-latex for surface treatment of polyarylate cord, the production steps of which are as follows:

[0079] (1) Preparation of a one-bath dipping solution: 1.48 parts by weight of sorbitol glycidyl ether was added to 100 parts by weight of deionized water and stirred at room temperature for 5 minutes to obtain a uniform aqueous solution, and then 9.86 parts by weight of caprolactam-blocked 4,4'-diphenylmethane diisocyanate was added and stirred at room temperature for 2 hours to obtain a one-bath dipping solution.

[0080] (2) Preparation of the second-bath dipping solution: 21.34 parts by weight of a hydroxyl acrylic dispersion resin having a hydroxyl value of 4.2 and 8.89 parts by weight of CYMEL-327 amino resin were added to 100 parts by weight of deionized water, and then 108 parts by weight of butylpyrrolidone latex was added and stirred at room temperature for 2 hours to obtain the second-bath dipping solution.

[0081] (3) Dipping treatment: The polyarylate cord is first dipped in a first-bath dipping solution for dipping, and is dipped at room temperature for 5 seconds; the dipped cord is then placed in an oven at 150°C for drying for 72 seconds and cured at 230°C for 72 seconds, and then the dipped aramid cord is dipped in a second-bath dipping solution for dipping, and is dipped at room temperature for 5 seconds; the dipped cord is then placed in an oven at 150°C for drying for 72 seconds and cured at 230°C for 72 seconds, so that the dipping solution adheres to the surface of the aramid cord, thereby obtaining the dipped polyarylate cord.

[0082] Example 4

[0083] A two-bath dipping system of hydroxylated acrylic dispersion resin-amino resin-latex for surface treatment of polyarylate cord, the production steps of which are as follows:

[0084] (1) Preparation of a one-bath dipping solution: 1.48 parts by weight of sorbitol glycidyl ether was added to 100 parts by weight of deionized water and stirred at room temperature for 5 minutes to obtain a uniform aqueous solution, and then 9.86 parts by weight of caprolactam-blocked 4,4'-diphenylmethane diisocyanate was added and stirred at room temperature for 2 hours to obtain a one-bath dipping solution.

[0085] (2) Preparation of the second-bath dipping solution: 20 parts by weight of a hydroxyl acrylic dispersion resin having a hydroxyl value of 4.2 and 7.5 parts by weight of CYMEL-325 amino resin were added to 100 parts by weight of deionized water, and then 108 parts by weight of butylpyrrolidone latex was added and stirred at room temperature for 2 hours to obtain the second-bath dipping solution.

[0086] (3) Dipping treatment: The polyarylate cord is first dipped in a first-bath dipping solution for dipping, and is dipped at room temperature for 5 seconds; the dipped cord is then placed in an oven at 150°C for drying for 72 seconds and cured at 230°C for 72 seconds, and then the dipped aramid cord is dipped in a second-bath dipping solution for dipping, and is dipped at room temperature for 5 seconds; the dipped cord is then placed in an oven at 150°C for drying for 72 seconds and cured at 230°C for 72 seconds, so that the dipping solution adheres to the surface of the aramid cord, thereby obtaining the dipped polyarylate cord.

[0087] Example 5

[0088] A two-bath dipping system of hydroxylated acrylic dispersion resin-amino resin-latex for surface treatment of polyarylate cord, the production steps of which are as follows:

[0089] (1) Preparation of a one-bath dipping solution: 1.48 parts by weight of sorbitol glycidyl ether was added to 100 parts by weight of deionized water and stirred at room temperature for 5 minutes to obtain a uniform aqueous solution, and then 9.86 parts by weight of caprolactam-blocked 4,4'-diphenylmethane diisocyanate was added and stirred at room temperature for 2 hours to obtain a one-bath dipping solution.

[0090] (2) Preparation of the second-bath dipping solution: 23 parts by weight of a hydroxyl acrylic dispersion resin having a hydroxyl value of 4.2 and 9.5 parts by weight of CYMEL-325 amino resin were added to 100 parts by weight of deionized water, and then 108 parts by weight of butylpyrrolidone latex was added and stirred at room temperature for 2 hours to obtain the second-bath dipping solution.

