Preparation method of aerogel type papermaking additive based on composite fiber material

Through the aerogel-type papermaking additive of composite fiber materials, the preparation of composite aerogels and porous carbon nanosheets through co-precipitation and hydrothermal methods, the problem of low bonding rate of existing additives is solved and the paper is significantly improved The tensile and ring compressive strength meets the high-strength needs of special industries.

CN118910922AActive Publication Date: 2024-11-08SUZHOU SIWECO ENVIRONMENTAL SOLUTIONS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411186361.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-08
Estimated Expiration
2044-08-28

AI Technical Summary

Technical Problem

The existing papermaking additives have problems such as low bonding rate and limited chemical bond formation conditions in improving paper strength, which cannot meet the high requirements for paper strength in special industries.

Method used

The aerogel-type papermaking additive preparation method based on composite fiber material is adopted. The composite type is prepared by co-precipitation and hydrothermal method by combining aspartic acid and copper. Aerogel and combined with porous carbon nanosheets and carbon fibers, a porous structure is formed by ultrasonic and mechanical stirring, which enhances the bonding strength between the fibers.

Benefits of technology

Aerogel-type composite fiber material with high friction resistance and stable mesh structure has been formed, which significantly improves the tensile strength and ring pressure strength of the paper and meets the high-strength needs of special industries.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of papermaking processing, in particular to a preparation method of an aerogel type papermaking additive based on a composite fiber material, which comprises the following steps: S1, diluting an additive intermediate with water, adjusting the pH value to 9.0-9.5, stirring and mixing for 12-18 minutes, and controlling the temperature at 32-36 DEG C to obtain an additive intermediate solution; s2, glyoxal is added into the auxiliary intermediate solution under stirring to adjust the pH value to 9.0-9.3, reaction is stopped until the material viscosity reaches 20-50 cps and the pH value is adjusted to 2.5-4.0, after the reaction is finished, an aerogel type composite fiber material is added, full stirring and dispersing are conducted, and the papermaking auxiliary is obtained. The papermaking additive prepared by the invention is introduced into a papermaking process, so that the tensile strength and ring crush compression resistance of paper can be effectively improved, and the paper has excellent strength and toughness and can better meet the requirements of special industries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of papermaking processing, and in particular to a method for preparing an aerogel-type papermaking auxiliary agent based on composite fiber materials. Background Art

[0002] The dry strength of paper is one of the structural characteristics of paper. The dry strength of paper is mainly obtained with the formation of the fiber network and the bonding between fibers after drying. In fact, the strength of paper mainly depends on the strength of a single fiber and the degree of bonding between fibers, the number, the distribution of fiber bonding, etc. The strength of the fiber network can be improved by mechanical beating and refining, because after increasing the beating degree, the number of fine fibers increases, thereby increasing the formation of bonds between fibers. In the binding force between fibers, although there are covalent bonds, ionic bonds and van der Waals forces, the key role is played by hydrogen bonds. Unlike other bonds, hydrogen bonds can only be formed within a very short distance and must interact when the molecules are in close contact.

[0003] For example, Chinese patent CN103866629A discloses a papermaking processing aid and a preparation method thereof, which is composed of the following components in weight ratio: 13-15 parts of toluene diisocyanate, 2-4 parts of C9 petroleum resin, 9-12 parts of potassium octadecylbenzene sulfonate, 1-2 parts of potassium oxalate, 4-5 parts of propylene glycol, 4-6 parts of ethyl acetate, and 120-124 parts of deionized water; the papermaking aid improves the strength of paper by increasing the bonding between paper fibers, but the formation of bonds between paper fibers is affected by various factors such as reaction dimension and pH, and not only has a low bonding rate, but the formed chemical bonds must interact only when the molecules are in close contact, so the improvement of paper strength is poor, so that the paper strength can only meet daily use, and cannot meet the needs of some special industries with high paper strength requirements. Summary of the invention

[0004] In view of the problems existing in the prior art, the object of the present invention is to provide a method for preparing an aerogel-type papermaking auxiliary agent based on composite fiber materials.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A method for preparing an aerogel-type papermaking auxiliary agent based on a composite fiber material, the preparation method comprising the following steps:

[0007] S1. Dilute the auxiliary agent intermediate with water, adjust the pH value to 9.0-9.5, stir and mix for 12-18 minutes, and control the temperature at 32-36° C. to obtain an auxiliary agent intermediate solution;

[0008] S2, adding glyoxal to the auxiliary agent intermediate solution with the aid of a circulation pump under stirring, controlling the absolute dry mass ratio of the auxiliary agent intermediate to glyoxal to be (3.2-7.6):1, adjusting the pH value to 9.0-9.3, reacting until the viscosity of the material reaches 20-50cps, and stopping the reaction when the pH value is adjusted to 2.5-4.0. After the reaction is completed, adding an aerogel-type composite fiber material, fully stirring and dispersing, and obtaining a papermaking auxiliary agent;

[0009] The preparation method of the aerogel type composite fiber material comprises the following steps:

[0010] 1) A mixture of sodium alginate / carrageenan / chitosan was used as a precursor, and the precursor was prepared by wet spinning technology. A composite aerogel was prepared by co-precipitation using aspartic acid as an organic ligand and copper as a metal center.

[0011] 2) synthesizing porous nanosheets by a hydrothermal method, and using the porous nanosheets as a substrate, depositing nanowires on the surface of the substrate to obtain nanomaterials, and combining the nanomaterials with carbon fibers by physical bonding to obtain composite fiber materials;

[0012] 3) After the composite fiber material and the composite aerogel are fully mixed by vacuum treatment under ultrasonic and mechanical stirring, the composite fiber material and the composite aerogel are placed in a reaction solution composed of a sulfur source and an antimony source for hydrothermal reaction to obtain an aerogel-type composite fiber material.

