Manufacturing method of low-resistance high-trapping-efficiency glass filtering material

By adopting a glass filter material manufacturing method with low resistance and high capture efficiency, the problem of low resistance or short life of the existing range hood filter material is solved, and efficient filtration and environmentally friendly production are achieved. The materials are cheap and the structure is firm, and they meet green environmental standards.

CN118910927AInactive Publication Date: 2024-11-08EAP ELECTRIC APPLIANCE CO LTD

Patent Information

Application Number
CN202410956578.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The filter materials of existing range hoods have low resistance and low filtration efficiency, or high resistance and short life, high cost, unecotch production, complex structure, inconvenient installation and use, poor durability, and inconvenient cleaning.

Method used

The glass filter material manufacturing method is adopted with low resistance and high capture efficiency. By preparing adhesives and glass fibers, the filter material is made by wet paper forming method, and the flame retardant is applied after drying to form a multi-layer three-dimensional combined structure to ensure The product has low resistance, high filtration efficiency and durability.

Benefits of technology

It realizes the cheap and easy-to-access materials, environmentally friendly production, firm structure, excellent flame retardant effect, water and high temperature resistance, and meets green and environmental protection requirements, has high filtration efficiency, and is directly landfilled and treated with waste materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910927A_ABST
    Figure CN118910927A_ABST
Patent Text Reader

Abstract

The invention discloses a manufacturing method of a low-resistance high-trapping-efficiency glass filtering material, which comprises the following steps: step 1, preparing an adhesive: selecting the type of the adhesive, mixing and stirring the adhesive to obtain the required adhesive, and placing the adhesive in a dip coating machine for later use; step 2, preparing glass fibers: heating a specific glass raw material to proper temperature, pressure and humidity conditions so that the glass raw material becomes soft and is easy to wiredraw, and mixing and stirring the glass raw material into slurry; the slurry in the second step is prepared into a filter material according to an existing wet papermaking forming method, the filter material sequentially passes through three sets of drying cylinders, and the fourth step of finished product detection.The materials are low in price and easy to obtain, production is easy, manufacturing is easy, the production process is environmentally friendly, pollution is avoided, and the filter material is directly buried after being discarded and is treated in the same mode as sand; the material and the structure are firm in structure, low in resistance, high in filtering efficiency, water-resistant, high-temperature-resistant, steam-resistant and excellent in flame-retardant effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of filter materials, in particular to a method for manufacturing a glass filter material with low resistance and high collection efficiency. Background Art

[0002] The existing material technology solutions for range hood filter elements mainly include the following: Metal filter elements are widely used due to their durability, and can be made of aluminum, stainless steel or galvanized steel. Aluminum filter elements can be improved in durability through anodizing, while stainless steel or galvanized steel filter elements are often used in high-end range hoods due to their corrosion resistance. Plant fibers extracted from crop straw are used as filter element materials. This material has low cost and can be replaced and uniformly handled according to actual usage, avoiding the problem of frequent wiping and cleaning of range hoods. Synthetic or organic fiber materials are also used to manufacture range hood filter elements. These materials can be disposable or reusable, depending on their structure and usage requirements. For example, coke activated carbon adsorbents and carbon molecular sieve adsorbents can form multi-layer filter elements with physical and chemical adsorption capabilities. At the same time, the regeneration adsorption force after chemical adsorption is also strong, the service life is long, and it has efficient oil fume purification capabilities. The new nanofiber material is suitable for places that require high-temperature cleaning or high-efficiency oil fume filtration due to its high-efficiency oil fume filtration characteristics. Activated carbon is used to make range hood filter elements due to its strong adsorption properties, which can effectively absorb grease and odor in oil fume. Considering that the range hood filter element may rust after long-term contact with oil fume, some technical solutions use special anti-rust materials or surface treatment technologies to improve the durability of the filter element and the convenience of maintenance.

[0003] These material options each have their own advantages. The durability and corrosion resistance of metal materials make them suitable for long-term use, while plant fiber materials are favored for their cost-effectiveness and environmental protection properties. Nanofiber and activated carbon materials are suitable for specific needs due to their efficient filtering performance. The choice of filter element material depends on the design of the range hood, its expected service life and the user's maintenance habits.

[0004] The existing structural technical solutions for range hood filter elements include the following: Multi-layer adsorbent material structure: composed of three layers of high-efficiency adsorbent materials, such as the upper layer of inorganic polymer coke activated carbon adsorbent, the middle layer of carbon molecular sieve adsorbent, and the lower layer of coke activated carbon adsorbent. Each layer is separated and packaged with non-woven fabrics and installed in a porous frame body made of plastic injection molding; Ionization wire tensioning structure: including two support plates and two positive poles located between the two support plates, with ionization wires connected between the positive poles, and conductive springs connected at both ends of the ionization wires. One end of the conductive spring is hooked to the positive pole through a fixed bent end to achieve tensioning of the ionization wire and reduce bending of the ionization wire; Easy-to-remove filter element structure: the filter barrel is barrel-shaped, with an open upper end, a closed lower end, and a mesh barrel wall; the spirally twisted steel wire fixes and attaches the filter cotton to the inner side of the barrel wall, which is convenient for removing and replacing the filter cotton ; Filter element plate structure: including a box-shaped shell, in which a number of parallel positive plates connected to the positive pole of the power supply and a negative plate connected to the negative pole of the power supply are vertically arranged, forming an electric field to absorb oil fume particles; Range hood filter structure: including a connecting shell, a filter assembly and a drive assembly; The filter assembly includes at least two filter nets, at least two filter elements, and at least two fixing frames, which are used to improve the filtering efficiency and facilitate maintenance. These technical solutions are designed through different structures to improve the filtering efficiency of the range hood filter element, facilitate installation and disassembly, and extend the service life.

