Water-resistant corrugated packaging material

By modifying silica to form a composite micro-nano structure and combining hydrophobic modifiers, the problems of poor water resistance and insufficient durability of corrugated cartons are solved, and the superhydrophobicity and durability of corrugated cartons are improved.

CN118910928AActive Publication Date: 2024-11-08ZHENGYE INT HLDG CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410952568.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08
Estimated Expiration
2044-07-16

AI Technical Summary

Technical Problem

Due to the material properties of corrugated cartons, poor water resistance, existing coating technology is difficult to achieve long-term superhydrophobic effects, and is prone to failure due to friction and wear.

Method used

The nano-sized silica and epoxy silane coupling agent are modified to modify the micro-sized silica to form a composite micro-nano structure, and self-polymerization is used to use dopamine hydrochloride hydrochloride, combined with silanoxy hydrophobic modifier. Modified fillers are prepared to form low-surface energy coatings, giving corrugated cartons superhydrophobicity and durability.

Benefits of technology

The superhydrophobicity and durability of the surface of the corrugated carton are realized, which can effectively resist wear and damage in actual use and maintain long-term superhydrophobic properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004947628530000121
    Figure BDA0004947628530000121
  • Figure BDA0004947628530000131
    Figure BDA0004947628530000131
Patent Text Reader

Abstract

The invention relates to a water-resistant corrugated packaging material, and belongs to the technical field of corrugated packaging materials. The preparation method comprises the following steps: firstly, treating nanoscale silicon dioxide by using an amino silane coupling agent and modifying the nanoscale silicon dioxide with an amino group, treating micron-sized silicon dioxide by using an epoxy silane coupling agent and modifying micron-sized silicon dioxide with an epoxy group, and then compounding the nanoscale silicon dioxide on the surface of the micron-sized silicon dioxide under the action of the amino group and the epoxy group. The preparation method comprises the following steps: firstly, preparing a micro-nano structure, then, carrying out self-polymerization-wrapping on the micro-nano structure by utilizing dopamine hydrochloride under aerobic and alkaline conditions to provide a secondary modification platform, and finally, adding a siloxy hydrophobic modifier, so that the micro-nano structure has low surface energy under the action of siloxy and hydroxyl, thereby preparing the modified filler. When the coating obtained by mixing the super-hydrophobic coating with other components is applied to coating of corrugated cartons, the super-hydrophobic coating endows the surfaces of the corrugated cartons with super-hydrophobic properties and is excellent in durability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of corrugated packaging materials, and in particular relates to a water-resistant corrugated packaging material. Background Art

[0002] Corrugated box is a very commonly used corrugated packaging material, which is made of corrugated cardboard through die-cutting, creasing, nailing or gluing. In daily life, corrugated boxes are widely used in the packaging of goods due to their many advantages such as portability and low cost. However, since the raw materials for the preparation of corrugated boxes / corrugated cardboard are mainly chemical components such as cellulose and hemicellulose, their water resistance is very poor. The large amount of hydrophilic hydroxyl groups on the surface make it very easy to get damp, which seriously affects the normal packaging function. In order to solve this technical problem, many existing technologies will use lamination to give corrugated boxes It is water-resistant and moisture-proof. For example, by introducing hydrophobic functional fillers into the film-forming material, a hydrophobic surface can be well formed, thereby improving water resistance. However, this technology still has disadvantages that limit its actual application effect. This is because on the one hand, the water resistance after coating is still limited and the super-hydrophobic property cannot be achieved. On the other hand, even if the super-hydrophobic property is achieved, there will be a lot of friction and wear on the surface of the corrugated box during actual use. At this time, the micro-nano rough structure formed by the hydrophobic functional filler will be easily destroyed, which in turn affects the durability and cannot achieve the long-term super-hydrophobic effect. Summary of the invention

[0003] In view of the problems existing in the prior art, the purpose of the present invention is to provide a water-resistant corrugated packaging material. The present invention first uses an aminosilane coupling agent to treat nano-scale silica to modify the amino group, uses an epoxysilane coupling agent to treat micron-scale silica to modify the epoxy group, and then through the action of the amino group and the epoxy group, the surface of the micron-scale silica is composited with nano-scale silica to form a micro-nano structure, and then dopamine hydrochloride is used to self-polymerize and wrap it under aerobic and alkaline conditions to provide a secondary modification platform, and finally a silaneoxy hydrophobic modifier is added to make the micro-nano structure have low surface energy through the action of silaneoxy and hydroxyl groups, thereby preparing a modified filler, and when the coating obtained after mixing with other components is applied to the coating of corrugated boxes, it not only gives the surface of the corrugated boxes super-hydrophobic properties, but also has excellent durability.