[0013] As a further preferred embodiment of the present invention, the preparation method of the auxiliary agent intermediate comprises the following steps:

[0014] According to weight parts, 30-42 parts of acrylamide monomer, 4-7 parts of anionic monomer, 28-42 parts of cationic monomer, 1-3 parts of chain transfer agent and 0.02-0.05 parts of complexing agent are added into a reaction kettle, soft water is added to prepare an aqueous solution with a mass percentage concentration of 20-28%, nitrogen is introduced for 25-50 minutes, 2-6 parts of pH value regulator are added to adjust the pH value to 4.0-5.5, 3-5 parts of catalyst and 1-3 parts of initiator are uniformly added dropwise at 68-72° C., stirring for reaction for 120-170 minutes, keeping warm for 50-100 minutes, stopping the reaction, cooling to room temperature, adding 0.1-0.5 parts of antibacterial agent, and obtaining an auxiliary agent intermediate.

[0015] As a further preferred embodiment of the present invention, the cationic monomer is composed of dimethyldiallylammonium chloride monomer and acryloyloxyethyltrimethylammonium chloride monomer in equal weight;

[0016] The anionic monomer is selected from one or more of itaconic acid, 2-acrylamido-2-methylpropanesulfonic acid and their salts;

[0017] The initiator is selected from one or more of ammonium persulfate, sodium persulfate, potassium persulfate, azobisisobutylamidine hydrochloride, and azobisisopropylimidazoline hydrochloride;

[0018] The pH value regulator includes alkali and acid, wherein the alkali is selected from one or more of sodium hydroxide and ammonia water; the acid is selected from one or more of hydrochloric acid, phosphoric acid, formic acid and citric acid;

[0019] The chain transfer agent is sodium formate, the catalyst is phosphoric acid, the complexing agent is disodium ethylenediaminetetraacetate, and the antibacterial agent is isothiazolinone.

[0020] As a further preferred embodiment of the present invention, the composite aerogel is specifically prepared by the following method:

[0021] Sodium alginate, kappa carrageenan and chitosan in a mass ratio of (3-4):1:(2-3) are mixed to obtain a precursor, and then an aqueous solution of the precursor is prepared, and then ethanol is used as a coagulation bath, and the precipitated gel is solidified in a copper nitrate solution with a mass fraction of 5-8%, and then placed in a muffle furnace after drying, and carbonized at 800-830°C for 2-3h, and the obtained product is soaked in acetic acid, then repeatedly washed with deionized water and dried to obtain a carbon aerogel;

[0022] 2) L-aspartic acid is dissolved in a sodium hydroxide solution with a concentration of 6.0-6.8 mol / L, and then the carbon aerogel is added, and ultrasonic treatment is performed for 30-50 min. After uniform dispersion, a copper nitrate solution with a concentration of 0.5-0.8 mol / L is added, and the reaction is stirred for 3-5 h. After the obtained product is centrifuged, it is repeatedly washed with deionized water, acetic acid solution and ethanol solution in turn, and then dried to obtain a composite aerogel.

[0023] Furthermore, the precursor aqueous solution has a mass fraction of 3-5%;

[0024] The ratio of the L-aspartic acid, sodium hydroxide solution, carbon aerogel and copper nitrate solution is (0.04-0.07) mol: (10-20) mL: (0.3-0.5) g: (100-130) mL.

[0025] As a further preferred embodiment of the present invention, the composite fiber material is specifically prepared by the following method:

[0026] 1) 0.2-0.5 g of nano magnesium oxide is placed in 100-160 mL of methanol solution, ultrasonically dispersed for 30-50 min, then 1.2-1.8 g of zinc nitrate is added, stirred for 1-2 h, to obtain solution A, 1.4-2.0 g of 2-methylimidazole is uniformly dispersed in 300-500 mL of methanol solution, to obtain solution B, solution A and solution B are mixed, stirred and reacted at room temperature for 24-30 h, the obtained product is centrifuged, repeatedly washed with methanol, and dried to obtain a skeleton template material;

[0027] 2) The pre-crushed asphalt, potassium bicarbonate and skeleton template material are placed in a mortar and mixed evenly, then placed in a tube furnace, heated to 300-320°C, and kept at this temperature for 30-50 minutes, then heated to 900-950°C at the same rate, kept at this temperature for 1-2 hours, and then naturally cooled to room temperature, and the obtained product is stirred and soaked in a hydrochloric acid solution for 24-30 hours, and filtered, washed, dried and ground to obtain a porous carbon nanosheet;

[0028] 3) Add copper nitrate, potassium permanganate and manganese sulfate into deionized water, stir magnetically for 30-50 min to form a uniform solution, then add porous carbon nanosheets, disperse evenly and seal in a reactor, react at 160-165° C. for 12-15 h under the action of ultrasound, cool naturally to room temperature after the reaction is completed, wash the product obtained after centrifugation repeatedly with water and ethanol, and dry to obtain a composite nanomaterial;

[0029] 4) Add the carbon fiber and the composite nanomaterial into a container, add deionized water, first mechanically stir for 1-2 hours, then ultrasonically treat for 1-2 hours, and after the treatment is completed, filter the product and dry it to obtain the composite fiber material.

[0030] Furthermore, the stirring reaction has a rotation speed of 500-600 r / min;

[0031] The mass ratio of the asphalt, potassium bicarbonate and skeleton template material is (1.0-1.8): (3.0-5.4): (1.0-1.8);

[0032] The heating rate is 5-8°C / min;

[0033] The hydrochloric acid solution has a concentration of 0.1-0.3 mol / L.

[0034] Furthermore, the ratio of the copper nitrate, potassium permanganate, manganese sulfate, deionized water, and porous carbon nanosheets is (0.025-0.030) mol: (0.14-0.18) mol: (0.045-0.052) mol: (70-100) mL: (5-8) g;

[0035] The ultrasonic effect has a power of 100-150W;

[0036] The ratio of the carbon fiber, the composite nanomaterial, and the deionized water is (10-20) g: (3-7) g: (200-300) mL;

[0037] The mechanical stirring speed is 800-1200r / min;

[0038] The ultrasonic treatment has a power of 500-600W.