[0091] (3) Dipping treatment: The polyarylate cord is first dipped in a first-bath dipping solution for dipping, and is dipped at room temperature for 5 seconds; the dipped cord is then placed in an oven at 150°C for drying for 72 seconds and cured at 230°C for 72 seconds, and then the dipped aramid cord is dipped in a second-bath dipping solution for dipping, and is dipped at room temperature for 5 seconds; the dipped cord is then placed in an oven at 150°C for drying for 72 seconds and cured at 230°C for 72 seconds, so that the dipping solution adheres to the surface of the aramid cord, thereby obtaining the dipped polyarylate cord.

[0092] Example 6

[0093] A two-bath dipping system of hydroxylated acrylic dispersion resin-amino resin-latex for surface treatment of polyarylate cord, the production steps of which are as follows:

[0094] (1) Preparation of a one-bath dipping solution: 1.48 parts by weight of sorbitol glycidyl ether was added to 100 parts by weight of deionized water and stirred at room temperature for 5 minutes to obtain a uniform aqueous solution, and then 9.86 parts by weight of caprolactam-blocked 4,4'-diphenylmethane diisocyanate was added and stirred at room temperature for 2 hours to obtain a one-bath dipping solution.

[0095] (2) Preparation of the second-bath dipping solution: 21 parts by weight of a hydroxyl acrylic dispersion resin having a hydroxyl value of 4.2 and 8 parts by weight of CYMEL-325 amino resin are added to 100 parts by weight of deionized water, and then 108 parts by weight of butylpyrrolidone latex is added and stirred at room temperature for 2 hours to obtain the second-bath dipping solution.

[0096] (3) Dipping treatment: The polyarylate cord is first dipped in a first-bath dipping solution for dipping, and is dipped at room temperature for 5 seconds; the dipped cord is then placed in an oven at 150°C for drying for 72 seconds and cured at 230°C for 72 seconds, and then the dipped aramid cord is dipped in a second-bath dipping solution for dipping, and is dipped at room temperature for 5 seconds; the dipped cord is then placed in an oven at 150°C for drying for 72 seconds and cured at 230°C for 72 seconds, so that the dipping solution adheres to the surface of the aramid cord, thereby obtaining the dipped polyarylate cord.

[0097] Example 7

[0098] A two-bath dipping system of hydroxylated acrylic dispersion resin-amino resin-latex for surface treatment of polyarylate cord, the production steps of which are as follows:

[0099] (1) Preparation of a one-bath dipping solution: 1.48 parts by weight of sorbitol glycidyl ether was added to 100 parts by weight of deionized water and stirred at room temperature for 5 minutes to obtain a uniform aqueous solution, and then 9.86 parts by weight of caprolactam-blocked 4,4'-diphenylmethane diisocyanate was added and stirred at room temperature for 2 hours to obtain a one-bath dipping solution.

[0100] (2) Preparation of the second-bath dipping solution: 21.34 parts by weight of a hydroxyl acrylic dispersion resin having a hydroxyl value of 4.2 and 7.6 parts by weight of CYMEL-325 amino resin were added to 100 parts by weight of deionized water, and then 108 parts by weight of butylpyrrolidone latex was added and stirred at room temperature for 2 hours to obtain the second-bath dipping solution.

[0101] (3) Dipping treatment: The polyarylate cord is first dipped in a first-bath dipping solution for dipping, and is dipped at room temperature for 5 seconds; the dipped cord is then placed in an oven at 150°C for drying for 72 seconds and cured at 230°C for 72 seconds, and then the dipped aramid cord is dipped in a second-bath dipping solution for dipping, and is dipped at room temperature for 5 seconds; the dipped cord is then placed in an oven at 150°C for drying for 72 seconds and cured at 230°C for 72 seconds, so that the dipping solution adheres to the surface of the aramid cord, thereby obtaining the dipped polyarylate cord.

