Production line and process for preparing acrylic protective paper based on nanofibers
By adding amphoteric cellulose nanocrystals, polyamide epoxychlorohydrin resin and coniferous wood pulp to the paper production line, combined with electric motor-controlled coating and tensile detection, the problems of reduced tensile strength and high testing cost are solved. , achieving improvement in paper performance and testing efficiency.
Patent Information
- Application Number
- CN202411248727.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
During the existing paper production process, the tensile strength of the paper is reduced after production and needs to be tested with a tensile tester, which increases manual transportation and testing costs.
A production line for acrylic protective paper based on nanofibers was designed. By adding amphoteric cellulose nanocrystals and polyamide epoxychlorohydrin resin to the crusher, the coating liquid was controlled by using an electric motor. Emission, enhance the dry tensile strength and wet tensile strength of the paper, and combine it with the tensile detection mechanism to achieve paper performance testing.
Improves the dry tensile strength, wet tensile strength and tear of paper, simplifies the paper testing process, and reduces manual transportation and testing costs.
Smart Images

Figure CN118910910A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of paper production, and in particular to a production line and a process for preparing acrylic protective paper based on nanofibers. Background Art
[0002] At present, during paper production, the pulp, including imported coniferous wood pulp, needs to be crushed first. In order to enhance the tensile strength of the paper, tensile liquid is added into and outside the paper. However, the tensile strength of the current paper is reduced after production, and the paper needs to be tested separately with the help of a tensile testing machine after production. This process not only increases the labor of manual transportation and operation, but also increases the cost of paper testing. Summary of the invention
[0003] The present invention discloses a production line for preparing acrylic protective paper based on nanofibers and a process thereof. Amphoteric cellulose nanocrystals and polyamide epichlorohydrin resin are respectively added to the inner side of a storage tank, imported coniferous wood pulp is added to the interior of a first storage shell, a rotating shaft and crushing teeth are controlled to rotate, and amphoteric cellulose nanocrystals and polyamide epichlorohydrin resin are sequentially added to the interior of the first storage shell. When the crushing teeth rotate, a paddle shakes the liquid inside the first storage shell to fully mix the coniferous wood pulp, amphoteric cellulose nanocrystals and polyamide epichlorohydrin resin. An electric motor is controlled to drive a baffle to move accurately in the lateral direction. The discharge flow rate of the coating liquid is controlled by adjusting the position of the baffle. The mixed coating liquid moves to the outside of a coating roller, and the paper is coated when the coating roller rotates.
[0004] According to a first aspect of the present disclosure, a production line for preparing acrylic protective paper based on nanofibers and a process thereof are provided, which specifically include: a stable main body, a group of crushers and a group of tension detection mechanisms are installed at the inner side of the stable main body, the tension detection mechanism is composed of a cylinder, a tension detector and a pressing rod, the crusher is composed of a first storage shell, a rotating shaft, crushing teeth and a paddle, a positioning sleeve is respectively provided on both sides of the first storage shell, a group of storage tanks are installed at the position of the positioning sleeve, an electric motor is installed at the bottom position of the first storage shell, a second storage shell and a group of coating rollers are installed at the inner side of the stable main body, the second storage shell is installed at the bottom position of the coating roller, a group of clamping mechanisms are installed at one side of the stable main body, the clamping mechanism is composed of a driver, a first positioning frame, a first rack, a second positioning frame, a second rack and a clamping plate, a water spray shell is installed at the upper position of one side of the stable main body, and a positioning bolt is respectively installed on both sides of the first positioning frame and the second positioning frame.
[0005] Furthermore, four groups of symmetrically distributed sliding grooves are opened on the inner side surface of the stable body. The sliding groove is a T-shaped structure. A sliding block is respectively provided on both sides of the first positioning frame and the second positioning frame, and a sliding block is also provided on one side of the first rack and the second rack. The sliding blocks are respectively installed inside the sliding grooves.
[0006] Furthermore, a first storage shell is installed on the inner side of the stabilizing body, two stabilizing blocks are provided on both sides of the first storage shell, a rotating shaft is installed on the inner side of the first storage shell, the rotating shaft passes through the first storage shell and a pulley is installed on the outer side, the pulley is used to install the transmission belt, and a group of crushing teeth are installed on the outer side of the rotating shaft.
[0007] Furthermore, two positioning rods are installed on the inner side of the first storage shell, a supporting spring and a paddle are installed on the outer side of the positioning rods, and a friction block is provided on one side of the crushing tooth, and the friction block is an arc structure.
[0008] Furthermore, the storage tank includes a floating frame and a position sensor. A stabilizing plate is provided on the inner side of the storage tank. A sliding groove corresponding to the stabilizing plate is opened on one side of the floating frame. The floating frame is installed on the outer side of the stabilizing plate in conjunction with the sliding groove. A stabilizing groove is opened above the floating frame. A position sensor is installed on the inner side of the stabilizing groove. A sliding groove is opened on one side of the storage tank. The sliding groove is a T-shaped structure. A laser emitter is installed on the inner side of the sliding groove.