[0039] As a further preferred embodiment of the present invention, the specific preparation method of the aerogel-type composite fiber material is as follows:

[0040] 1) dispersing the composite fiber material in deionized water to obtain a dispersion, then adding the composite aerogel to the dispersion, evacuating to 50-100 Pa, and maintaining at 200-300 r / min and 200-300 W ultrasonic action for 30-50 min. After the treatment is completed, centrifuging the product to obtain a pretreated composite fiber material;

[0041] 2) dissolving potassium antimony tartrate in deionized water, stirring magnetically for 15-30 minutes, adding polyvinyl pyrrolidone, continuing to stir for 15-30 minutes, and then adding thioacetamide to the resulting mixed solution, stirring thoroughly to obtain a reaction solution;

[0042] 3) The pretreated composite fiber material is ultrasonically cleaned with acetone, distilled water and ethanol for 10-20 minutes respectively, and then added to the reaction solution after drying. After ultrasonic treatment for 10-20 minutes, it is transferred to a reactor, sealed and placed in an oven, and heated at a constant temperature of 180-186°C for 24-26 hours. After the reaction is completed, it is cooled to room temperature, the product is centrifuged, repeatedly washed with deionized water, and dried.

[0043] Furthermore, the dispersion has a solid content of 5-8 wt %;

[0044] The solid-liquid ratio of the composite aerogel and the dispersion is 1: (150-260) g / mL;

[0045] The ratio of potassium antimony tartrate, deionized water, polyvinyl pyrrolidone and thioacetamide is (0.6-1.4) mol: (60-130) mL: (0.3-0.6) g: (1.3-2.1) mol;

[0046] The ratio of the pretreated composite fiber material to the reaction solution is (5-12) g: (160-280) mL.

[0047] Compared with the prior art, the present invention has the following beneficial effects:

[0048] In the present invention, a sodium alginate / carrageenan / chitosan mixture is used as a precursor, and a precursor is prepared by wet spinning technology. Then, in the precursor, aspartic acid is used as an organic ligand and copper is used as a metal center, and a composite aerogel is prepared by coprecipitation. The introduced metal copper is deposited on the pore wall of the porous structure of the aerogel to form nano copper particles, thereby increasing the roughness of the pore wall, which is beneficial to increase the friction resistance between the pore wall and the nanowire.

[0049] Then, using asphalt as a carbon source, a skeleton template material synthesized from magnesium oxide, zinc nitrate, and 2-methylimidazole as raw materials as a dual template and auxiliary carbon source, and potassium bicarbonate as an activator, a porous carbon nanosheet was prepared by a template-induced coupling chemical method. The porous carbon nanosheet has a large number of holes on its surface, which is conducive to the embedding of nanowires into the holes after deposition, thereby enhancing the bonding strength between the two.

[0050] Then, a hydrothermal method is used to take a porous carbon nanosheet as a substrate, and nanowires are deposited on the surface of the substrate to obtain a nanomaterial; during the carbonization process of carbon fiber, a large amount of non-carbon elements escape in the form of gas, thereby forming defects such as holes and protrusions on the surface of the carbon fiber; mechanical stirring and ultrasonic dispersion are used to embed the nanomaterial into the surface defects of the carbon fiber through the nanosheet through physical bonding, thereby realizing the physical structure of the nanomaterial and the carbon fiber; and because the nanosheet has a porous structure, it is easy to adapt to the protrusion defects on the surface of the carbon fiber, thereby making the bonding strength between the two good, and the structure of the formed composite fiber material is stable;

[0051] Finally, the composite fiber material and the composite aerogel are fully mixed by vacuum treatment under ultrasound and mechanical stirring to obtain a pretreated composite fiber material. The nanowires in the composite fiber material are embedded in the pores of the composite aerogel under the capillary action of the porous structure of the composite aerogel. The vacuum treatment helps to increase the depth of the nanowires embedded in the pores, so that the nanowires embedded in the pores are more likely to contact each other. In addition, under ultrasound and mechanical stirring, the nanowires embedded in the pores will be entangled and connected together, so that the composite fiber material is combined together through the entanglement between the nanowires, thereby forming independent network structures. Moreover, since the connection nodes between the composite fiber materials are in the composite aerogel, the porous skeleton structure of the composite aerogel can effectively disperse and transfer stress and has good external force resistance. Therefore, it can play a good protective role on the connection nodes, avoiding the connection nodes from being disconnected by the force, thereby improving the stability of the network structure.

[0052] At the same time, potassium antimony tartrate and thioacetamide are used as antimony source and sulfur source to form a reaction solution, the pretreated composite fiber material is washed and added to the reaction solution, and after a hydrothermal reaction, the generated antimony sulfide nanoparticles are deposited and attached to the surface of the pretreated composite fiber material, and as the hydrothermal reaction proceeds, the antimony sulfide nanoparticles agglomerate, and a network structure grows from the surface, thereby embedding the surface of the pretreated composite fiber material. On the one hand, after the composite aerogel is embedded, the nanowires can be further prevented from detaching from the pores of the composite aerogel, which helps to improve the stability of the connection nodes, so that the network structure constructed between the composite fiber materials is not easy to collapse; at the same time, the formed network structure increases the surface roughness of the aerogel-type composite fiber material, so that the friction resistance between the aerogel-type composite fiber materials is large, and it is difficult to separate after contacting each other.

[0053] By adding synthetic aerogel-type composite fiber materials to the papermaking process, independent small-scale mesh structures can be formed in the paper. The small-scale mesh structures are randomly dispersed in the paper, which can continuously change the stress transmission path, thereby increasing the resistance of the paper. At the same time, the contact area between the small-scale mesh structures is large. During the tearing process of the paper, the friction resistance between them is large and it is not easy to separate, so the paper is not easy to break.