[0004] The purpose of the present invention can be achieved through the following technical solutions:

[0005] A method for preparing a water-resistant corrugated packaging material, the method comprising the following steps:

[0006] (1) The coating is applied on the surface of the corrugated box, dried, and a coating is formed, and the preparation is completed.

[0007] As a preferred technical solution of the present invention, the coating in step (1) is prepared from 75-80 parts by weight of epoxy resin, 18-20 parts by weight of curing agent, 4-5 parts by weight of modified filler and 0.5-1 parts by weight of film-forming aid.

[0008] Furthermore, the epoxy resin is directly purchased from the market.

[0009] Furthermore, the curing agent is at least one of diethylenetriamine and triethylenetetramine.

[0010] Furthermore, the modified filler is prepared by the following steps:

[0011] Step a: adding 5-7 parts by weight of nano-scale silica, 0.5-1 parts by weight of deionized water and 0.3-0.5 parts by weight of an aminosilane coupling agent to 80-100 parts by weight of anhydrous ethanol, stirring at 65-70° C. for 23-25 ​​hours, filtering, removing the filtrate, washing with anhydrous ethanol, and finally vacuum drying at 50-60° C. until constant weight, to obtain amino-modified nano-scale silica;

[0012] Step b: adding 5-7 parts by weight of micron-sized silica, 0.5-1 parts by weight of deionized water and 0.3-0.5 parts by weight of epoxy silane coupling agent to 80-100 parts by weight of anhydrous ethanol, stirring at 65-70° C. for 23-25 ​​hours, filtering, removing the filtrate, washing with anhydrous ethanol, and finally vacuum drying at 50-60° C. until constant weight, to obtain epoxylated micron-sized silica;

[0013] Step c: adding 5-7 parts by weight of amino-modified nano-scale silica to 80-100 parts by weight of anhydrous ethanol, stirring and mixing at room temperature for 5-10 minutes to obtain dispersion a; adding 10-12 parts by weight of epoxy-modified micron-scale silica to 140-150 parts by weight of anhydrous ethanol, stirring and mixing at room temperature for 5-10 minutes to obtain dispersion b; adding dispersion a dropwise to dispersion b at 30-40° C. while stirring, continuing to stir at a constant temperature for 2-3 hours after the addition is completed, filtering, removing the filtrate, washing with anhydrous ethanol, and finally vacuum drying at 50-60° C. until constant weight is obtained to obtain composite micro-nano-scale silica;

[0014] Step d: adding 3-5 parts by weight of composite micro-nano silica and 5-6 parts by weight of dopamine hydrochloride to 100-120 parts by weight of Tris-HCl buffer, stirring at 25-30° C. for 12-14 hours in contact with air, filtering, removing the filtrate, washing with deionized water, and finally vacuum drying at 50-60° C. until constant weight, to obtain organically coated micro-nano silica;

[0015] Step e: add 5-7 parts by weight of organically coated micro-nano silica to 80-100 parts by weight of deionized water, stir for 5-10 minutes at room temperature to mix, then add 0.5-1 parts by weight of siloxy hydrophobic modifier dropwise while stirring at 70-80°C, continue stirring at constant temperature for 10-12 hours after the addition is completed, filter, remove the filtrate, wash with deionized water, and finally vacuum dry at 50-60°C until constant weight, and the preparation is completed.

[0016] Preferably, the particle size of the nano-scale silicon dioxide in step a is 10-30 nm.

[0017] Preferably, the aminosilane coupling agent in step a is at least one of γ-aminopropyltrimethoxysilane and γ-aminopropyltriethoxysilane.

[0018] Preferably, the particle size of the micron-sized silicon dioxide in step b is 0.15-0.2 μm.

[0019] Preferably, the epoxysilane coupling agent in step b is at least one of 3-(2,3-epoxypropoxy)propyltrimethoxysilane and 3-[(2,3)-epoxypropoxy]propylmethyldimethoxysilane.

[0020] Preferably, the dripping rate in step c is controlled at 1-3 drops / s.

[0021] Preferably, the pH of the Tris-HCl buffer in step d is 8-8.5.

[0022] Preferably, the dripping rate in step e is controlled at 1 drop / s.

[0023] Preferably, the silaneoxy hydrophobic modifier in step e is at least one of dodecyltrimethoxysilane, dodecyltriethoxysilane and hexadecyltrimethoxysilane.

[0024] Furthermore, the film-forming aid is dodecyl alcohol ester.

[0025] As a preferred technical solution of the present invention, the coating in step (1) is prepared by the following steps:

[0026] Step X: Add curing agent, modified filler and film-forming aid to epoxy resin, then stir and mix at a speed of 1500-2000 r / min at room temperature for 5-10 minutes, and finally vacuum degas for 5 minutes to complete the preparation.

[0027] As a preferred technical solution of the present invention, the drying in step (1) refers to drying at 50° C. for 7-8 hours.