[0102] Example 8

[0103] A two-bath dipping system of hydroxylated acrylic dispersion resin-amino resin-latex for surface treatment of polyarylate cord, the production steps of which are as follows:

[0104] (1) Preparation of a one-bath dipping solution: 1.48 parts by weight of sorbitol glycidyl ether was added to 100 parts by weight of deionized water and stirred at room temperature for 5 minutes to obtain a uniform aqueous solution, and then 9.86 parts by weight of caprolactam-blocked 4,4'-diphenylmethane diisocyanate was added and stirred at room temperature for 2 hours to obtain a one-bath dipping solution.

[0105] (2) Preparation of the second-bath dipping solution: 20.08 parts by weight of a hydroxyl acrylic dispersion resin having a hydroxyl value of 4.2 and 8 parts by weight of CYMEL-325 amino resin were added to 100 parts by weight of deionized water, and then 108 parts by weight of butylpyrrolidone latex was added and stirred at room temperature for 2 hours to obtain the second-bath dipping solution.

[0106] (3) Dipping treatment: The polyarylate cord is first dipped in a first-bath dipping solution for dipping, and is dipped at room temperature for 5 seconds; the dipped cord is then placed in an oven at 150°C for drying for 72 seconds and cured at 230°C for 72 seconds, and then the dipped aramid cord is dipped in a second-bath dipping solution for dipping, and is dipped at room temperature for 5 seconds; the dipped cord is then placed in an oven at 150°C for drying for 72 seconds and cured at 230°C for 72 seconds, so that the dipping solution adheres to the surface of the aramid cord, thereby obtaining the dipped polyarylate cord.

[0107] Comparative Example 1

[0108] Comparative Example 1 is a polyarylate cord treated by a conventional RFL dipping system. The polyarylate cord impregnated by the conventional RFL dipping system is used directly without dipping.

[0109] Comparative Example 2

[0110] A two-bath dipping system of hydroxylated acrylic dispersion resin-amino resin-latex for surface treatment of polyarylate cord, the production steps of which are as follows:

[0111] (1) Preparation of a one-bath dipping solution: 1.48 parts by weight of sorbitol glycidyl ether was added to 100 parts by weight of deionized water and stirred at room temperature for 5 minutes to obtain a uniform aqueous solution, and then 9.86 parts by weight of caprolactam-blocked 4,4'-diphenylmethane diisocyanate was added and stirred at room temperature for 2 hours to obtain a one-bath dipping solution.

[0112] (2) Preparation of the second-bath dipping solution: 15.24 parts by weight of a hydroxyl acrylic dispersion resin having a hydroxyl value of 4.2 and 6.36 parts by weight of CYMEL-325 amino resin were added to 100 parts by weight of deionized water, and then 108 parts by weight of butylpyrrolidone latex was added and stirred at room temperature for 2 hours to obtain the second-bath dipping solution.

[0113] (3) Dipping treatment: The polyarylate cord is first dipped in a first-bath dipping solution for dipping, and is dipped at room temperature for 5 seconds; the dipped cord is then placed in an oven at 150°C for drying for 72 seconds and cured at 230°C for 72 seconds, and then the dipped aramid cord is dipped in a second-bath dipping solution for dipping, and is dipped at room temperature for 5 seconds; the dipped cord is then placed in an oven at 150°C for drying for 72 seconds and cured at 230°C for 72 seconds, so that the dipping solution adheres to the surface of the aramid cord, thereby obtaining the dipped polyarylate cord.

[0114] Comparative Example 3

[0115] A two-bath dipping system of hydroxylated acrylic dispersion resin-amino resin-latex for surface treatment of polyarylate cord, the production steps of which are as follows:

[0116] (1) Preparation of a one-bath dipping solution: 1.48 parts by weight of sorbitol glycidyl ether was added to 100 parts by weight of deionized water and stirred at room temperature for 5 minutes to obtain a uniform aqueous solution, and then 9.86 parts by weight of caprolactam-blocked 4,4'-diphenylmethane diisocyanate was added and stirred at room temperature for 2 hours to obtain a one-bath dipping solution.