[0054] The papermaking auxiliary prepared in the present invention is introduced into the papermaking process to effectively improve the tensile strength and ring crush strength of paper, so that the paper has excellent strength and toughness, and can better meet the needs of special industries. DETAILED DESCRIPTION

[0055] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0056] In the embodiments of the present invention, chitosan, with a deacetylation degree greater than 80%, was purchased from Sinopharm Chemical Reagent Co., Ltd.; κ-type carrageenan and sodium alginate, food grade, were purchased from Qingdao Bairen Biotechnology Co., Ltd.;

[0057] The cationic monomer is composed of equal masses of dimethyldiallylammonium chloride monomer and acryloyloxyethyltrimethylammonium chloride monomer;

[0058] The anionic monomer is selected from itaconic acid; the initiator is selected from ammonium persulfate; the pH value regulator includes a base and an acid, the base is selected from sodium hydroxide, and the acid is selected from hydrochloric acid; the chain transfer agent is sodium formate; the catalyst is phosphoric acid; the complexing agent is disodium ethylenediaminetetraacetate; and the antibacterial agent is isothiazolinone.

[0059] Example 1

[0060] A method for preparing an aerogel-type papermaking additive based on a composite fiber material, specifically comprising the following steps:

[0061] S1. Dilute the auxiliary agent intermediate with water, adjust the pH value to 9.0, stir and mix for 12 minutes, and control the temperature at 32° C. to obtain an auxiliary agent intermediate solution;

[0062] S2. Add glyoxal to the auxiliary agent intermediate solution with the aid of a circulation pump under stirring, control the absolute dry mass ratio of the auxiliary agent intermediate to glyoxal to be 3.2:1, adjust the pH value to 9.0, react until the material viscosity reaches 20 cps, and stop the reaction when the pH value is adjusted to 2.5. After the reaction is completed, add the aerogel composite fiber material, fully stir and disperse, and obtain a papermaking auxiliary agent;

[0063] The preparation method of the aerogel type composite fiber material comprises the following steps:

[0064] 1) Sodium alginate, kappa carrageenan and chitosan in a mass ratio of 3:1:2 are mixed to obtain a precursor, and then a 3% precursor aqueous solution is prepared, and then ethanol is used as a coagulation bath, and wet spinning is performed to precipitate the precipitated gel, and the precipitated gel is solidified in a 5% copper nitrate solution by mass, and after drying, it is placed in a muffle furnace and carbonized at 800°C for 2h, and the obtained product is soaked in acetic acid, and then repeatedly washed with deionized water and dried to obtain a carbon aerogel;

[0065] 2) 0.04 mol L-aspartic acid was dissolved in 10 mL of 6.0 mol / L sodium hydroxide solution, and then 0.3 g of carbon aerogel was added, and ultrasonic treatment was performed at 300 W for 30 min. After uniform dispersion, 100 mL of 0.5 mol / L copper nitrate solution was added, and the mixture was stirred at 200 r / min for 3 h. The obtained product was centrifuged, and then repeatedly washed with deionized water, acetic acid solution and ethanol solution, and dried to obtain a composite aerogel;

[0066] 3) 0.2 g of nano-magnesium oxide was placed in 100 mL of methanol solution, and ultrasonically dispersed at 200 W for 30 min, and then 1.2 g of zinc nitrate was added, and stirred at 150 r / min for 1 h to obtain solution A, and 1.4 g of 2-methylimidazole was evenly dispersed in 300 mL of methanol solution to obtain solution B, and solution A and solution B were mixed, and stirred at 500 r / min at room temperature for 24 h. The obtained product was centrifuged and repeatedly washed with methanol, and dried to obtain a skeleton template material;

[0067] 4) 1.0 g of pre-crushed asphalt, 3.0 g of potassium bicarbonate and 1.0 g of skeleton template material were placed in a mortar and mixed evenly, then placed in a tube furnace, heated to 300°C at 5°C / min, and kept at this temperature for 30 min, then heated to 900°C at the same rate, kept at this temperature for 1 h, and then naturally cooled to room temperature. The obtained product was stirred and soaked in a 0.1 mol / L hydrochloric acid solution for 24 h, filtered, washed, dried and ground to obtain a porous carbon nanosheet;

[0068] 5) 0.025 mol of copper nitrate, 0.14 mol of potassium permanganate and 0.045 mol of manganese sulfate were added to 70 mL of deionized water, and magnetic stirring was performed for 30 min to form a uniform solution. Then 5 g of porous carbon nanosheets were added, and the mixture was evenly dispersed and sealed in a reactor. Under the action of 100 W ultrasound, the mixture was kept at a constant temperature of 160 ° C for 12 h. After the reaction was completed, the mixture was naturally cooled to room temperature. The product obtained after centrifugation was repeatedly washed with water and ethanol, and dried to obtain a composite nanomaterial;

[0069] 6) 10 g of carbon fiber and 3 g of composite nanomaterial were added to a container, and 200 mL of deionized water was added. The mixture was first mechanically stirred at 800 r / min for 1 h, and then subjected to 500 W ultrasonic treatment for 1 h. After the treatment was completed, the product was filtered and dried to obtain a composite fiber material;

[0070] 7) dispersing the composite fiber material in deionized water to obtain a dispersion with a solid content of 5 wt%, then adding the composite aerogel to the dispersion at a solid-liquid ratio of 1:150 g / mL, evacuating to 50 Pa, and maintaining at 200 r / min and 200 W ultrasonic action for 30 minutes. After the treatment is completed, the product is centrifuged to obtain a pretreated composite fiber material;

[0071] 8) 0.6 mol of potassium antimony tartrate was dissolved in 60 mL of deionized water, and after magnetic stirring for 15 min, 0.3 g of polyvinyl pyrrolidone was added, and stirring was continued for 15 min. Then, 1.3 mol of thioacetamide was added to the resulting mixed solution, and the mixture was stirred thoroughly to obtain a reaction solution;

[0072] 9) 5 g of the pretreated composite fiber material was ultrasonically cleaned with acetone, distilled water and ethanol for 10 min respectively, dried and added to 160 mL of the reaction solution, ultrasonically treated at 200 W for 10 min, transferred to a reactor, sealed and placed in an oven, heated at 180 ° C for 24 h, cooled to room temperature after the reaction was completed, the product was centrifuged, repeatedly washed with deionized water, and dried.