[0009] Furthermore, a stabilizing bar is provided on each side of the baffle, and two bending plates are provided at the bottom of the first storage shell. The bending plates are of a U-shaped structure. The stabilizing bar passes through the interior of the stabilizing plate. A group of meshing teeth are provided on the inner side of the stabilizing bar. A gear is installed at the outer position of the driving shaft of the electric motor, and the meshing teeth are meshed with the gear. A discharge hole is opened at the bottom of the electric motor.
[0010] Furthermore, the driver is installed on the outer side of the stable main body, a first rack is provided on both sides of the first positioning frame, and a second rack is provided on both sides of the second positioning frame. A gear is installed on the outer side of the driving shaft of the driver, and the gear is respectively engaged with the first rack and the second rack, and a group of clamping plates are respectively installed on the inner sides of the first positioning frame and the second positioning frame.
[0011] Furthermore, a tension detector is installed at the upper position of the push rod of the cylinder, and a pressing rod is installed at the upper position of the tension detector. The first positioning frame and the second positioning frame are respectively composed of two parts. A stabilizing bar is provided on one side of the first positioning frame and the second positioning frame respectively. A sliding hole is opened in the middle position of the stabilizing bar. A positioning bolt passes through the inside of the stabilizing hole. A nut is installed on one side of the positioning bolt, and a support spring is installed on the outer side of the positioning bolt. The outer side of the pressing rod is provided with two groups of symmetrically distributed extrusion bevel blocks.
[0012] Furthermore, a production process for preparing acrylic protective paper based on nanofibers comprises the following steps:
[0013] 1). When coating paper, first add amphoteric cellulose nanocrystals and polyamide epichlorohydrin resin to the inner side of the storage tank, add imported softwood pulp to the inside of the first storage shell, control the rotation of the rotating shaft and the crushing teeth, add amphoteric cellulose nanocrystals and polyamide epichlorohydrin resin to the inside of the first storage shell in sequence, when the crushing teeth rotate, the friction block pushes the paddle to one side, and the paddle can swing back and forth under the push of the supporting spring again, shaking the liquid inside the first storage shell, so that the softwood pulp, amphoteric cellulose nanocrystals and polyamide epichlorohydrin resin are fully mixed, and the electric motor is controlled to drive the baffle to move horizontally and accurately, and the discharge flow of the coating liquid is controlled by adjusting the position of the baffle, and the mixed coating liquid moves to the outside of the coating roller, and the paper is coated when the coating roller rotates;
[0014] 2). Using the advantages of high specific surface area and high aspect ratio of amphoteric cellulose nanocrystals to enhance the retention of polyamide epichlorohydrin resin on the surface of hand sheets, thereby enhancing the dry tensile strength, wet tensile strength and tear strength of the hand sheets and a series of other properties. The fiber morphology of the hand sheets and the retention of polyamide epichlorohydrin resin were observed through a Leica microscope, and then the nanocellulose graft copolymer polyacrylate Pickering emulsion was prepared and coated on the paper;
[0015] 3). When using the protective paper production line to prepare acrylic protective base paper, firstly, pulping is performed. First, a certain amount of pulp board fragments are torn off, placed in a bucket and soaked in water for eight hours or more, and then the pulping operation is performed using a vertical pulping machine. The pulping is performed for about six minutes, and the pulp is placed in a filter screen, squeezed to filter out the water, and then torn into small pieces for subsequent moisture balance and weighing. The small pieces are placed in a sealed bag, marked, and placed in a constant temperature refrigerator. After balancing the moisture for 24 hours, the moisture content of the pulp pieces is measured, and the beating degree is measured. After the moisture content is obtained, the mass of pulp required for making a piece of paper is calculated according to the requirement of the hand sheet of 40g / m2, and then the pulp fragments are weighed;
[0016] 4). Then, the filler is prepared according to the requirements of the dosage of amphoteric nanocellulose and polyamide epichlorohydrin in the experimental design; first, the actual loading amount of amphoteric nanocellulose and polyamide epichlorohydrin with different gradient concentrations is calculated, and then the medicine is weighed, the amphoteric nanocellulose is fully dispersed in the polyamide epichlorohydrin, and then the amphoteric nanocellulose is disintegrated together with the pulp;
[0017] 5). Then proceed with the deflaking operation. Put the weighed pulp fragments into the deflaking bucket, add appropriate amount of water and filler into it, and pay attention to rinse the beaker loaded with filler two or three times, and then proceed with the deflaking. The deflaking takes about six minutes. After the deflaking is completed, use a washing bottle to clean the stirring impeller of the deflaking machine to reduce the error;
[0018] 6). Then, make a sheet. Pour the debonded pulp into a sheet making machine, add an appropriate amount of water and perform bubble homogenization to make the pulp fibers evenly dispersed. Then, perform filtering. After the wet paper sheet is formed on the wire, open the vacuum valve to further filter the water. Then, take the wet paper sheet off the wire for pressing and vacuum drying. Finally, obtain a hand sheet, mark it and place it in a constant temperature and humidity environment for 24 hours for performance testing.