[0005] However, traditional filter materials have the following disadvantages:

[0006] (1) Existing range hood filter materials use metal aluminum mesh, which has a strong structure, fire resistance and low resistance, but has extremely low filtration efficiency, with an oil collection efficiency of less than 20%; or non-woven fabrics / paper materials, which have a high filtration efficiency of more than 70%, but have a rapid increase in resistance and a short lifespan, are not fireproof, and are prone to structural collapse;

[0007] (2) Existing range hood filter materials are expensive, the manufacturing process is complex, the production process is not environmentally friendly, and toxic and harmful gases are generated; discarded filters are not environmentally friendly and require special classification and treatment;

[0008] (3) In terms of the performance of existing range hood filter materials, the structure is complex, the installation and use are inconvenient, the durability is poor, the filtration efficiency is low, the service life ends quickly, and it is inconvenient to clean. Summary of the invention

[0009] The purpose of the present invention is to provide a method for manufacturing a low-resistance and high-capture efficiency glass filter material, so as to solve the problems mentioned in the above background technology that the existing metal aluminum mesh used for range hood filter materials, although it has a strong structure and is fireproof and has low resistance, has extremely low filtration efficiency, and the oil collection efficiency is less than 20%; or non-woven fabric materials / paper materials, although the filtration efficiency is high and can be greater than 70%, the resistance increases rapidly and the life is short, and it is not fireproof and the structure is prone to collapse; the existing range hood filter materials have high costs, complex manufacturing processes, and the production process is not environmentally friendly, and toxic and harmful gases are generated; discarded filters are not environmentally friendly and require special classification and treatment; in terms of performance, the existing range hood filter materials have complex structures, inconvenient installation and use, poor durability, low filtration efficiency, quick end of life, and inconvenient cleaning.

[0010] To achieve the above object, the present invention provides the following technical solution: a method for manufacturing a low-resistance and high-collection-efficiency glass filter material, comprising the following steps:

[0011] Step 1: Prepare adhesive: select the type of adhesive and mix and stir it to obtain the required adhesive, and place the adhesive in the Cezannealing coating machine for standby use;

[0012] Step 2: Prepare glass fiber: Use specific glass raw materials, heat them to appropriate temperature, pressure and humidity conditions to make them soft and easy to draw, mix them, and stir them into slurry;

[0013] Step 3, finished product preparation: the slurry in step 2 is made into filter material according to the existing wet papermaking forming method, the filter material is passed through three groups of drying cylinders in sequence to dry the filter material, the adhesive and inorganic flame retardant prepared in step 1 are coated on both sides of the dried filter material, and the filter material is passed through two groups of drying cylinders in sequence to dry the filter material, so that the moisture content of the dried filter material is less than 5%;

[0014] Step 4: Finished product testing: Test the performance indicators of the finished products required for preparation.

[0015] As a preferred technical solution of the present invention, the glass raw material in step 2 is specifically glass particles or glass rods.

[0016] As a preferred technical solution of the present invention, the main components of the glass fiber in step 2 include multiple oxides such as silicon dioxide, aluminum oxide, calcium oxide, magnesium oxide, boron oxide and sodium oxide.

[0017] As a preferred technical solution of the present invention, the glass fiber in step 2 includes the following raw material compositions by weight: 10-20 parts of E-glass fiber, 10-20 parts of C-glass fiber, 10-20 parts of A-glass fiber, 10-20 parts of E-CR glass fiber, 10-20 parts of D-glass fiber, 10-20 parts of S-glass fiber and 10-20 parts of AR-glass fiber, wherein E-glass fiber does not contain boron, has excellent electrical insulation properties and mechanical strength, and is widely used in reinforcing materials and electrical insulation materials of composite materials, and C-glass fiber contains more alkaline oxides, such as sodium oxide. and calcium oxide, has good chemical stability and chemical corrosion resistance, and is suitable for certain specific industrial uses; A-glass fiber usually refers to aluminoborosilicate glass, which has good physical and chemical properties and is suitable for the production of high-strength glass fibers; E-CR glass fiber is an improved alkali-free glass with higher water resistance and acid resistance, and is suitable for applications in certain special environments; D-glass fiber has a low expansion coefficient and is suitable for applications requiring high dimensional stability; S-glass fiber has higher strength and elastic modulus than E-glass fiber and is generally used in high-performance composite materials; AR-glass fiber has high acid resistance and is suitable for chemical and environmental protection fields.

[0018] As a preferred technical solution of the present invention, the temperature in step 2 is based on the melting of glass fiber. The melting of glass fiber refers to the process in which the batch material undergoes silicate reaction, melting and then transforms into homogeneous glass liquid at high temperature. The specific melting temperature depends on the raw materials and production process used. The melting temperature of glass is between 1000°C and 2000°C.

[0019] As a preferred technical solution of the present invention, the pressure in step 2 is based on the flame drawing process commonly used for the preparation process of high-melting-point glass fiber products. In this process, the pressure of oxygen introduced into the oxygen pipe is 0.06-0.1MPa, and the pressure of the gas introduced into the gas pipe is 0.06-0.1MPa.