[0073] Example 2

[0074] A method for preparing an aerogel-type papermaking additive based on a composite fiber material, specifically comprising the following steps:

[0075] S1. Dilute the auxiliary agent intermediate with water, adjust the pH value to 9.5, stir and mix for 15 minutes, and control the temperature at 35° C. to obtain an auxiliary agent intermediate solution;

[0076] S2. Add glyoxal to the auxiliary agent intermediate solution with the aid of a circulation pump under stirring, control the absolute dry mass ratio of the auxiliary agent intermediate to glyoxal to be 5.3:1, adjust the pH value to 9.3, react until the viscosity of the material reaches 35 cps, and stop the reaction when the pH value is adjusted to 3.5. After the reaction is completed, add the aerogel type composite fiber material, fully stir and disperse, and obtain a papermaking auxiliary agent;

[0077] The preparation method of the aerogel type composite fiber material comprises the following steps:

[0078] 1) Sodium alginate, kappa carrageenan and chitosan in a mass ratio of 3.5:1:2.5 are mixed to obtain a precursor, and then a 4% precursor aqueous solution is prepared, and then ethanol is used as a coagulation bath, and wet spinning is performed to precipitate the precipitated gel, and the precipitated gel is solidified in a 7% copper nitrate solution, and then placed in a muffle furnace after drying, and carbonized at 820°C for 2.5h, and the obtained product is soaked in acetic acid, and then repeatedly washed with deionized water and dried to obtain a carbon aerogel;

[0079] 2) 0.05 mol L-aspartic acid was dissolved in 15 mL of 6.5 mol / L sodium hydroxide solution, and then 0.4 g of carbon aerogel was added, and ultrasonic treatment was performed at 400 W for 40 min. After uniform dispersion, 120 mL of 0.7 mol / L copper nitrate solution was added, and the mixture was stirred at 260 r / min for 4 h. The obtained product was centrifuged, and then repeatedly washed with deionized water, acetic acid solution and ethanol solution, and dried to obtain a composite aerogel;

[0080] 3) 0.3 g of nano-magnesium oxide was placed in 130 mL of methanol solution, and ultrasonically dispersed at 260 W for 40 min, and then 1.6 g of zinc nitrate was added, and stirred at 200 r / min for 1.5 h to obtain solution A, and 1.8 g of 2-methylimidazole was evenly dispersed in 400 mL of methanol solution to obtain solution B. After solution A and solution B were mixed, they were stirred at 550 r / min at room temperature for 27 h, and the obtained product was centrifuged and repeatedly washed with methanol, and dried to obtain a skeleton template material;

[0081] 4) 1.5 g of pre-crushed asphalt, 4.5 g of potassium bicarbonate and 1.5 g of skeleton template material were mixed in a mortar, then placed in a tube furnace, heated to 310°C at 6°C / min, and kept at this temperature for 40 min, then heated to 920°C at the same rate, kept at this temperature for 1.5 h, and then naturally cooled to room temperature. The obtained product was stirred and soaked in a 0.2 mol / L hydrochloric acid solution for 27 h, filtered, washed, dried and ground to obtain a porous carbon nanosheet;

[0082] 5) 0.028 mol of copper nitrate, 0.16 mol of potassium permanganate and 0.050 mol of manganese sulfate were added to 85 mL of deionized water, and magnetically stirred for 40 min to form a uniform solution. Then 7 g of porous carbon nanosheets were added, and the mixture was evenly dispersed and sealed in a reactor. Under the action of 130 W ultrasound, the mixture was kept at a constant temperature of 162 ° C for 13 h. After the reaction was completed, the mixture was naturally cooled to room temperature. The product obtained after centrifugation was repeatedly washed with water and ethanol, and dried to obtain a composite nanomaterial;

[0083] 6) 15 g of carbon fiber and 5 g of composite nanomaterial were added to a container, and 260 mL of deionized water was added. The mixture was first mechanically stirred at 1000 r / min for 1.5 h, and then subjected to 550 W ultrasonic treatment for 1.5 h. After the treatment was completed, the product was filtered and dried to obtain a composite fiber material;

[0084] 7) dispersing the composite fiber material in deionized water to obtain a dispersion with a solid content of 7 wt%, then adding the composite aerogel to the dispersion at a solid-liquid ratio of 1:210 g / mL, evacuating to 80 Pa, and maintaining at 250 r / min and 250 W ultrasonic action for 40 min. After the treatment is completed, the product is centrifuged to obtain a pretreated composite fiber material;

[0085] 8) 1.2 mol of potassium antimony tartrate was dissolved in 100 mL of deionized water, and after magnetic stirring for 25 min, 0.5 g of polyvinyl pyrrolidone was added, and stirring was continued for 25 min. Then, 1.8 mol of thioacetamide was added to the resulting mixed solution, and the mixture was stirred thoroughly to obtain a reaction solution;

[0086] 9) 8 g of the pretreated composite fiber material was ultrasonically cleaned with acetone, distilled water and ethanol for 15 min respectively, dried and added to 220 mL of the reaction solution, ultrasonically treated at 250 W for 15 min, transferred to a reactor, sealed and placed in an oven, heated at 182 ° C for 25 h, cooled to room temperature after the reaction was completed, the product was centrifuged, repeatedly washed with deionized water, and dried.