[0019] 7). Then conduct characterization observation, use Leica DVM6 video microscope to observe the hand copy, first make sure there is no sample or debris on the stage, turn on the computer, turn on the equipment, and then open the software; before measuring, to ensure color accuracy, place a piece of white paper for white balance operation, and then select the magnification. After the selection is completed, adjust the focus. You can first focus automatically and then manually to obtain the best picture. Right-click anywhere on the live image and click "Export Image" to save. After using the instrument, close the software, turn off the instrument, turn off the computer, and tidy up the desktop to ensure that the desktop is clean;
[0020] 8). Then, quantitative, dry tensile strength, wet tensile strength, expansion ratio and tearing degree are measured. When measuring dry tensile strength and expansion ratio, first control the first positioning frame and the second positioning frame to press the two ends of the paper, then set the quantitative, and then cut the sample into paper strips with a width of 15 mm and a moderate length, place it on a horizontal computer tensile tester, and measure and record the dry tensile strength performance and expansion ratio. When measuring wet tensile strength, first set the quantitative, and then cut the sample into paper strips with a width of 15 mm and a moderate length, place it on a horizontal computer tensile tester, control the extrusion inclined block to expand the first positioning frame and the second positioning frame outward, at this time, the paper between the first positioning frame and the second positioning frame can be tested for dry tensile strength, use a rubber dropper to drop two drops of water in the middle of the paper strip, and use a filter paper strip to absorb the water after five seconds, and then measure and record the wet tensile strength performance and expansion ratio. When measuring tearing degree, first set the quantitative, and then cut the sample into a size of 63 mm × 50 mm, place it on the tearing degree tester for measurement and recording.
[0021] The present invention provides a production line and process for preparing acrylic protective paper based on nanofibers, which has the following beneficial effects:
[0022] A crusher is set up to beat the imported softwood pulp, and the amphoteric cellulose nanocrystals and polyamide epichlorohydrin resin are fully mixed with the imported softwood pulp inside the crusher. The crusher includes a storage shell, a rotating shaft, crushing teeth, and a paddle. The specific beneficial effects are as follows:
[0023] When the crushing teeth rotate, the friction block pushes the paddle to one side, and the paddle can swing back and forth under the push of the supporting spring again, and the paddle shakes the liquid inside the first storage shell to fully mix the conifer pulp, the amphoteric cellulose nanocrystals and the polyamide epichlorohydrin resin;
[0024] Storage tanks are set up to store amphoteric cellulose nanocrystals and polyamide epichlorohydrin resin respectively. Floating racks, position sensors and laser transmitters are installed at the locations of the storage tanks. The position sensor moves with the height of the liquid level. The position sensor cooperates with the scale to automatically detect the liquid inside the storage tank. When the position sensor moves to the position of the laser transmitter, the position sensor alarms to remind the staff to add liquid to the inside of the storage tank in time.
[0025] An electric motor and a baffle are arranged on the basis of the crusher to achieve the effect of quantitative discharge of the mixed slurry. The control of the electric motor can drive the baffle to move horizontally and accurately.
[0026] A clamping mechanism is provided to achieve the effect of clamping both ends of the paper, a water spray shell is provided to moisten the paper to facilitate the detection of the paper, and a cylinder is provided to stretch the tension detector and the pressing rod downward. At this time, the paper is stretched by force, thereby achieving the effect of convenient testing of the dry tensile strength and wet tensile strength of the paper. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the technical solution of the embodiment of the present invention, the drawings of the embodiment are briefly introduced below.
[0028] The drawings described below are only related to some embodiments of the present invention, but are not intended to limit the present invention.
[0029] In the attached picture:
[0030] Figure 1 The schematic diagram of the axle side structure after the production line of the present application is shown;
[0031] Figure 2 This application shows Figure 1 Axial structural diagram from an upward angle;
[0032] Figure 3 This application shows Figure 1 A schematic diagram of the left-angle structural view;
[0033] Figure 4 A schematic diagram of the partial axial structure of the production line of the present application is shown;
[0034] Figure 5 This application shows Figure 3 A schematic diagram of the axle side structure from a rear perspective;
[0035] Figure 6 Schematic diagram showing the first storage housing, baffle, and second storage housing bottom-up view axis structure of the present application
[0036] Figure 7 This application shows Figure 4 A schematic diagram of the enlarged structure at point A;
[0037] Figure 8 This application shows Figure 4 A schematic diagram of the enlarged structure at B;
[0038] Fig. 9 This application shows Figure 4 A schematic diagram of the enlarged structure at C;
[0039] Fig.10 This application shows Figure 5 Schematic diagram of the enlarged structure at D.