[0020] As a preferred technical solution of the present invention, the adhesive in step 1 includes the following raw materials in parts by weight: 5-20 parts of silicone sealant, 10-20 parts of polyurethane sealant, 10-20 parts of acrylic sealant, 5-30 parts of modified polymer sealant, 15-30 parts of silicone sealant, 10-20 parts of epoxy resin adhesive and 10-20 parts of modified silane sealant. Among them, silicone sealant is commonly used in building curtain walls, doors and windows, and sun room outdoor fields due to its excellent weather resistance, high and low temperature resistance, UV resistance and aging resistance. Polyurethane adhesive has good bonding strength, water resistance, chemical resistance and weather resistance, and is suitable for a variety of outdoor Bonding and sealing of building structures, acrylic adhesives are suitable for bonding a variety of outdoor materials such as metal, ceramics, and wood due to their strong bonding force, high initial adhesion, and good weather resistance. Modified polymer sealants have good weather resistance, flexibility, and adhesion, and are suitable for sealing joints on building exterior walls. In addition to silicone sealants, other silicone-based sealants are also widely used due to their weather resistance, temperature resistance, and chemical resistance. Epoxy resin adhesives have very good bonding strength and chemical resistance, and some modified epoxy resins also have good outdoor weather resistance. Modified silane sealants combine the weather resistance of silane with the flexibility of polyurethane, and are suitable for sealing outdoor joints and cracks.

[0021] As a preferred technical solution of the present invention, the performance indicators in step 2 are specifically diameter, length, toughness, expansion coefficient and brittleness. The diameter is specifically the diameter of the monofilament of the glass fiber ranging from a few microns to more than 20 microns. Specifically, the monofilament diameter of the primary fiber is greater than 20 μm, the monofilament diameter of the intermediate fiber is between 10-20 μm, and the monofilament diameter of the advanced fiber is in the range of 3-10 μm. Sometimes glass fibers with a diameter of less than 4 μm are also called ultrafine fibers. In practical applications, modern production technology produces finer fibers, such as some products. 7μm glass fiber is used. The length is specifically the length of the glass fiber. There is no specific indicator range, but it is determined according to the production process and application requirements. For example, continuous glass fiber is an infinitely long fiber, while the length of short fiber or fixed-length fiber is cut according to the needs. The toughness, the toughness of glass fiber is usually measured by its tensile strength and elongation at break. The tensile strength is 6.3-6.9g / d in the standard state and 5.4-5.8g / d in the wet state. The elongation at break is usually around 3%. The expansion coefficient is the thermal expansion coefficient of the glass fiber in the range of 2-8×

[0022] ^

[0023] 10^ -6 / ℃ range, the brittleness specifically refers to the brittleness of the glass fiber, which is related to its composition and production process. The main components of the glass fiber are silicon dioxide, aluminum oxide, calcium oxide, boron oxide, magnesium oxide, and sodium oxide. According to the alkali content in the glass, it is divided into alkali-free, medium-alkali and high-alkali glass fibers. Different types of glass fibers have different performances in chemical corrosion resistance and water resistance, but usually have higher hardness and brittleness.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] 1. The materials are cheap and easy to obtain, the production is simple and easy to manufacture, the production process is environmentally friendly and does not produce pollution, and it can be directly landfilled after being discarded, just like sand;

[0026] 2. The material and structure have a strong structure, low resistance and high filtration efficiency, are resistant to water, high temperature and steam, and have excellent flame retardant effect;

[0027] 3. Made of glass fiber, it is fireproof and ensures the stiffness of the filter. It adopts a multi-layer three-dimensional combination structure of coarse and fine fibers in one layer, and through the program design of the production process, it produces a multi-layer sandwich structure with two layers of high-density skin or high-density center layer, ensuring low resistance and high filtration efficiency.

[0028] 4. A special water-based adhesive formula is used to ensure that the product structure does not deform at a high temperature of 200 degrees, and can withstand a high humidity environment of 100 degrees water vapor without hydrolysis reaction to damage the structure, and no formaldehyde or VOC harmful gases are generated, meeting green environmental protection requirements;

[0029] 5. Use special inorganic flame retardant ingredients to ensure extreme conditions (oil coating 200g / m 2 ) to ensure that the fire will be extinguished within 3 seconds and the fire area is less than 10cm 2 At the same time, unlike ordinary phosphorus-nitrogen flame retardants, it does not guarantee the above fire resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 is a flow chart of the present invention;

[0031] Figure 2 This is a flow chart of the oil capture test of the glass fiber filter of the present invention;

[0032] Figure 3 This is a flow chart of the formaldehyde test of the glass fiber filter of the present invention;

[0033] Figure 4 This is a result diagram of the formaldehyde test of the glass fiber filter of the present invention;

[0034] Figure 5 This is a flow chart of the pressure loss test of the glass fiber filter of the present invention;

[0035] Figure 6 This is a result diagram of the pressure loss test of the glass fiber filter of the present invention;

[0036] Figure 7 It is a flow chart of the glass fiber filter collapse test of the present invention;

[0037] Figure 8 The figure is a flow chart of the glass fiber filter combustion test of the present invention. DETAILED DESCRIPTION

[0038] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0039] See also Figure 1-8 The present invention provides a method for manufacturing a glass filter material with low resistance and high collection efficiency, comprising the following steps:

[0040] Step 1: Prepare adhesive: select the type of adhesive and mix and stir it to obtain the required adhesive, and place the adhesive in the Cezannealing coating machine for standby use;

[0041] Step 2: Prepare glass fiber: Use specific glass raw materials, heat them to appropriate temperature, pressure and humidity conditions to make them soft and easy to draw, mix them, and stir them into slurry;

[0042] Step 3, finished product preparation: the slurry in step 2 is made into filter material according to the existing wet papermaking forming method, the filter material is passed through three groups of drying cylinders in sequence to dry the filter material, the adhesive and inorganic flame retardant prepared in step 1 are coated on both sides of the dried filter material, and the filter material is passed through two groups of drying cylinders in sequence to dry the filter material, so that the moisture content of the dried filter material is less than 5%;

[0043] Step 4: Finished product testing: Test the performance indicators of the finished products required for preparation.