[0087] Example 3

[0088] A method for preparing an aerogel-type papermaking additive based on a composite fiber material, specifically comprising the following steps:

[0089] S1. Dilute the auxiliary agent intermediate with water, adjust the pH value to 9.5, stir and mix for 18 minutes, and control the temperature at 36° C. to obtain an auxiliary agent intermediate solution;

[0090] S2. Add glyoxal to the auxiliary agent intermediate solution with the aid of a circulation pump under stirring, control the absolute dry mass ratio of the auxiliary agent intermediate to glyoxal to be 7.6:1, adjust the pH value to 9.3, react until the material viscosity reaches 50 cps, and stop the reaction when the pH value is adjusted to 4.0. After the reaction is completed, add the aerogel type composite fiber material, fully stir and disperse, and obtain a papermaking auxiliary agent;

[0091] The preparation method of the aerogel type composite fiber material comprises the following steps:

[0092] 1) Sodium alginate, kappa carrageenan and chitosan in a mass ratio of 4:1:3 are mixed to obtain a precursor, and then a 5% by mass aqueous solution of the precursor is prepared, and then ethanol is used as a coagulation bath, and wet spinning is performed to precipitate the precipitated gel, and the precipitated gel is solidified in a copper nitrate solution with a mass fraction of 8%, and after drying, it is placed in a muffle furnace and carbonized at 830°C for 3h, and the obtained product is soaked in acetic acid, and then repeatedly washed with deionized water and dried to obtain a carbon aerogel;

[0093] 2) 0.07 mol L-aspartic acid was dissolved in 20 mL of 6.8 mol / L sodium hydroxide solution, and then 0.5 g of carbon aerogel was added, and ultrasonic treatment was performed at 500 W for 50 min. After uniform dispersion, 130 mL of 0.8 mol / L copper nitrate solution was added, and the mixture was stirred at 300 r / min for 5 h. The obtained product was centrifuged, and then repeatedly washed with deionized water, acetic acid solution and ethanol solution, and dried to obtain a composite aerogel;

[0094] 3) 0.5 g of nano-magnesium oxide was placed in 160 mL of methanol solution, and ultrasonically dispersed at 300 W for 50 min, and then 1.8 g of zinc nitrate was added, and stirred at 260 r / min for 2 h to obtain solution A, 2.0 g of 2-methylimidazole was evenly dispersed in 500 mL of methanol solution to obtain solution B, and solution A and solution B were mixed, and stirred at 600 r / min at room temperature for 30 h. The obtained product was centrifuged and repeatedly washed with methanol, and dried to obtain a skeleton template material;

[0095] 4) 1.8 g of pre-crushed asphalt, 5.4 g of potassium bicarbonate and 1.8 g of skeleton template material were mixed in a mortar, then placed in a tube furnace, heated to 320°C at 8°C / min, and kept at this temperature for 50 min, then heated to 950°C at the same rate, kept at this temperature for 2 h, and then naturally cooled to room temperature. The obtained product was stirred and soaked in a 0.3 mol / L hydrochloric acid solution for 30 h, filtered, washed, dried and ground to obtain a porous carbon nanosheet;

[0096] 5) 0.030 mol of copper nitrate, 0.18 mol of potassium permanganate and 0.052 mol of manganese sulfate were added to 100 mL of deionized water, and magnetic stirring was performed for 50 min to form a uniform solution. Then 8 g of porous carbon nanosheets were added, and the mixture was evenly dispersed and sealed in a reactor. Under the action of 150 W ultrasound, the mixture was kept at a constant temperature of 165 ° C for 15 h. After the reaction was completed, the mixture was naturally cooled to room temperature. The product obtained after centrifugation was repeatedly washed with water and ethanol, and dried to obtain a composite nanomaterial;

[0097] 6) 20 g of carbon fiber and 7 g of composite nanomaterial were added to a container, 300 mL of deionized water was added, mechanical stirring was performed at 1200 r / min for 2 h, and then ultrasonic treatment was performed at 600 W for 2 h. After the treatment was completed, the product was filtered and dried to obtain a composite fiber material;

[0098] 7) dispersing the composite fiber material in deionized water to obtain a dispersion with a solid content of 8 wt%, then adding the composite aerogel to the dispersion at a solid-liquid ratio of 1:260 g / mL, evacuating to 100 Pa, and maintaining at 300 r / min and 300 W ultrasonic action for 50 min. After the treatment is completed, the product is centrifuged to obtain a pretreated composite fiber material;

[0099] 8) 1.4 mol of potassium antimony tartrate was dissolved in 130 mL of deionized water, and after magnetic stirring for 30 min, 0.6 g of polyvinyl pyrrolidone was added, and stirring was continued for 30 min. Then, 2.1 mol of thioacetamide was added to the resulting mixed solution, and the mixture was stirred thoroughly to obtain a reaction solution;

[0100] 9) 12 g of the pretreated composite fiber material was ultrasonically cleaned with acetone, distilled water and ethanol for 20 min respectively, dried and added to 280 mL of the reaction solution, ultrasonically treated at 300 W for 20 min, transferred to a reactor, sealed and placed in an oven, heated at 186 ° C for 26 h, cooled to room temperature after the reaction was completed, the product was centrifuged, repeatedly washed with deionized water, and dried.

[0101] Comparative Example 1: This comparative example is basically the same as Example 1, except that in the preparation of the aerogel-type composite fiber material, steps 1)-2) are omitted.

[0102] Comparative Example 2: This comparative example is basically the same as Example 1, except that in the preparation of the aerogel-type composite fiber material, steps 3) to 5) are omitted.

[0103] Comparative Example 3: This comparative example is basically the same as Example 1, except that in the preparation of the aerogel-type composite fiber material, steps 6)-7) are omitted.

[0104] Comparative Example 4: This comparative example is basically the same as Example 1, except that in the preparation of the aerogel type composite fiber material, steps 8)-9) are omitted.

[0105] Comparative Example 5: This comparative example is basically the same as Example 1, except that it does not contain aerogel-type composite fiber material.

[0106] Test experiment:

[0107] The papermaking aids prepared in Examples 1-3 and Comparative Examples 1-5 were applied to papermaking, ensuring that other conditions in the papermaking process were the same. After papermaking was completed, the tensile strength and ring crush strength of the paper prepared using the papermaking aids prepared in Examples 1-3 and Comparative Examples 1-5 were tested.