[0040] Reference numerals list
[0041] 1. Stabilize the subject;
[0042] 2. Crusher; 201. First storage shell; 202. Rotating shaft; 203. Crushing teeth; 204. Pick;
[0043] 3. Storage tank; 301. Floating rack; 302. Position sensor;
[0044] 4. Electric motor; 401. Baffle;
[0045] 5. A second storage shell;
[0046] 6. Coating roller;
[0047] 7. Clamping mechanism; 701. Driver; 702. First positioning frame; 703. First rack; 704. Second positioning frame; 705. Second rack; 706. Clamping plate;
[0048] 8. Tension detection mechanism; 801. Cylinder; 802. Tension detector; 803. Pressing rod;
[0049] 9. Water spray housing;
[0050] 10. Positioning bolts. DETAILED DESCRIPTION
[0051] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution of the embodiment of the present invention will be clearly and completely described below in conjunction with the accompanying drawings of the embodiment of the present invention. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0052] Example 1: Please refer to Figures 1 to 10 :
[0053] The present invention proposes a production line and a process for preparing acrylic protective paper based on nanofibers, comprising: a stable main body 1, a group of breaker 2 and a group of tension detection mechanism 8 are installed at the inner side of the stable main body 1, the tension detection mechanism 8 is composed of a cylinder 801, a tension detector 802 and a pressing rod 803, the breaker 2 is composed of a first storage shell 201, a rotating shaft 202, a crushing tooth 203 and a paddle 204, a positioning sleeve is respectively provided on both sides of the first storage shell 201, a group of storage tanks 3 are installed at the position of the positioning sleeve, an electric motor 4 is installed at the bottom position of the first storage shell 201, a second storage shell 5 and a group of coating rollers 6 are installed at the inner side of the stable main body 1, and the second storage shell 5 is installed at the coating roller 6 At the bottom, the second storage shell 5 collects the coating liquid so that the coating roller 6 at the bottom can effectively adhere to the liquid. The upper and lower coating rollers 6 cooperate with each other to achieve the effect of coating the two sides of the paper respectively. A group of clamping mechanisms 7 are installed at one side of the stable main body 1. The clamping mechanism 7 is composed of a driver 701, a first positioning frame 702, a first rack 703, a second positioning frame 704, a second rack 705 and a clamping plate 706. A water spray shell 9 is installed at the upper position on one side of the stable main body 1. After the water spray shell 9 is connected to the water pump, the water spray shell 9 sprays atomized water on the paper to moisten the paper. At this time, the effect of wet tensile strength detection of the paper can be achieved. A positioning bolt 10 is installed on both sides of the first positioning frame 702 and the second positioning frame 704.
[0054] In the embodiments of the present disclosure, reference Figures 1 to 10 As shown, four groups of symmetrically distributed sliding grooves are opened on the inner side of the stable main body 1, and the sliding groove is a T-shaped structure. A sliding block is respectively provided on both sides of the first positioning frame 702 and the second positioning frame 704, and a sliding block is also provided on one side of the first rack 703 and the second rack 705. The sliding blocks are respectively installed inside the sliding grooves, and the sliding grooves realize the circumferential and front-to-back positioning of the sliding positions of the first positioning frame 702 and the second positioning frame 704, and the first positioning frame 702 and the second positioning frame 704 move up and down stably along the sliding grooves.
[0055] In the embodiments of the present disclosure, reference Figures 1 to 10As shown, a first storage shell 201 is installed at the inner side of the stable main body 1, and two stabilizing blocks are arranged on both sides of the first storage shell 201. After the first storage shell 201 is installed, it cooperates with the stabilizing blocks to achieve the effect of stabilizing the installation position. A rotating shaft 202 is installed at the inner side of the first storage shell 201. The rotating shaft 202 passes through the first storage shell 201 and a pulley is installed on the outer side. The pulley is used to install the transmission belt. A group of crushing teeth 203 are installed at the outer side of the rotating shaft 202. When the rotating shaft 202 rotates, the crushing teeth 203 are driven to rotate. The crushing teeth 203 beat and crush the imported coniferous wood pulp, and when the crushing teeth 203 rotate, the coniferous wood pulp, amphoteric cellulose nanocrystals and polyamide epichlorohydrin resin can be mixed.
[0056] In the embodiments of the present disclosure, reference Figures 1 to 10 As shown, two positioning rods are installed on the inner side of the first storage shell 201, and a supporting spring and a paddle 204 are installed on the outer side of the positioning rod. The supporting spring pushes the paddle 204 to reset. A friction block is provided on one side of the crushing tooth 203. The friction block is an arc structure. When the crushing tooth 203 rotates, the friction block pushes the paddle 204 to one side. The paddle 204 can swing back and forth under the further push of the supporting spring. The paddle 204 shakes the liquid inside the first storage shell 201 to fully mix the coniferous wood pulp, amphoteric cellulose nanocrystals and polyamide epichlorohydrin resin.
[0057] In the embodiments of the present disclosure, reference Figures 1 to 10 As shown, the storage tank 3 includes a floating frame 301 and a position sensor 302. A stabilizing plate is provided at the inner side of the storage tank 3. A sliding groove corresponding to the stabilizing plate is provided on one side of the floating frame 301. The floating frame 301 is installed at the outer side of the stabilizing plate in cooperation with the sliding groove. The stabilizing plate realizes the effect of lateral and circumferential positioning of the sliding position of the floating frame 301, so that the floating frame 301 can move up and down stably. After liquid or emulsion is added to the interior of the storage tank 3, the floating frame 301 will move with the height of the liquid level. A stabilizing groove is provided at the upper position of the floating frame 301. The inner position of the stabilizing groove A position sensor 302 is installed, and the stabilizing groove ensures that the installation position of the position sensor 302 is stable. When the floating frame 301 floats up and down, it will drive the position sensor 302 to move synchronously. The position sensor 302 can automatically detect the liquid inside the storage tank 3 with the scale. A sliding groove is opened on one side of the storage tank 3. The sliding groove is a T-shaped structure. A laser emitter is installed on the inner side of the sliding groove. When the position sensor 302 moves to the position of the laser emitter, the position sensor 302 alarms to remind the staff to add liquid to the inside of the storage tank 3 in time.