[0117] (2) Preparation of the second-bath dipping solution: 21.34 parts by weight of a hydroxyl acrylic dispersion resin having a hydroxyl value of 2.0 and 8.89 parts by weight of CYMEL-1141 carboxyl-modified amino resin were added to 100 parts by weight of deionized water, and then 108 parts by weight of butylpyrrolidone latex was added and stirred at room temperature for 2 hours to obtain the second-bath dipping solution.

[0118] (3) Dipping treatment: The polyarylate cord is first dipped in a first-bath dipping solution for dipping, and is dipped at room temperature for 5 seconds; the dipped cord is then placed in an oven at 150°C for drying for 72 seconds and cured at 230°C for 72 seconds, and then the dipped aramid cord is dipped in a second-bath dipping solution for dipping, and is dipped at room temperature for 5 seconds; the dipped cord is then placed in an oven at 150°C for drying for 72 seconds and cured at 230°C for 72 seconds, so that the dipping solution adheres to the surface of the aramid cord, thereby obtaining the dipped polyarylate cord.

[0119] Comparative Example 4

[0120] A two-bath dipping system of hydroxylated acrylic dispersion resin-amino resin-latex for surface treatment of polyarylate cord, the production steps of which are as follows:

[0121] (1) Preparation of a one-bath dipping solution: 1.48 parts by weight of sorbitol glycidyl ether was added to 100 parts by weight of deionized water and stirred at room temperature for 5 minutes to obtain a uniform aqueous solution, and then 9.86 parts by weight of caprolactam-blocked 4,4'-diphenylmethane diisocyanate was added and stirred at room temperature for 2 hours to obtain a one-bath dipping solution.

[0122] (2) Preparation of the second-bath dipping solution: 21.34 parts by weight of a hydroxyl acrylic dispersion resin having a hydroxyl value of 4.2, 8.89 parts by weight of CYMEL-325 amino resin and 2 parts of amine-blocked dodecylbenzene sulfonic acid as an accelerator are added to 100 parts by weight of deionized water, and then 108 parts by weight of butylpyrrolidone latex is added and stirred at room temperature for 2 hours to obtain the second-bath dipping solution.

[0123] (3) Dipping treatment: The polyarylate cord is first dipped in a first-bath dipping solution for dipping, and is dipped at room temperature for 5 seconds; the dipped cord is then placed in an oven at 150°C for drying for 72 seconds and cured at 230°C for 72 seconds, and then the dipped aramid cord is dipped in a second-bath dipping solution for dipping, and is dipped at room temperature for 5 seconds; the dipped cord is then placed in an oven at 150°C for drying for 72 seconds and cured at 230°C for 72 seconds, so that the dipping solution adheres to the surface of the aramid cord, thereby obtaining the dipped polyarylate cord.

[0124] Comparative Example 5

[0125] A two-bath dipping system of hydroxylated acrylic dispersion resin-amino resin-latex for surface treatment of polyarylate cord, the production steps of which are as follows:

[0126] (1) Preparation of a one-bath dipping solution: 1.48 parts by weight of sorbitol glycidyl ether was added to 100 parts by weight of deionized water and stirred at room temperature for 5 minutes to obtain a uniform aqueous solution, and then 9.86 parts by weight of caprolactam-blocked 4,4'-diphenylmethane diisocyanate was added and stirred at room temperature for 2 hours to obtain a one-bath dipping solution.

[0127] (2) Preparation of the second-bath dipping solution: 21.34 parts by weight of a hydroxyl acrylic dispersion resin having a hydroxyl value of 4.2 and 8.89 parts by weight of XT-303 amino resin were added to 100 parts by weight of deionized water, and then 108 parts by weight of butylpyrrolidone latex was added and stirred at room temperature for 2 hours to obtain the second-bath dipping solution.