[0044] The glass raw material in step 2 is specifically glass particles or glass rods.

[0045] The main components of the glass fiber in step 2 include various oxides such as silicon dioxide, aluminum oxide, calcium oxide, magnesium oxide, boron oxide and sodium oxide.

[0046] In step 2, the glass fiber includes the following raw material compositions by weight: 10-20 parts of E-glass fiber, 10-20 parts of C-glass fiber, 10-20 parts of A-glass fiber, 10-20 parts of E-CR glass fiber, 10-20 parts of D-glass fiber, 10-20 parts of S-glass fiber and 10-20 parts of AR-glass fiber, wherein E-glass fiber does not contain boron, has excellent electrical insulation properties and mechanical strength, and is widely used in reinforcing materials and electrical insulation materials of composite materials, and C-glass fiber contains more alkaline oxides, such as sodium oxide and calcium oxide, and has good A-glass fiber usually refers to aluminoborosilicate glass, which has good physical and chemical properties and is suitable for the production of high-strength glass fibers; E-CR glass fiber is an improved alkali-free glass with higher water resistance and acid resistance, suitable for applications in certain special environments; D-glass fiber has a low expansion coefficient and is suitable for applications requiring high dimensional stability; S-glass fiber has higher strength and elastic modulus than E-glass fiber and is usually used in high-performance composite materials; AR-glass fiber has high acid resistance and is suitable for chemical and environmental protection fields.

[0047] The temperature in step 2 is based on the melting of glass fiber. The melting of glass fiber refers to the process in which the batch materials undergo silicate reaction, melting and then transform into homogeneous glass liquid at high temperature. The specific melting temperature depends on the raw materials and production process used. The melting temperature of glass is between 1000°C and 2000°C.

[0048] The pressure in step 2 is based on the flame drawing process commonly used for the preparation of high melting point glass fiber products. In this process, the pressure of oxygen introduced into the oxygen pipe is 0.06-0.1MPa, and the pressure of the gas introduced into the gas pipe is 0.06-0.1MPa.

[0049] The adhesive in step 1 includes the following raw materials in parts by weight: 5-20 parts of silicone sealant, 10-20 parts of polyurethane sealant, 10-20 parts of acrylic sealant, 5-30 parts of modified polymer sealant, 15-30 parts of silicone sealant, 10-20 parts of epoxy resin adhesive and 10-20 parts of modified silane sealant. Among them, silicone sealant is commonly used in building curtain walls, doors and windows, and sun rooms for its excellent weather resistance, high and low temperature resistance, UV resistance and aging resistance. Polyurethane adhesive has good bonding strength, water resistance, chemical resistance and weather resistance, and is suitable for bonding and bonding of various outdoor building structures. Sealing, acrylic adhesives are suitable for bonding a variety of outdoor materials such as metal, ceramics, and wood due to their strong bonding force, high initial adhesion, and good weather resistance. Modified polymer sealants have good weather resistance, flexibility, and adhesion, and are suitable for sealing joints on building exterior walls. In addition to silicone sealants, other silicone-based sealants are also widely used due to their weather resistance, temperature resistance, and chemical resistance. Epoxy resin adhesives have excellent bonding strength and chemical resistance, and some modified epoxy resins also have good outdoor weather resistance. Modified silane sealants combine the weather resistance of silane and the flexibility of polyurethane, and are suitable for sealing outdoor joints and cracks.

[0050] The performance indicators in step 2 are specifically diameter, length, toughness, expansion coefficient and brittleness. The diameter is specifically the diameter of the single filament of the glass fiber, which ranges from a few microns to more than twenty microns. Specifically, the single filament diameter of the primary fiber is greater than 20μm, the single filament diameter of the intermediate fiber is between 10-20μm, and the single filament diameter of the advanced fiber is in the range of 3-10μm. Sometimes glass fibers with a diameter of less than 4μm are also called ultrafine fibers. In practical applications, modern production technology produces finer fibers. For example, some products use 7μm glass fibers. The length is specifically the length of the glass fiber. There is no specific indicator range, but it is determined according to the production process and application requirements. For example, continuous glass fiber is an infinitely long fiber, while the length of short fiber or fixed length fiber is cut as needed. Toughness. The toughness of glass fiber is usually measured by its tensile strength and elongation at break. The tensile strength is 6.3-6.9g / d in standard state and 5.4-5.8g / d in wet state. The elongation at break is usually around 3%. The expansion coefficient is the thermal expansion coefficient of the glass fiber.

[0051] ^

[0052] Expansion coefficient is 2-8×10^ -6 / ℃ range, the brittleness is specifically related to the brittleness of glass fiber and its composition and production process. The main components of glass fiber are silicon dioxide, aluminum oxide, calcium oxide, boron oxide, magnesium oxide, and sodium oxide. According to the alkali content in the glass, it is divided into alkali-free, medium alkali and high alkali glass fiber. Different types of glass fiber have different performances in chemical corrosion resistance and water resistance, but usually have higher hardness and brittleness.

[0053] Embodiment 1:

[0054] In the present invention, the adhesive type is selected and mixed and stirred to obtain the required adhesive, wherein 20 parts of silicone sealant, 10 parts of polyurethane sealant, 10 parts of acrylic sealant, 5 parts of modified polymer sealant, 15 parts of organic silicon sealant, 20 parts of epoxy resin adhesive and 20 parts of modified silane sealant are obtained; specific glass raw materials are used, and are heated to appropriate temperature, pressure and humidity conditions to make them soft and easy to draw, so as to obtain the required glass fiber, and the performance indicators thereof are tested; wherein 10 parts of E-glass fiber, 10 parts of C -glass fiber 10 parts, A-glass fiber 10 parts, E-CR glass fiber 10 parts, D-glass fiber 20 parts, S-glass fiber 20 parts and AR-glass fiber 20 parts, the slurry is made into filter material according to the existing wet papermaking molding method, the filter material is passed through three groups of drying cylinders in sequence to dry the filter material, the adhesive and inorganic flame retardant prepared in step 1 are coated on both sides of the dried filter material, and the filter material is passed through two groups of drying cylinders in sequence to dry the filter material, so that the moisture content of the dried filter material is less than 5%, and the performance indicators of the prepared finished product are tested.