[0058] In the embodiments of the present disclosure, reference Figures 1 to 10As shown, a stabilizing bar is provided on each side of the baffle 401, and two bending plates are provided at the bottom of the first storage shell 201. The bending plates are of a U-shaped structure. The stabilizing bar passes through the inside of the stabilizing plate. At this time, the bending plate realizes the up and down and circumferential positioning effect of the baffle 401. The baffle 401 can move stably laterally at the bottom of the first storage shell 201. A group of meshing teeth is provided on the inner side of the stabilizing bar, and a gear is installed at the outer position of the driving shaft of the electric motor 4. The meshing teeth and the gear are meshed, and the electric motor 4 is controlled to drive the baffle 401 to move laterally accurately. A discharge hole is opened at the bottom of the electric motor 4, and the baffle 401 blocks the position of the discharge hole. The discharge flow rate of the coating liquid is controlled by adjusting the position of the baffle 401.
[0059] In the embodiments of the present disclosure, reference Figures 1 to 10 As shown, the driver 701 is installed at the outer position of the stable main body 1, a first rack 703 is provided on both sides of the first positioning frame 702, and a second rack 705 is provided on both sides of the second positioning frame 704. A gear is installed on the outer side of the driving shaft of the driver 701, and the gears are respectively engaged with the first rack 703 and the second rack 705. A group of clamping plates 706 are respectively installed at the inner positions of the first positioning frame 702 and the second positioning frame 704. The driver 701 drives the gear to rotate. When the gear rotates, the first positioning frame 702 and the second positioning frame 704 are controlled to move in opposite directions, so that the first positioning frame 702 and the second positioning frame 704 cooperate with the clamping plate 706 to clamp the two ends of the paper, which is convenient for paper detection.
[0060] In the embodiments of the present disclosure, reference Figures 1 to 10 As shown, a tension detector 802 is installed at the upper position of the push rod of the cylinder 801, and a pressing rod 803 is installed at the upper position of the tension detector 802. The cylinder 801 is controlled to stretch the tension detector 802 and the pressing rod 803 downward. The first positioning frame 702 and the second positioning frame 704 are respectively composed of two parts. A stabilizing bar is provided on one side of the first positioning frame 702 and the second positioning frame 704. A sliding hole is opened in the middle of the stabilizing bar. The positioning bolt 10 passes through the inside of the stabilizing hole. With the cooperation of the sliding groove, the first positioning frame 702 and the first positioning frame 704 are secured. The second positioning frame 704 is effectively expanded outward, a nut is installed on one side of the positioning bolt 10, and a support spring is installed on the outside of the positioning bolt 10. The support spring can effectively support the two parts of the first positioning frame 702 and the second positioning frame 704 inward respectively. The outer side surface of the pressing rod 803 is provided with two groups of symmetrically distributed extrusion bevel blocks. After the pressing rod 803 moves downward, the extrusion bevel blocks can expand the first positioning frame 702 and the second positioning frame 704 outward. At this time, the paper between the first positioning frame 702 and the second positioning frame 704 can be tested for dry tensile strength.
[0061] Embodiment 2, based on embodiment 1, refers to Figures 1 to 10 As shown, it is necessary to install a solenoid valve at the bottom of the storage tank 3, and the quantitative discharge of the amphoteric cellulose nanocrystals and the polyamide epichlorohydrin resin can be achieved by manipulating the solenoid valve.
[0062] The working principle of this embodiment:
[0063] During installation, first install a set of crushers 2 and a set of tension detection mechanisms 8 on the inner side of the stable main body 1, then install a set of storage tanks 3 at the position of the positioning sleeve, and after the storage tanks 3 are installed, complete the installation of the floating frame 301 and the position sensor 302 at the same time, install an electric motor 4 at the bottom of the first storage shell 201, install a second storage shell 5 and a set of coating rollers 6 on the inner side of the stable main body 1, and install the second storage shell 5 at the bottom of the coating roller 6, install the driver 701, the first positioning frame 702, the first rack 703, the second positioning frame 704, the second rack 705 and the clamping plate 706 on one side of the stable main body 1, install a water spray shell 9 on the upper side of one side of the stable main body 1, and install the positioning bolts 10 on both sides of the first positioning frame 702 and the second positioning frame 704 respectively;
[0064] When coating the paper, firstly add the amphoteric cellulose nanocrystals and the polyamide epichlorohydrin resin to the inner side of the storage tank 3 respectively, add the imported softwood pulp to the inside of the first storage shell 201, control the rotation of the rotating shaft 202 and the crushing teeth 203, add the amphoteric cellulose nanocrystals and the polyamide epichlorohydrin resin to the inside of the first storage shell 201 in sequence, when the crushing teeth 203 rotate, the friction block pushes the paddle 204 to one side, and the paddle 204 can swing back and forth under the push of the supporting spring again, and the paddle 204 shakes the liquid inside the first storage shell 201 to fully mix the softwood pulp, the amphoteric cellulose nanocrystals and the polyamide epichlorohydrin resin, control the electric motor 4 to drive the baffle 401 to move accurately in the lateral direction, and control the discharge flow of the coating liquid by adjusting the position of the baffle 401, and the mixed coating liquid moves to the outside of the coating roller 6, and the paper is coated when the coating roller 6 rotates;
[0065] The advantages of high specific surface area and high aspect ratio of amphoteric cellulose nanocrystals are used to enhance the retention of polyamide epichlorohydrin resin on the surface of hand sheets, thereby enhancing a series of properties of the hand sheets such as dry tensile strength, wet tensile strength and tear resistance. The fiber morphology of the hand sheets and the retention of polyamide epichlorohydrin resin are observed through a Leica microscope, and then a nanocellulose graft copolymer polyacrylate Pickering emulsion is prepared and coated on paper.