[0128] (3) Dipping treatment: The polyarylate cord is first dipped in a first-bath dipping solution for dipping, and is dipped at room temperature for 5 seconds; the dipped cord is then placed in an oven at 150°C for drying for 72 seconds and cured at 230°C for 72 seconds, and then the dipped aramid cord is dipped in a second-bath dipping solution for dipping, and is dipped at room temperature for 5 seconds; the dipped cord is then placed in an oven at 150°C for drying for 72 seconds and cured at 230°C for 72 seconds, so that the dipping solution adheres to the surface of the aramid cord, thereby obtaining the dipped polyarylate cord.

[0129] Comparative Example 6

[0130] A two-bath dipping system of hydroxylated acrylic dispersion resin-amino resin-latex for surface treatment of polyarylate cord, the production steps of which are as follows:

[0131] (1) Preparation of a one-bath dipping solution: 1.48 parts by weight of sorbitol glycidyl ether was added to 100 parts by weight of deionized water and stirred at room temperature for 5 minutes to obtain a uniform aqueous solution, and then 9.86 parts by weight of caprolactam-blocked 4,4'-diphenylmethane diisocyanate was added and stirred at room temperature for 2 hours to obtain a one-bath dipping solution.

[0132] (2) Preparation of the second-bath dipping solution: 21.34 parts by weight of aqueous solid hydroxylated acrylic dispersion resin and 8.89 parts by weight of CYMEL-325 amino resin were added to 100 parts by weight of deionized water, and then 108 parts by weight of butylpyrrolidone latex was added and stirred at room temperature for 2 hours to obtain the second-bath dipping solution.

[0133] (3) Dipping treatment: The polyarylate cord is first dipped in a first-bath dipping solution for dipping, and is dipped at room temperature for 5 seconds; the dipped cord is then placed in an oven at 150°C for drying for 72 seconds and cured at 230°C for 72 seconds, and then the dipped aramid cord is dipped in a second-bath dipping solution for dipping, and is dipped at room temperature for 5 seconds; the dipped cord is then placed in an oven at 150°C for drying for 72 seconds and cured at 230°C for 72 seconds, so that the dipping solution adheres to the surface of the aramid cord, thereby obtaining the dipped polyarylate cord.

[0134] Comparative Example 7

[0135] A two-bath dipping system of hydroxylated acrylic dispersion resin-amino resin-latex for surface treatment of polyarylate cord, the production steps of which are as follows:

[0136] (1) Preparation of dipping solution: One-bath dipping solution and two-bath dipping solution were prepared according to the method of Example 7 in CN115748256A.

[0137] (2) Dipping treatment: The polyarylate cord is first dipped in a first-bath dipping solution for dipping, and is dipped at room temperature for 5 seconds; the dipped cord is then placed in an oven at 150°C for drying for 72 seconds and cured at 230°C for 72 seconds, and then the dipped aramid cord is placed in a second-bath dipping solution for dipping, and is dipped at room temperature for 5 seconds; the dipped cord is then placed in an oven at 150°C for drying for 72 seconds and cured at 230°C for 72 seconds, so that the dipping solution adheres to the surface of the aramid cord, thereby obtaining the dipped polyarylate cord.

[0138] The dipped polyarylate cords obtained in Examples 1 to 8 and Comparative Examples 1 to 7 were subjected to extraction test specimen preparation. The specific preparation method is as follows: referring to the standard GB / T36795-2018, the standard rubber is completely coated on the dipped cord to prepare the extraction pattern, and finally it is placed on a flat vulcanizer for vulcanization, the vulcanization temperature is 150°C, the vulcanization pressure is 5MPa, and the vulcanization time is 20min. After the preparation is completed, the surface morphology of the fiber after being pulled out of the rubber is observed by a scanning electron microscope, and the pulled out fiber is cut into small segments and fixed to the sample table with conductive glue.