[0108] The paper obtained by papermaking in Examples 1-3 and Comparative Examples 1-5 was cut into 10 cm × 10 cm pieces, and the two sides of the pieces were pulled until the pieces broke. The tensile strength value was obtained by dividing the tensile force when the pieces broke by the area of ​​the pieces.

[0109] The paper obtained by papermaking in Examples 1-3 and Comparative Examples 1-5 was cut into paper pieces with a diameter of 10 cm, and the paper pieces were inserted into the sample holder to form a ring shape. Pressure was applied between the upper and lower pressing plates. The maximum force that the paper piece could withstand before being crushed was the ring compression strength.

[0110] After the test data were summarized and counted, the test data of Comparative Example 5 was used as the control group, and the test data of Examples 1-3 and Comparative Examples 1-4 were used as the experimental group. The experimental group data were compared with the control group, and the changes in the experimental group data were recorded. The results are shown in Table 1.

[0111] Table 1

[0112] Example 1 Example 2 Example 3 Comparative Example 1 Tensile strength improvement rate % 38.6 39.3 39.0 32.9 Ring compression strength improvement rate % 35.1 36.2 35.7 30.3 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Tensile strength improvement rate % 30.7 28.4 34.5 - Ring compression strength improvement rate % 28.6 25.3 31.7 -

[0113] It can be seen from Table 1 that the papermaking additive in the present invention, when introduced into the papermaking process, can effectively improve the tensile strength and ring crush strength of paper, so that the paper has excellent strength and toughness, and can better meet the needs of special industries.

[0114] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for preparing an aerogel-type papermaking additive based on composite fiber materials, characterized in that: The preparation method comprises the following steps: S1. Dilute the auxiliary agent intermediate with water, adjust the pH value to 9.0-9.5, stir and mix for 12-18 minutes, and control the temperature at 32-36° C. to obtain an auxiliary agent intermediate solution; S2. Add glyoxal to the auxiliary agent intermediate solution with the help of a circulation pump under stirring, control the absolute dry mass ratio of the auxiliary agent intermediate to glyoxal to be (3.2-7.6):1, adjust the pH value to 9.0-9.3, react until the viscosity of the material reaches 20-50cps, and stop the reaction when the pH value is adjusted to 2.5-4.

0. After the reaction is completed, add the aerogel type composite fiber material, fully stir and disperse, and obtain a papermaking auxiliary agent; The preparation method of the aerogel type composite fiber material comprises the following steps: 1) A mixture of sodium alginate / carrageenan / chitosan was used as a precursor, and the precursor was prepared by wet spinning technology. A composite aerogel was prepared by co-precipitation using aspartic acid as an organic ligand and copper as a metal center. 2) synthesizing porous nanosheets by a hydrothermal method, and using the porous nanosheets as a substrate, depositing nanowires on the surface of the substrate to obtain nanomaterials, and combining the nanomaterials with carbon fibers by physical bonding to obtain composite fiber materials; 3) After the composite fiber material and the composite aerogel are fully mixed by vacuum treatment under ultrasonic and mechanical stirring, the composite fiber material and the composite aerogel are placed in a reaction solution composed of a sulfur source and an antimony source for hydrothermal reaction to obtain an aerogel-type composite fiber material.

2. The method for preparing an aerogel-type papermaking additive based on composite fiber materials according to claim 1, characterized in that: The preparation method of the auxiliary agent intermediate comprises the following steps: According to weight parts, 30-42 parts of acrylamide monomer, 4-7 parts of anionic monomer, 28-42 parts of cationic monomer, 1-3 parts of chain transfer agent and 0.02-0.05 parts of complexing agent are added into a reaction kettle, soft water is added to prepare an aqueous solution with a mass percentage concentration of 20-28%, nitrogen is introduced for 25-50 minutes, 2-6 parts of pH value regulator are added to adjust the pH value to 4.0-5.5, 3-5 parts of catalyst and 1-3 parts of initiator are uniformly added dropwise at 68-72° C., stirring for reaction for 120-170 minutes, keeping warm for 50-100 minutes, stopping the reaction, cooling to room temperature, adding 0.1-0.5 parts of antibacterial agent, and obtaining an auxiliary agent intermediate.

3. The method for preparing an aerogel-type papermaking additive based on composite fiber materials according to claim 1, characterized in that: The cationic monomer is composed of dimethyldiallylammonium chloride monomer and acryloyloxyethyltrimethylammonium chloride monomer in equal amounts; The anionic monomer is selected from one or more of itaconic acid, 2-acrylamido-2-methylpropanesulfonic acid and their salts; The initiator is selected from one or more of ammonium persulfate, sodium persulfate, potassium persulfate, azobisisobutylamidine hydrochloride, and azobisisopropylimidazoline hydrochloride; The pH value regulator includes alkali and acid, wherein the alkali is selected from one or more of sodium hydroxide and ammonia water; the acid is selected from one or more of hydrochloric acid, phosphoric acid, formic acid and citric acid; The chain transfer agent is sodium formate, the catalyst is phosphoric acid, the complexing agent is disodium ethylenediaminetetraacetate, and the antibacterial agent is isothiazolinone.

4. The method for preparing an aerogel-type papermaking additive based on composite fiber materials according to claim 1, characterized in that: The specific preparation method of the composite aerogel is as follows: Sodium alginate, kappa carrageenan and chitosan in a mass ratio of (3-4):1:(2-3) are mixed to obtain a precursor, and then an aqueous solution of the precursor is prepared, and then ethanol is used as a coagulation bath, and the precipitated gel is solidified in a copper nitrate solution with a mass fraction of 5-8%, and then placed in a muffle furnace after drying, and carbonized at 800-830°C for 2-3h, and the obtained product is soaked in acetic acid, then repeatedly washed with deionized water and dried to obtain a carbon aerogel; 2) L-aspartic acid is dissolved in a sodium hydroxide solution with a concentration of 6.0-6.8 mol / L, and then the carbon aerogel is added, and ultrasonic treatment is performed for 30-50 min. After uniform dispersion, a copper nitrate solution with a concentration of 0.5-0.8 mol / L is added, and the reaction is stirred for 3-5 h. After the obtained product is centrifuged, it is repeatedly washed with deionized water, acetic acid solution and ethanol solution in turn, and then dried to obtain a composite aerogel.