[0066] When using the protective paper production line to prepare acrylic protective base paper, firstly, pulping is performed. First, a certain amount of pulp board fragments are torn off, placed in a bucket and soaked in water for eight hours or more, and then the pulping operation is performed using a vertical pulping machine. The pulping is performed for about six minutes, and the pulp is placed in a filter screen, squeezed to filter out the water, and then torn into small pieces for subsequent moisture balance and weighing. The small pieces are placed in a sealed bag, marked, and placed in a constant temperature refrigerator. After balancing the moisture for 24 hours, the moisture content of the pulp fragments is measured, and the beating degree is measured. After the moisture content is obtained, the mass of pulp required for making a piece of paper is calculated according to the requirement of the hand-made sheet of 40g / m2, and then the pulp fragments are weighed;
[0067] Then, the filler is prepared according to the requirements of the dosage of amphoteric nanocellulose and polyamide epichlorohydrin in the experimental design. First, the actual amount of amphoteric nanocellulose and polyamide epichlorohydrin with different gradient concentrations is calculated, and then the drugs are weighed, the amphoteric nanocellulose is fully dispersed in the polyamide epichlorohydrin, and then the amphoteric nanocellulose is decomposed together with the pulp;
[0068] Then proceed with the deflagration operation. Put the weighed pulp fragments into the deflagration bucket, add appropriate amount of water and filler into it, pay attention to rinse the beaker loaded with filler two or three times, and then proceed with the deflagration. The deflagration takes about six minutes. After the deflagration is completed, use a washing bottle to clean the stirring impeller of the deflagration machine to reduce the error.
[0069] Then, the paper sheet is made. The debonded pulp is poured into the paper sheet making machine. After adding an appropriate amount of water, the bubble homogenization operation is performed to make the pulp fibers evenly dispersed. Then, the filtering operation is performed. After the wet paper sheet is formed on the wire, the vacuum valve is opened to further filter the water. Then, the wet paper sheet is taken out from the wire for pressing and vacuum drying. Finally, the hand sheet is obtained, marked and placed in a constant temperature and humidity environment for 24 hours for performance testing.
[0070] Then, characterization observation was carried out. The hand-copied film was observed using a Leica DVM6 video microscope. First, make sure that there is no sample or debris on the stage, then turn on the computer, turn on the equipment, and then open the software. Before measurement, to ensure color accuracy, place a piece of white paper for white balance operation, and then select the magnification. After the selection is completed, adjust the focus. You can first focus automatically and then manually to obtain the best picture. Right-click anywhere on the live image and click "Export Image" to save. After using the instrument, close the software, turn off the instrument, turn off the computer, and tidy up the desktop to ensure that the desktop is clean;
[0071] Then, the quantitative, dry tensile strength, wet tensile strength, expansion ratio, and tearing degree are measured. When measuring the dry tensile strength and expansion ratio, the first positioning frame 702 and the second positioning frame 704 are first controlled to press the two ends of the paper tightly, and then the quantitative is set, and then the sample is cut into paper strips with a width of 15 mm and a moderate length, and placed on a horizontal computer tensile tester to measure and record the dry tensile strength performance and expansion ratio. When measuring the wet tensile strength, the quantitative is set first, and then the sample is cut into paper strips with a width of 15 mm and a moderate length, and placed on a horizontal computer tensile tester. On the computer tensile tester, controlling the extrusion bevel can expand the first positioning frame 702 and the second positioning frame 704 outward. At this time, the paper between the first positioning frame 702 and the second positioning frame 704 can be tested for dry tensile strength. Use a rubber-tipped dropper to drop two drops of water in the middle of the paper strip. After five seconds, use a filter paper strip to absorb the water, and then measure and record the wet tensile strength performance and expansion rate. When measuring the tear strength, first set the quantity, and then cut the sample into a size of 63mm×50mm, put it on the tear strength tester for measurement and recording.
[0072] In this article, there are a few points to note:
[0073] 1. The drawings of the embodiments of the present disclosure only involve structures related to the embodiments of the present disclosure, and other structures may refer to general designs.
[0074] 2. In the absence of conflict, the embodiments of the present disclosure and the features therein may be combined with each other to obtain new embodiments.
[0075] The above are only specific embodiments of the present disclosure, but the protection scope of the present disclosure is not limited thereto. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed in the present disclosure, which should be included in the protection scope of the present disclosure. Therefore, the protection scope of the present disclosure should be based on the protection scope of the claims.