[0139] Figures 1 to 3 These are electron microscope images of the polyarylate cords of Examples 1 to 3 after treatment. It can be seen that the rubber is evenly attached to the fiber surface. After H extraction, the fiber surface is rough and attached with a large amount of rubber, and the interface damage mode is mainly concentrated in the rubber matrix. Figure 1 and Figure 3 In the figure, after H extraction, the fiber surface is rough and attached with a large amount of rubber. The interface damage is mainly concentrated in the rubber matrix, but there is also some damage between the impregnation layer and the rubber interface. Figure 4 This is an electron microscope picture of the polyarylate cord in Example 1 after treatment. It can be seen that the rubber is evenly attached to the fiber surface. After H extraction, the fiber surface is rough and attached with a large amount of rubber, and the interface damage mode is mainly concentrated in the rubber matrix. Figures 5 to 7 They are electron microscope images of the polyarylate cords of comparative examples 2 to 4 after treatment. It can be seen that the adhesive is evenly attached to the fiber surface. After H extraction, the fiber surface is rough and attached with a large amount of rubber. The interface damage is mainly concentrated in the rubber matrix, but there is also damage between some of the impregnation layers and the rubber interface.

[0140] The adhesive performance test of the dipped polyarylate cords obtained in Examples 1 to 8 and Comparative Examples 1 to 7 was carried out, and the test method referred to the H extraction test method specified in GB / T36795-2018. The results of the adhesive performance test are shown in Table 1:

[0141] Table 1 Adhesive properties of samples obtained from the embodiments of the present invention and comparative examples

[0142]

[0143]

[0144] It can be seen from the data in the above table that after the fiber is dipped in the two-bath dipping system of hydroxy acrylic dispersion resin-amino resin-latex in Examples 1 to 8, its bonding effect is equivalent to that of the RFL system. In addition, the dipping solution of Comparative Example 4 is basically the same as that of Example 2, the only difference being that a commonly used accelerator is added thereto. After dipping in Comparative Example 4 and Example 2 respectively, the bonding effect is equivalent, and the original bonding function is maintained. The dipping solution of Comparative Example 6 is basically the same as that of Example 2, the only difference being that a commonly used solid hydroxy acrylic resin is used. The bonding effect after dipping in Comparative Example 6 is far inferior to that after dipping in Example 2.

[0145] The hydroxy acrylic dispersion resin-amino resin-latex dipping solution of Example 2 was freeze-dried, vulcanized at 150°C, and cured at 230°C. Part of the sample was cut and low-temperature polished, and the PF-QNM test mode was selected to observe and test the sample slices. Finally, the Young's modulus diagram was selected to analyze the phase structure and modulus distribution of the material. The AFM image obtained is as follows: Figure 8 As shown. Figure 8 It can be seen that there are a large number of high modulus island phase structure areas in the sample, which are the reactant resins of hydroxyl acrylic resin-amino resin formed after a large amount of resin is cured. There are also low modulus sea phase latex matrix areas in the sample. The resin and latex together form the sea island structure of the dip layer. A large number of resin structures are distributed in the low modulus latex matrix, which plays the role of connecting fibers and latex and enhancing the strength of the dip layer.

[0146] The stability performance test of the dipping system of Example 2 was carried out. The first bath dipping solution and the second bath dipping solution were placed at room temperature for 24h, 48h, and 72h, respectively. After the time was up, the polyarylate fiber was dipped in the same way as in step (3) of Example 2. After the dipping was completed, a composite material was prepared with rubber and the H extraction force was measured. The method for preparing the composite material with rubber was the same as described above, and the extraction force test method was the same as described above. The results are shown in FIG. Fig. 9 shown. Fig. 9There are four groups, and all four groups use the one-bath dipping solution and the two-bath dipping solution of Example 2 for dipping. It should be noted that the HAAL group uses the one-bath dipping solution and the two-bath dipping solution prepared immediately for dipping, which are actually the dipped polyarylate cords obtained in Example 2, for comparison with the other three groups; the 24h group uses the one-bath dipping solution and the two-bath dipping solution that have been placed at room temperature for 24h for dipping; the 48h group uses the one-bath dipping solution and the two-bath dipping solution that have been placed at room temperature for 48h for dipping; the 72h group uses the one-bath dipping solution and the two-bath dipping solution that have been placed at room temperature for 72h for dipping. Fig. 9 It can be seen that the first-bath dipping solution and the second-bath dipping solution of Example 2 can still maintain the same performance as the initial preparation after being placed at room temperature for three days, indicating that they can be stably stored and used for a long time, which is convenient for industrial production.