[0055] Embodiment 2:

[0056] In the present invention, the adhesive type is selected and mixed and stirred to obtain the required adhesive, wherein 10 parts of silicone sealant, 10 parts of polyurethane sealant, 10 parts of acrylic sealant, 10 parts of modified polymer sealant, 30 parts of organic silicon sealant, 20 parts of epoxy resin adhesive and 10 parts of modified silane sealant are used; specific glass raw materials are heated to appropriate temperature, pressure and humidity conditions to make them soft and easy to draw, and the required glass fiber is obtained, and its performance indicators are tested; wherein 20 parts of E-glass fiber, 20 parts of C -glass fiber 20 parts, A-glass fiber 20 parts, E-CR glass fiber 10 parts, D-glass fiber 10 parts, S-glass fiber 10 parts and AR-glass fiber 10 parts, prepare filter material by the existing wet papermaking method, pass the filter material through three groups of drying cylinders in sequence to dry the filter material, apply the adhesive and inorganic flame retardant prepared in step 1 on both sides of the dried filter material, pass the filter material through two groups of drying cylinders in sequence to dry the filter material, make the moisture content of the dried filter material less than 5%, and test the performance indicators of the finished product required for preparation.

[0057] Embodiment 3:

[0058] In the present invention, the adhesive type is selected and mixed and stirred to obtain the required adhesive, wherein 20 parts of silicone sealant, 10 parts of polyurethane sealant, 10 parts of acrylic sealant, 10 parts of modified polymer sealant, 30 parts of organic silicon sealant, 10 parts of epoxy resin adhesive and 10 parts of modified silane sealant are obtained; specific glass raw materials are used, and are heated to appropriate temperature, pressure and humidity conditions to make them soft and easy to draw, so as to obtain the required glass fiber, and the performance indicators thereof are tested; wherein 10 parts of E-glass fiber, 20 parts of C-glass fiber, 20 parts of A-glass fiber, 20 parts of E-CR glass fiber, 10 parts of D-glass fiber, 10 parts of S-glass fiber and 10 parts of AR-glass fiber, the slurry is made into filter material according to the existing wet papermaking molding method, the filter material is passed through three groups of drying cylinders in sequence to dry the filter material, the adhesive prepared in step 1 and the inorganic flame retardant are coated on both sides of the dried filter material, and the filter material is passed through two groups of drying cylinders in sequence to dry the filter material, so that the moisture content of the dried filter material is less than 5%, and the performance index of the prepared finished product is tested

[0059] Embodiment 4:

[0060] In the present invention, the adhesive type is selected and mixed and stirred to obtain the required adhesive, wherein 20 parts of silicone sealant, 10 parts of polyurethane sealant, 10 parts of acrylic sealant, 5 parts of modified polymer sealant, 25 parts of organic silicon sealant, 20 parts of epoxy resin adhesive and 10 parts of modified silane sealant are obtained; specific glass raw materials are used, and are heated to appropriate temperature, pressure and humidity conditions to make them soft and easy to draw, so as to obtain the required glass fiber, and the performance indicators thereof are tested; wherein 10 parts of E-glass fiber, 10 parts of C -glass fiber 20 parts, A-glass fiber 10 parts, E-CR glass fiber 10 parts, D-glass fiber 10 parts, S-glass fiber 20 parts and AR-glass fiber 20 parts, the slurry is made into filter material according to the existing wet papermaking molding method, the filter material is passed through three groups of drying cylinders in sequence to dry the filter material, the adhesive and inorganic flame retardant prepared in step 1 are coated on both sides of the dried filter material, and the filter material is passed through two groups of drying cylinders in sequence to dry the filter material, so that the moisture content of the dried filter material is less than 5%, and the performance indicators of the prepared finished product are tested.

[0061] Embodiment 5:

[0062] In the present invention, the adhesive type is selected and mixed and stirred to obtain the required adhesive, wherein 20 parts of silicone sealant, 10 parts of polyurethane sealant, 15 parts of acrylic sealant, 10 parts of modified polymer sealant, 15 parts of organic silicon sealant, 20 parts of epoxy resin adhesive and 20 parts of modified silane sealant are obtained; specific glass raw materials are used, and are heated to appropriate temperature, pressure and humidity conditions to make them soft and easy to draw, so as to obtain the required glass fiber, and the performance indicators thereof are tested; wherein 10 parts of E-glass fiber, 10 parts of C -glass fiber 20 parts, A-glass fiber 10 parts, E-CR glass fiber 20 parts, D-glass fiber 10 parts, S-glass fiber 10 parts and AR-glass fiber 20 parts, the slurry is made into filter material according to the existing wet papermaking molding method, the filter material is passed through three groups of drying cylinders in sequence to dry the filter material, the adhesive and inorganic flame retardant prepared in step 1 are coated on both sides of the dried filter material, and the filter material is passed through two groups of drying cylinders in sequence to dry the filter material, so that the moisture content of the dried filter material is less than 5%, and the performance indicators of the prepared finished product are tested.