Claims
1. A production line for preparing acrylic protective paper based on nanofibers, include: A stable main body (1), a crusher (2) and a tension detection mechanism (8), wherein a group of crushers (2) and a group of tension detection mechanisms (8) are installed at the inner side of the stable main body (1), characterized in that the tension detection mechanism (8) is composed of a cylinder (801), a tension detector (802) and a pressing rod (803), the crusher (2) is composed of a first storage shell (201), a rotating shaft (202), crushing teeth (203) and a paddle (204), a positioning sleeve is respectively provided on both sides of the first storage shell (201), a group of storage tanks (3) are installed at the position of the positioning sleeve, and an electric motor is installed at the bottom of the first storage shell (201) (4), a second storage shell (5) and a group of coating rollers (6) are installed on the inner side of the stable main body (1), the second storage shell (5) is installed at the bottom of the coating roller (6), a group of clamping mechanisms (7) are installed on one side of the stable main body (1), the clamping mechanism (7) is composed of a driver (701), a first positioning frame (702), a first rack (703), a second positioning frame (704), a second rack (705) and a clamping plate (706), a water spray shell (9) is installed on the upper side of one side of the stable main body (1), and a positioning bolt (10) is installed on both sides of the first positioning frame (702) and the second positioning frame (704).
2. According to claim 1, a production line for preparing acrylic protective paper based on nanofibers, It is characterized in that Four groups of symmetrically distributed sliding grooves are provided on the inner side surface of the stable body (1), a sliding block is provided on both sides of the first positioning frame (702) and the second positioning frame (704), and a sliding block is also provided on one side of the first rack (703) and the second rack (705), and the sliding blocks are respectively installed inside the sliding grooves.
3. The production line for preparing acrylic protective paper based on nanofibers according to claim 1, It is characterized in that A first storage shell (201) is installed on the inner side of the stabilizing body (1), two stabilizing blocks are provided on both sides of the first storage shell (201), a rotating shaft (202) is installed on the inner side of the first storage shell (201), the rotating shaft (202) passes through the first storage shell (201) and a pulley is installed on the outer side, the pulley is used to install a transmission belt, and a group of crushing teeth (203) are installed on the outer side of the rotating shaft (202).
4. The production line for preparing acrylic protective paper based on nanofibers according to claim 1, It is characterized in that Two positioning rods are installed on the inner side of the first storage shell (201), and a supporting spring and a paddle (204) are installed on the outer side of the positioning rod. A friction block is provided on one side of the crushing tooth (203), and the friction block is an arc structure.
5. The production line for preparing acrylic protective paper based on nanofibers according to claim 1, It is characterized in that The storage tank (3) comprises a floating frame (301) and a position sensor (302), a stabilizing plate is provided on the inner side of the storage tank (3), a sliding groove corresponding to the stabilizing plate is provided on one side of the floating frame (301), the floating frame (301) is installed on the outer side of the stabilizing plate in cooperation with the sliding groove, a stabilizing groove is provided on the upper side of the floating frame (301), a position sensor (302) is installed on the inner side of the stabilizing groove, a sliding groove is provided on one side of the storage tank (3), the sliding groove is a T-shaped structure, and a laser transmitter is installed on the inner side of the sliding groove.
6. The production line for preparing acrylic protective paper based on nanofibers according to claim 1, It is characterized in that A stabilizing bar is provided on each side of the baffle (401), and two bent plates are provided at the bottom of the first storage shell (201). The bent plates are of a U-shaped structure. The stabilizing bar passes through the inside of the stabilizing plate, and a group of meshing teeth are provided on the inner side of the stabilizing bar. A gear is installed at the outer position of the driving shaft of the electric motor (4), and the meshing teeth are meshed with the gear. A discharge hole is opened at the bottom of the electric motor (4).
7. The production line for preparing acrylic protective paper based on nanofibers according to claim 1, It is characterized in that The driver (701) is installed at the outer side of the stable main body (1), and a first rack (703) is provided on both sides of the first positioning frame (702), and a second rack (705) is provided on both sides of the second positioning frame (704). A gear is installed on the outer side of the driving shaft of the driver (701), and the gear is meshed with the first rack (703) and the second rack (705) respectively. A group of clamping plates (706) are installed on the inner sides of the first positioning frame (702) and the second positioning frame (704).
8. The production line for preparing acrylic protective paper based on nanofibers according to claim 1, It is characterized in that A tension detector (802) is installed at the upper position of the push rod of the cylinder (801), and a pressing rod (803) is installed at the upper position of the tension detector (802). The first positioning frame (702) and the second positioning frame (704) are respectively composed of two parts. A stabilizing bar is provided on one side of the first positioning frame (702) and the second positioning frame (704), and a sliding hole is opened in the middle position of the stabilizing bar. A positioning bolt (10) passes through the inside of the stabilizing hole. A nut is installed on one side of the positioning bolt (10), and a supporting spring is installed on the outer side of the positioning bolt (10). The outer side of the pressing rod (803) is provided with two groups of symmetrically distributed extrusion inclined blocks.