[0028] As a preferred technical solution of the present invention, the forming of a coating in step (1) refers to forming a coating with a thickness of 0.1-0.2 mm.

[0029] A water-resistant corrugated packaging material prepared by the preparation method as described above.

[0030] Beneficial effects of the present invention:

[0031] (1) The present invention first uses an aminosilane coupling agent to treat nano-scale silica to modify the amino group, and uses an epoxysilane coupling agent to treat micron-scale silica to modify the epoxy group. Then, through the action of the amino group and the epoxy group, the surface of the micron-scale silica is composited with nano-scale silica to form a micro-nano structure. Then, dopamine hydrochloride is used to self-polymerize and wrap it under aerobic and alkaline conditions to provide a secondary modification platform. Finally, a silaneoxy hydrophobic modifier is added to make the micro-nano structure have a low surface energy through the action of the silaneoxy and hydroxyl groups, thereby preparing a modified filler. When the coating obtained by mixing the filler with other components is applied to the coating of corrugated boxes, it not only gives the surface of the corrugated boxes super-hydrophobic properties, but also has excellent durability.

[0032] (2) The present invention creatively combines nano-scale silica and micron-scale silica through the action of chemical bonds to construct a very stable micro-nano structure, and then uses dopamine hydrochloride to self-polymerize and encapsulate the micro-nano structure under aerobic and alkaline conditions. After encapsulation, on the one hand, a secondary modification platform can be provided. Polydopamine is a substance containing a large number of hydroxyl groups and amino groups. Its hydroxyl groups can react with the silaneoxy groups of the silaneoxy hydrophobic modifier, thereby giving the micro-nano structure a low surface energy, while its amino groups can participate in the curing in the epoxy resin-amine system, thereby bonding the micro-nano structure to the epoxy resin in the form of a chemical bond. In actual use, the wear and damage of the micro-nano structure caused by the action of external forces can be effectively reduced. On the other hand, it also transforms from an organic phase-inorganic phase to an organic phase-organic phase. The epoxy resin has good compatibility and strong dispersibility with the modified filler, which can better exert the wear-resistant effect of silica itself, further reduce the wear and damage that may occur to the micro-nano structure, and thus ensure the durability and long-term effect of the super hydrophobic property.

[0033] (3) The surface of the corrugated packaging material provided by the present invention has a super-hydrophobic property, excellent water resistance and strong practicality. DETAILED DESCRIPTION

[0034] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.

[0035] The corrugated paper boxes in all the embodiments and comparative examples of the present invention are from Zhengye Packaging (Zhongshan) Co., Ltd., and the corrugated paper boxes are made of E-type corrugated paperboard, and the basis weight of the E-type corrugated paperboard is 445g / m 2 ; All epoxy resins were purchased directly from the market, the manufacturer was American Hanson, model number was Epikote 6520-WH-53A.

[0036] Example 1

[0037] A method for preparing a water-resistant corrugated packaging material, the method comprising the following steps:

[0038] (1) The coating is applied on the surface of the corrugated box, dried, and a coating is formed, and the preparation is completed.

[0039] The coating in step (1) is prepared from 75 parts by weight of epoxy resin, 18 parts by weight of curing agent, 4 parts by weight of modified filler and 0.5 parts by weight of film-forming aid.

[0040] The epoxy resin is directly purchased from the market.

[0041] The curing agent is diethylenetriamine.

[0042] The modified filler is prepared by the following steps:

[0043] Step a: adding 5 parts by weight of nano-scale silica, 0.5 parts by weight of deionized water and 0.3 parts by weight of an aminosilane coupling agent to 80 parts by weight of anhydrous ethanol, stirring at 65° C. for 23 hours, filtering, removing the filtrate, washing with anhydrous ethanol, and finally vacuum drying at 50° C. until constant weight, to obtain amino-modified nano-scale silica;

[0044] Step b: adding 5 parts by weight of micron-sized silica, 0.5 parts by weight of deionized water and 0.3 parts by weight of epoxy silane coupling agent to 80 parts by weight of anhydrous ethanol, stirring at 65° C. for 23 hours, filtering, removing the filtrate, washing with anhydrous ethanol, and finally vacuum drying at 50° C. until constant weight, to obtain epoxylated micron-sized silica;

[0045] Step c: adding 5 parts by weight of amino-modified nano-scale silica to 80 parts by weight of anhydrous ethanol, stirring and mixing at room temperature for 5 minutes to obtain dispersion a; adding 10 parts by weight of epoxy-modified micron-scale silica to 140 parts by weight of anhydrous ethanol, stirring and mixing at room temperature for 5 minutes to obtain dispersion b; adding dispersion a dropwise to dispersion b at 30° C. while stirring, continuing to stir at a constant temperature for 2 hours after the addition is completed, filtering, removing the filtrate, washing with anhydrous ethanol, and finally vacuum drying at 50° C. until constant weight, to obtain composite micro-nano-scale silica;