[0063] The drawing process of glass fiber requires the use of specific glass raw materials, which are usually glass particles or glass rods. By heating to an appropriate temperature, they become soft and easy to draw. The main components of glass fiber include silicon dioxide, and it also contains a variety of oxides such as aluminum oxide, calcium oxide, magnesium oxide, boron oxide, and sodium oxide. Different components and proportions determine the performance and application areas of glass fiber. The choice of adhesive should be determined according to the specific application environment, the type of bonding material, and the required performance characteristics. For example, for joints that need to withstand large displacements or deformations, it is necessary to choose a sealant with better flexibility and elasticity. For applications that are directly exposed to sunlight and adverse weather conditions, it is necessary to choose a sealant with stronger weather resistance. Adhesive with good and UV resistance, humidity conditions are also very important in the production process of glass fiber, especially in the raw silk drying stage. According to, the purpose of raw silk drying is to remove moisture in the raw silk cake and reduce its moisture content to the specified index. The drying temperature is in the range of 120-135℃ and the drying time is in the range of 8-18 hours. Factors affecting the drying of glass fiber raw silk include temperature, air volume and relative humidity. Usually, the raw silk goes through multiple processes such as drawing, unwinding, warping and weaving for a long time, so it only needs natural drying to meet the requirements of production process and products. It should be noted that the specific processing temperature, pressure and humidity conditions will vary according to production facilities, raw material characteristics, product specifications and production efficiency factors.

[0064] In conjunction with the instruction manual Figure 2, weigh the fiberglass filter and record the weight, and mark it as "left or right", then weigh the left or right filter frame and record the weight, install the left fiberglass filter on the left filter frame, and install it into the frame along the edge of the filter frame, then align the wire rack and put it into the frame to fix the fiberglass filter. Note that the direction of the fiberglass filter with the red mark is placed on the same side as the wire rack, hold the protruding part of the filter frame with your hand, first hold the filter frame against the upper part of the range hood, and then put it into the lower part, place the wire rack facing outward, and after the left and right fiberglass filters are installed, turn on the anemometer, place it in front of the fiberglass filter for 2 minutes, keep a short distance from the fiberglass filter, and do not directly touch the fiberglass filter Filter, after the wind speed count value stabilizes, press "HOLD" to start moving slowly from one side of the glass fiber filter to the other side, from left to right, and then from top to bottom in a total of 3 lines to sweep the entire area of ​​the filter. The speed should not be too fast, and the total sweeping time should be about 1 minute; then press the "HOLD" key to stop, and then press the "MAX, MAIN, AVG" key to record the maximum, minimum and average wind speed values ​​during the entire measurement process, take some paper towels to weigh and record the weight values, then stand the paper towels upright and place them around the test bench, and fix them on the rope with small clips. At the same time, place a clean iron pot and a stainless steel bucket on the electric furnace, turn on the heating furnace to 600KW, and start heating; and place the oil and water on the electronic balance , return to zero at the same time, turn on the maximum air volume switch of the range hood to start running; at the same time, record the initial pressure loss value. When the temperature in the pot reaches about 350℃, start the test, turn on the oil and water supply switches at the same time and start timing, and lower all the curtains to avoid oil smoke splashing during the experiment; during the test, keep the temperature of the pot at about 270℃; record the oil and water supply data every 5 minutes, and record the pressure loss data at this time. After 30 minutes of the test, turn off the oil and water supply switches, turn off the electric furnace switch, and use the anemometer to detect the wind speed value again according to the previous method, and keep a record. The whole experimental process only needs to detect the wind speed twice. Spread the previously prepared (and weighed) paper towels flat on the work surface, and then remove the left or right fiberglass filter from Take it off the range hood, put it vertically on it, carefully remove the wire rack, take out the glass fiber filter and weigh it, and record the data; then wipe the oil adhering to the wire rack, the filter frame and the glass fiber filter rack on the oil collection test bench with a paper towel, then weigh the paper towel, subtract the original weight, and the amount of scattered oil, take down the paper towels around the test bench, wipe the table clean, wipe the range hood clean, wipe the pan and the stainless steel bucket clean, weigh the paper towel, subtract the original weight, and the amount of scattered oil, the oil collection efficiency calculation method: oil collection efficiency (%) = (oil amount on the left and right filters + oil amount) / (total added oil amount - scattered oil amount) * 100%, experimental results: the two test results of the present invention are: 77.49%, 76.63%, and the result of Xu Company is: 74.13%. .

[0065] In conjunction with the instruction manual Figure 3 , cut the glass fiber filter along the edge of the 150×50mm cardboard with a knife, cut it into 10 pieces of 150×50mm size, and mark the name and number of each glass fiber filter with a marker, evenly apply vaseline on the edge of the glass desiccator cover to ensure that the glass desiccator does not leak, put the three samples into the three corresponding marked glass desiccators, place 4 glass fiber filter samples vertically on the bottom edge of the glass desiccator, and then place three flat on the vertical top, and place three in the middle of the container to avoid overlapping of glass fiber filters to ensure that there is enough space for formaldehyde to be released, cover the lid tightly, plug it with a silicone plug, and leave it for 24 hours. After 10 hours, open the formaldehyde detection instrument and empty it for 10 minutes, then use the formaldehyde meter to detect the formaldehyde content. The purpose of emptying for 10 minutes is to eliminate the residual formaldehyde gas in the pipeline. Then choose the appropriate measurement time. If the concentration is low, 0-0.4PPM should select the No.008 gear on the instrument, about 30mins; if the concentration is high, 0-1PPM should select the No.009 gear on the instrument, about 15mins, and tightly plug the catheter with the silicone plug on the glass desiccant. Move quickly to avoid letting the gas inside escape, and then wait for the final reading of the formaldehyde detection instrument and record it. The experimental results are attached in conjunction with the instruction manual. Figure 4 The current product and the sample of Xu Company selected No. 009 gear for 15 minutes, but it still exceeded the detection range of the instrument, > 1PPM. The sample of the present invention selected No. 008 gear for 30 minutes and the result was 0.095PPM.