9. A process for preparing acrylic protective paper based on nanofibers according to any one of claims 1 to 8, It is characterized in that The following steps are involved: 1) When coating paper, firstly, add amphoteric cellulose nanocrystals and polyamide epichlorohydrin resin to the inner side of the storage tank (3), add imported softwood pulp to the inside of the first storage shell (201), control the rotation of the rotating shaft (202) and the crushing teeth (203), add amphoteric cellulose nanocrystals and polyamide epichlorohydrin resin to the inside of the first storage shell (201) in sequence, and when the crushing teeth (203) rotate, the friction block pushes the paddle (204) to one side, and the paddle (204) ) can swing back and forth again under the push of the supporting spring, the paddle (204) shakes the liquid inside the first storage shell (201), so that the softwood pulp, the amphoteric cellulose nanocrystals and the polyamide epichlorohydrin resin are fully mixed, and the electric motor (4) is controlled to drive the baffle (401) to move accurately in the lateral direction, and the discharge flow of the coating liquid is controlled by adjusting the position of the baffle (401), and the mixed coating liquid moves to the outside of the coating roller (6), and the coating roller (6) is coated on the paper when it rotates; 2). Using the advantages of high specific surface area and high aspect ratio of amphoteric cellulose nanocrystals to enhance the retention of polyamide epichlorohydrin resin on the surface of hand sheets, thereby enhancing the dry tensile strength, wet tensile strength and tear strength of the hand sheets and a series of other properties. The fiber morphology of the hand sheets and the retention of polyamide epichlorohydrin resin were observed through a Leica microscope, and then the nanocellulose graft copolymer polyacrylate Pickering emulsion was prepared and coated on the paper; 3). When using the protective paper production line to prepare acrylic protective base paper, firstly, pulping is performed. First, a certain amount of pulp board fragments are torn off, placed in a bucket and soaked in water for eight hours or more, and then the pulping operation is performed using a vertical pulping machine. The pulping is performed for about six minutes, and the pulp is placed in a filter screen, squeezed to filter out the water, and then torn into small pieces for subsequent moisture balance and weighing. The small pieces are placed in a sealed bag, marked, and placed in a constant temperature refrigerator. After balancing the moisture for 24 hours, the moisture content of the pulp pieces is measured, and the beating degree is measured. After the moisture content is obtained, the mass of pulp required for making a piece of paper is calculated according to the requirement of the hand sheet of 40g / m2, and then the pulp fragments are weighed; 4). Then, the filler is prepared according to the requirements of the dosage of amphoteric nanocellulose and polyamide epichlorohydrin in the experimental design; first, the actual loading amount of amphoteric nanocellulose and polyamide epichlorohydrin with different gradient concentrations is calculated, and then the medicine is weighed, the amphoteric nanocellulose is fully dispersed in the polyamide epichlorohydrin, and then the amphoteric nanocellulose is disintegrated together with the pulp; 5). Then proceed with the deflaking operation. Put the weighed pulp fragments into the deflaking bucket, add appropriate amount of water and filler into it, and pay attention to rinse the beaker loaded with filler two or three times, and then proceed with the deflaking. The deflaking takes about six minutes. After the deflaking is completed, use a washing bottle to clean the stirring impeller of the deflaking machine to reduce the error; 6). Then, make a sheet. Pour the debonded pulp into a sheet making machine, add an appropriate amount of water and perform bubble homogenization to make the pulp fibers evenly dispersed. Then, perform filtering. After the wet paper sheet is formed on the wire, open the vacuum valve to further filter the water. Then, take the wet paper sheet off the wire for pressing and vacuum drying. Finally, obtain a hand sheet, mark it and place it in a constant temperature and humidity environment for 24 hours for performance testing. 7). Then conduct characterization observation, use Leica DVM6 video microscope to observe the hand copy, first make sure there is no sample or debris on the stage, turn on the computer, turn on the equipment, and then open the software; before measuring, to ensure color accuracy, place a piece of white paper for white balance operation, and then select the magnification. After the selection is completed, adjust the focus. You can first focus automatically and then manually to obtain the best picture. Right-click anywhere on the live image and click "Export Image" to save. After using the instrument, close the software, turn off the instrument, turn off the computer, and tidy up the desktop to ensure that the desktop is clean; 8). Then, quantitative, dry tensile strength, wet tensile strength, expansion ratio, and tearing strength are measured. When measuring dry tensile strength and expansion ratio, the first positioning frame (702) and the second positioning frame (704) are first controlled to press the two ends of the paper tightly, and then the quantitative is set, and then the sample is cut into paper strips with a width of 15 mm and a moderate length, and placed on a horizontal computer tensile tester to measure and record the dry tensile strength performance and expansion ratio. When measuring wet tensile strength, the quantitative is set first, and then the sample is cut into paper strips with a width of 15 mm and a moderate length, and placed on a horizontal computer tensile tester. On the brain tensile tester, controlling the squeezing inclined block can expand the first positioning frame (702) and the second positioning frame (704) outward. At this time, the paper between the first positioning frame (702) and the second positioning frame (704) can be tested for dry tensile strength. Two drops of water are dripped in the middle of the paper strip using a rubber-tipped dropper. After five seconds, the water is absorbed using a filter paper strip, and the wet tensile strength performance and the expansion ratio are measured and recorded. When measuring the tear strength, the quantity is set first, and then the sample is cut into a size of 63mm×50mm and placed on the tear strength tester for measurement and recording.