Claims

1. A fiber surface treatment dipping system, characterized in that: The dipping system comprises a first-bath dipping solution and a second-bath dipping solution; The one-bath dipping solution is prepared from deionized water, a water-soluble epoxy resin and a blocked isocyanate; based on 100 parts by weight of deionized water, Deionized water 100 parts by weight 1-3 parts by weight of water-soluble epoxy resin Blocked isocyanate 8-10 parts by weight The second bath dipping solution is prepared from deionized water, hydroxyl acrylic acid dispersion resin, amino resin and rubber latex; based on 100 parts by weight of deionized water, Wherein, the amino resin is CYMEL-325 or CYMEL-327.

2. The dipping system according to claim 1, characterized in that: The one-bath dipping solution is calculated based on 100 parts by weight of deionized water. Deionized water 100 parts by weight 1-2 parts by weight of water-soluble epoxy resin Blocked isocyanate 8-9 parts by weight and / or The second bath dipping solution is calculated based on 100 parts by weight of deionized water. 。 3. The dipping system according to claim 1, characterized in that: The weight ratio of the amino resin to the hydroxylated acrylic dispersion resin is 0.36 to 0.42:1; and / or The weight ratio of the rubber latex to the resin is 1:0.65-0.75; the resin is the hydroxylated acrylic dispersion resin and the amino resin; and / or The mass ratio of the first bath dipping solution to the second bath dipping solution is 1:2-2.

5.

4. The dipping system according to claim 1, characterized in that: The solid content of the rubber latex is 20% to 40%; and / or The solid content of the hydroxylated acrylic dispersion resin is 40% to 50%, preferably 41% to 45%.

5. The dipping system according to claim 1, characterized in that: The hydroxyl value of the hydroxylated acrylic dispersion resin is at least one of 2.0 and 4.

2.

6. The dipping system according to claim 1, characterized in that: The water-soluble epoxy resin is at least one of sorbitol glycidyl ether, diphenol propane type epoxy resin, bisphenol A type liquid epoxy resin, trimethylolpropane glycidyl ether, tetraphenol ethane tetraglycidyl ether epoxy resin; and / or The blocked isocyanate is an isocyanate blocked by a blocking agent; the isocyanate is at least one of trimethyl-1,6-hexamethylene diisocyanate, tetramethylene diisocyanate, tetramethyl diisocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, isophorone diisocyanate, and diphenylmethane diisocyanate, and the blocking agent is at least one of caprolactam, butanone oxime, and phenol; and / or The rubber latex is at least one of butyl pyrrolidone latex, styrene butadiene latex, styrene butadiene pyrrolidone latex, chloroprene latex and nitrile butadiene latex.

7. A method for preparing a dipping system as claimed in any one of claims 1 to 6, characterized in that The method comprises: The water-soluble epoxy resin and the blocked isocyanate are added into the deionized water to obtain a first-bath dipping solution; and the hydroxylated acrylic dispersion resin, the amino resin and rubber latex are added into the deionized water to obtain a second-bath dipping solution.

8. A fiber, characterized in that: The fiber is obtained by dipping in the dipping system described in any one of claims 1 to 6.

9. The fiber according to claim 8, characterized in that: The fiber is one of nylon fiber cords, aramid cords, polyarylate fiber cords, or a mixed cord of two or more cords.

10. A method for preparing the fiber according to claim 9, characterized in that The method comprises: the fiber is prepared by the following steps: The cord is placed in a first-bath dipping solution for dipping, drying and curing; and then placed in a second-bath dipping solution for dipping, drying and curing to obtain the cord.

Citation Information

Cited By

  • Water-based polyhydroxy modified amino resin as well as preparation method and application thereof

    CN119859232A

  • Para-aramid fiber impregnation formula, preparation method, impregnation process and application

    CN120231234A