[0066] In conjunction with the instruction manual Figure 5 , cut the glass fiber filter along the edge of the cardboard into a size of 215×215mm, and mark the sample name and number of the glass fiber filter, put the cut glass fiber filter sample into the fixture according to the marked direction, and then put the fixture on the pressure loss detection instrument, and then rotate the screws around to fix the fixture, turn on the switch, and adjust the electronic voltage regulator on the left side of the instrument to 0.86mV, 1.79mV, 2.16mV, 2.72mV, 3.65mV, 4.58mV, and the corresponding surface wind speeds are 0.5m / s, 1.0m / s, 1.2m / s, 1.5m / s, 2.0m / s, 2.5m / s respectively; then write down the pressure loss value corresponding to the pressure loss table on the right at the same time, combined with the instructions attached Figure 6 The pressure loss of the product of the present invention is slightly higher than that of the glass fiber samples of the existing ventilation fans of Asahi Company and Duskin, and is a product that meets the requirements.

[0067] In conjunction with the instruction manual Figure 7, cut the glass fiber filter along the size of the cardboard into a size of 150*80mm, and mark the arrow along the direction of the glass fiber diameter, and clearly mark the name and number of the glass fiber filter sample, fill 1L of boiling water into the boiling pot, put the perforated partition into the boiling pot (the perforated partition is a component of the boiling pot), clamp the two types of glass fiber filter samples, a total of 4 PCS, on two ropes respectively, and hang them above the perforated partition, then cover the lid of the boiling pot, put the boiling pot on the electric stove, turn on the electric stove and rotate it to the 600W position ; Boil water for 2 hours. After the experiment, take down the boiling pot and open the lid. Put it on the platform to cool down and observe whether each glass fiber filter screen sample has collapse phenomenon and whether it has moisture regain and stickiness phenomenon. After 2 hours of boiling water experiment for two samples in the longitudinal and transverse directions of the present invention, the appearance of the glass fiber sample maintains a good shape, and no falling off between the glass fibers and no sticky moisture regain are found. After 2 hours of boiling water experiment for two samples in the longitudinal and transverse directions of Y company, the appearance of the glass fiber sample is completely deformed, the glass fibers fall off seriously, and it is found that the sticky moisture regain phenomenon is also very serious.

[0068] In conjunction with the instruction manual Figure 8, cut the glass fiber filter along the size of the cardboard into the required size, mark the name and number of the glass fiber filter sample, weigh the weight of each glass fiber filter with the corresponding number, keep a record, pour the Nissin oil into a clean tray, the amount of oil should be enough to completely soak the glass fiber filter, put the cut glass fiber filter into the tray with the right amount of oil, gently press the glass fiber filter with your hand to penetrate the oil into the glass fiber filter, and apply the oil to the glass fiber filter without oil by hand, Then change the glass fiber filter to the other side and repeat the operation. After soaking completely, pick up the glass fiber filter, clamp one corner of the glass fiber filter with a clip and hang it on the stand. The stand is placed directly above the tray, and then the oiled glass fiber filter is hung on the stand for 90 minutes. After 90 minutes, remove the glass fiber filter, wipe off the oil droplets on the surface of the bottom corner (the oil dripping part) with a clean cloth, and then place the removed glass fiber filter on a work surface covered with a clean towel. A clean cloth of the same size as the sample is also laid flat on the surface; depending on the oiling condition on the glass fiber filter, for areas with more oil droplets, gently press down with your hands to wipe off the excess oil on the surface; b. Then pick up the glass fiber filter and put it on an electronic balance for weighing. If the amount of oil on the glass fiber filter exceeds the standard requirements (sample size: 297*240mm, oiling amount: 11g; sample size: 340*240mm, oiling amount: 13g), remove the excess oil in the same way as a to meet the standard requirements; c. If it is found that there is too little oil when weighing, use a small brush to dip some oil and gently brush it on the edge of the tray or rub it on the cloth to remove excess oil to avoid excessive oil and uneven application of oil on the surface of the glass fiber filter; when brushing, use a brush to evenly apply from one side of the glass fiber filter to the other side, and then brush back and forth to ensure that the surface is evenly coated; make sure that both sides of the glass fiber filter are brushed when brushing; d.Weigh the weight of each piece of oil-coated glass fiber filter and make corresponding records; hang the oil-coated glass fiber filter on the rack in turn until all the samples are oiled, put the oil-coated glass fiber filter into the fixture in the combustion box, first fix it on the place with nails on the bottom of the fixture, ensure that the sample is placed in the middle of the fixture, then close the fixture, turn on the power of the flammability tester, press and hold the SELECT button to adjust the display of the flame height adjustment, then press the GASS supply button, ignite and adjust the flame height to 45mm, and the flame color is yellow; set the data of each parameter (heating time is 60s), and keep the instrument stable for 10 minutes after turning it on so that the gas in the internal pipeline can be evenly stabilized before entering To conduct the test, place the fixture holding the glass fiber filter in the combustion test instrument, then press the "SELECT key" to adjust to the "test" state (the light at the test mark is red), then press the "GASS supply key", and then press the "GASS supply key" and "heating start key" at the same time. When the glass fiber filter is observed to have a fire phenomenon or the flame begins to tilt to one side, press the "heating start key after ignition" and the instrument will automatically start timing; when the flame begins to go out, press the "residual flame stop" and "remaining personnel stop" keys, and record the residual flame time and remaining personnel time at the same time, remove the glass fiber filter, use a steel ruler to measure the size of the burned glass fiber surface, make a record, and calculate the combustion performance of the glass fiber filter according to the formula.