5. The method for preparing an aerogel-type papermaking additive based on composite fiber materials according to claim 4, characterized in that: The precursor aqueous solution has a mass fraction of 3-5%; The ratio of the L-aspartic acid, sodium hydroxide solution, carbon aerogel and copper nitrate solution is (0.04-0.07) mol: (10-20) mL: (0.3-0.5) g: (100-130) mL.

6. The method for preparing an aerogel-type papermaking auxiliary agent based on composite fiber materials according to claim 1, characterized in that: The composite fiber material, its specific preparation method is as follows: 1) 0.2-0.5 g of nano magnesium oxide is placed in 100-160 mL of methanol solution, ultrasonically dispersed for 30-50 min, then 1.2-1.8 g of zinc nitrate is added, stirred for 1-2 h, to obtain solution A, 1.4-2.0 g of 2-methylimidazole is uniformly dispersed in 300-500 mL of methanol solution, to obtain solution B, solution A and solution B are mixed, stirred and reacted at room temperature for 24-30 h, the obtained product is centrifuged, repeatedly washed with methanol, and dried to obtain a skeleton template material; 2) The pre-crushed asphalt, potassium bicarbonate and skeleton template material are placed in a mortar and mixed evenly, then placed in a tube furnace, heated to 300-320°C, and kept at this temperature for 30-50 minutes, then heated to 900-950°C at the same rate, kept at this temperature for 1-2 hours, and then naturally cooled to room temperature, and the obtained product is stirred and soaked in a hydrochloric acid solution for 24-30 hours, and filtered, washed, dried and ground to obtain a porous carbon nanosheet; 3) Add copper nitrate, potassium permanganate and manganese sulfate into deionized water, stir magnetically for 30-50 min to form a uniform solution, then add porous carbon nanosheets, disperse evenly and seal in a reactor, react at 160-165° C. for 12-15 h under the action of ultrasound, cool naturally to room temperature after the reaction is completed, wash the product obtained after centrifugation repeatedly with water and ethanol, and dry to obtain a composite nanomaterial; 4) Add the carbon fiber and the composite nanomaterial into a container, add deionized water, first mechanically stir for 1-2 hours, then ultrasonically treat for 1-2 hours, and after the treatment is completed, filter the product and dry it to obtain the composite fiber material.

7. The method for preparing an aerogel-type papermaking auxiliary agent based on composite fiber materials according to claim 6, characterized in that: The stirring reaction has a rotation speed of 500-600 r / min; The mass ratio of the asphalt, potassium bicarbonate and skeleton template material is (1.0-1.8): (3.0-5.4): (1.0-1.8); The heating rate is 5-8°C / min; The hydrochloric acid solution has a concentration of 0.1-0.3 mol / L.

8. The method for preparing an aerogel-type papermaking additive based on composite fiber materials according to claim 6, characterized in that: The ratio of the copper nitrate, potassium permanganate, manganese sulfate, deionized water and porous carbon nanosheets is (0.025-0.030) mol: (0.14-0.18) mol: (0.045-0.052) mol: (70-100) mL: (5-8) g; The ultrasonic effect has a power of 100-150W; The ratio of the carbon fiber, the composite nanomaterial, and the deionized water is (10-20) g: (3-7) g: (200-300) mL; The mechanical stirring speed is 800-1200r / min; The ultrasonic treatment has a power of 500-600W.

9. The method for preparing an aerogel-type papermaking additive based on composite fiber materials according to claim 1, characterized in that: The specific preparation method of the aerogel type composite fiber material is as follows: 1) dispersing the composite fiber material in deionized water to obtain a dispersion, then adding the composite aerogel to the dispersion, evacuating to 50-100 Pa, and maintaining at 200-300 r / min and 200-300 W ultrasonic action for 30-50 min. After the treatment is completed, centrifuging the product to obtain a pretreated composite fiber material; 2) dissolving potassium antimony tartrate in deionized water, stirring magnetically for 15-30 minutes, adding polyvinyl pyrrolidone, continuing to stir for 15-30 minutes, and then adding thioacetamide to the resulting mixed solution, stirring thoroughly to obtain a reaction solution; 3) The pretreated composite fiber material is ultrasonically cleaned with acetone, distilled water and ethanol for 10-20 minutes respectively, and then added to the reaction solution after drying. After ultrasonic treatment for 10-20 minutes, it is transferred to a reactor, sealed and placed in an oven, and heated at a constant temperature of 180-186°C for 24-26 hours. After the reaction is completed, it is cooled to room temperature, the product is centrifuged, repeatedly washed with deionized water, and dried.

10. The method for preparing an aerogel-type papermaking additive based on composite fiber materials according to claim 9, characterized in that: The dispersion has a solid content of 5-8wt%; The solid-liquid ratio of the composite aerogel and the dispersion is 1: (150-260) g / mL; The ratio of potassium antimony tartrate, deionized water, polyvinyl pyrrolidone and thioacetamide is (0.6-1.4) mol: (60-130) mL: (0.3-0.6) g: (1.3-2.1) mol; The ratio of the pretreated composite fiber material to the reaction solution is (5-12) g: (160-280) mL.

Citation Information

Patent Citations

  • Preparation method of Cu-OMS-2 catalyst and application of Cu-OMS-2 catalyst in degradation of organic pollutants

    CN110479352A

  • Papermaking additive and preparation method thereof

    CN116695485A

  • Powder-assembled composite micro-nano fiber and preparation method thereof

    US20240068160A1