[0069] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for producing a low-resistance and high-collection-efficiency glass filter material, characterized in that: The following steps are involved: Step 1: Prepare adhesive: select the type of adhesive and mix and stir it to obtain the required adhesive, and place the adhesive in the Cezannealing coating machine for standby use; Step 2: Prepare glass fiber: Use specific glass raw materials, heat them to appropriate temperature, pressure and humidity conditions to make them soft and easy to draw, mix them, and stir them into slurry; Step 3, finished product preparation: the slurry in step 2 is made into filter material according to the existing wet papermaking forming method, the filter material is passed through three groups of drying cylinders in sequence to dry the filter material, the adhesive and inorganic flame retardant prepared in step 1 are coated on both sides of the dried filter material, and the filter material is passed through two groups of drying cylinders in sequence to dry the filter material, so that the moisture content of the dried filter material is less than 5%; Step 4: Finished product testing: Test the performance indicators of the finished products required for preparation.

2. The method for manufacturing a low-resistance and high-collection-efficiency glass filter material according to claim 1, characterized in that: The glass raw material in step 2 is specifically glass particles or glass rods.

3. The method for manufacturing a low-resistance and high-collection-efficiency glass filter material according to claim 1, characterized in that: The main components of the glass fiber in step 2 include various oxides such as silicon dioxide, aluminum oxide, calcium oxide, magnesium oxide, boron oxide and sodium oxide.

4. The method for manufacturing a low-resistance and high-collection-efficiency glass filter material according to claim 1, characterized in that: The glass fiber in step 2 includes the following raw material compositions in parts by weight: 10-20 parts of E-glass fiber, 10-20 parts of C-glass fiber, 10-20 parts of A-glass fiber, 10-20 parts of E-CR glass fiber, 10-20 parts of D-glass fiber, 10-20 parts of S-glass fiber and 10-20 parts of AR-glass fiber.

5. The method for manufacturing a low-resistance and high-collection-efficiency glass filter material according to claim 1, characterized in that: The temperature in step 2 is based on the melting of glass fiber. The melting of glass fiber refers to the process in which the batch materials undergo silicate reaction, melting and then transform into homogeneous glass liquid at high temperature. The specific melting temperature depends on the raw materials and production process used. The melting temperature of glass is between 1000°C and 2000°C.

6. The method for manufacturing a low-resistance and high-collection-efficiency glass filter material according to claim 1, characterized in that: The pressure in step 2 is based on the commonly used preparation process for high melting point glass fiber products, which is to use flame drawing to produce wire. In this process, the pressure of oxygen introduced into the oxygen pipe is 0.06-0.1MPa, and the pressure of the gas introduced into the gas pipe is 0.06-0.1MPa.

7. The method for manufacturing a low-resistance and high-collection-efficiency glass filter material according to claim 1, characterized in that: The adhesive in step 1 comprises the following raw materials in parts by weight: 5-20 parts of silicone sealant, 10-20 parts of polyurethane sealant, 10-20 parts of acrylic sealant, 5-30 parts of modified polymer sealant, 15-30 parts of silicone sealant, 10-20 parts of epoxy resin adhesive and 10-20 parts of modified silane sealant.

8. The method for manufacturing a low-resistance and high-collection-efficiency glass filter material according to claim 1, characterized in that: The performance indicators in step 2 are specifically diameter, length, toughness, expansion coefficient and brittleness. The diameter is specifically the diameter of the monofilament of the glass fiber, which ranges from a few microns to more than twenty microns. Specifically, the monofilament diameter of the primary fiber is greater than 20μm, the monofilament diameter of the intermediate fiber is between 10-20μm, and the monofilament diameter of the advanced fiber is in the range of 3-10μm. Sometimes glass fibers with a diameter less than 4μm are also called ultrafine fibers. In practical applications, modern production technology produces finer fibers. For example, some products use 7μm glass fibers. The length is specifically the length of the glass fiber, which has no specific indicator range, but is determined according to the production process and application requirements. For example, continuous glass fibers are fibers of infinite length, while the length of short fibers or fixed-length fibers is cut as needed. The toughness, the toughness of glass fibers is usually measured by their tensile strength and elongation at break. The tensile strength is 6.3-6.9g / d in standard state and 5.4-5.8g / d in wet state. The elongation at break is usually around 3%,^ The expansion coefficient is the thermal expansion coefficient of glass fiber in the range of 2-8×10^ -6 / ℃ range, the brittleness specifically refers to the brittleness of the glass fiber, which is related to its composition and production process. The main components of the glass fiber are silicon dioxide, aluminum oxide, calcium oxide, boron oxide, magnesium oxide, and sodium oxide. According to the alkali content in the glass, it is divided into alkali-free, medium-alkali and high-alkali glass fibers. Different types of glass fibers have different performances in chemical corrosion resistance and water resistance, but usually have higher hardness and brittleness.

Citation Information

Patent Citations

  • Preparation method of smoke dust filter material by using glass fiber

    CN102527150A

  • High-strength glass fiber air filter paper and preparation method thereof

    CN103721477A

  • High-strength glass fiber

    CN107759095A

  • High temperature resistant epoxy sealant

    CN109280522A

  • Preparation technology of glass fiber F9 grade air filtering material

    CN110090493A

Cited By

  • Manufacturing method of low-resistance high-trapping-efficiency glass filtering material

    CN120393568A

  • Manufacturing process of glass fiber filter screen with high trapping efficiency and portable dismounting and mounting device

    CN120420745A

  • A manufacturing process and portable assembly / disassembly device for a high-capture-efficiency fiberglass filter.