[0046] Step d: adding 3 parts by weight of composite micro-nano silica and 5 parts by weight of dopamine hydrochloride to 100 parts by weight of Tris-HCl buffer, stirring at 25° C. for 12 hours in contact with air, filtering, removing the filtrate, washing with deionized water, and finally vacuum drying at 50° C. until constant weight, to obtain organically coated micro-nano silica;

[0047] Step e: Add 5 parts by weight of organically coated micro-nano silica to 80 parts by weight of deionized water, stir at room temperature for 5 minutes to mix, then add 0.5 parts by weight of siloxy hydrophobic modifier dropwise while stirring at 70°C, continue stirring at constant temperature for 10 hours after the addition is completed, filter, remove the filtrate, wash with deionized water, and finally vacuum dry at 50°C until constant weight, and the preparation is completed.

[0048] The particle size of the nano-scale silicon dioxide in step a is 10 nm.

[0049] The aminosilane coupling agent in step a is γ-aminopropyltrimethoxysilane.

[0050] The particle size of the micron-sized silicon dioxide in step b is 0.15 μm.

[0051] The epoxysilane coupling agent in step b is 3-(2,3-epoxypropoxy)propyltrimethoxysilane.

[0052] The dripping rate of step c is controlled at 1 drop / s.

[0053] The pH of the Tris-HCl buffer in step d is 8.

[0054] The dripping rate in step e is controlled at 1 drop / s.

[0055] The silaneoxy hydrophobic modifier in step e is dodecyltrimethoxysilane.

[0056] The film-forming aid is dodecyl alcohol ester.

[0057] The coating of step (1) is prepared by the following steps:

[0058] Step X: Add curing agent, modified filler and film-forming aid to epoxy resin, then stir and mix at a speed of 1500 r / min at room temperature for 5 minutes, and finally vacuum degas for 5 minutes to complete the preparation.

[0059] The drying in step (1) refers to drying at 50° C. for 7 hours.

[0060] The forming of a coating in step (1) refers to forming a coating with a thickness of 0.1 mm.

[0061] A water-resistant corrugated packaging material prepared by the preparation method as described above.

[0062] Example 2

[0063] A method for preparing a water-resistant corrugated packaging material, the method comprising the following steps:

[0064] (1) The coating is applied on the surface of the corrugated box, dried, and a coating is formed, and the preparation is completed.

[0065] The coating in step (1) is prepared from 80 parts by weight of epoxy resin, 20 parts by weight of curing agent, 5 parts by weight of modified filler and 1 part by weight of film-forming aid.

[0066] The epoxy resin is directly purchased from the market.

[0067] The curing agent is diethylenetriamine.

[0068] The modified filler is prepared by the following steps:

[0069] Step a: adding 7 parts by weight of nano-scale silica, 1 part by weight of deionized water and 0.5 parts by weight of an aminosilane coupling agent to 100 parts by weight of anhydrous ethanol, stirring at 70° C. for 25 hours, filtering, removing the filtrate, washing with anhydrous ethanol, and finally vacuum drying at 60° C. until constant weight, to obtain amino-modified nano-scale silica;

[0070] Step b: adding 7 parts by weight of micron-sized silica, 1 part by weight of deionized water and 0.5 parts by weight of epoxy silane coupling agent to 100 parts by weight of anhydrous ethanol, stirring at 70° C. for 25 hours, filtering, removing the filtrate, washing with anhydrous ethanol, and finally vacuum drying at 60° C. until constant weight, to obtain epoxylated micron-sized silica;

[0071] Step c: adding 7 parts by weight of amino-modified nano-scale silica to 100 parts by weight of anhydrous ethanol, stirring and mixing at room temperature for 10 minutes to obtain dispersion a; adding 12 parts by weight of epoxy-modified micron-scale silica to 150 parts by weight of anhydrous ethanol, stirring and mixing at room temperature for 10 minutes to obtain dispersion b; adding dispersion a dropwise to dispersion b at 40° C. while stirring, continuing to stir at a constant temperature for 3 hours after the addition is completed, filtering, removing the filtrate, washing with anhydrous ethanol, and finally vacuum drying at 60° C. until constant weight, to obtain composite micro-nano-scale silica;

[0072] Step d: adding 5 parts by weight of composite micro-nano silica and 6 parts by weight of dopamine hydrochloride to 120 parts by weight of Tris-HCl buffer, stirring at 30° C. for 14 hours in contact with air, filtering, removing the filtrate, washing with deionized water, and finally vacuum drying at 60° C. until constant weight, to obtain organically coated micro-nano silica;

[0073] Step e: Add 7 parts by weight of organically coated micro-nano silica to 100 parts by weight of deionized water, stir at room temperature for 10 minutes to mix, then add 1 part by weight of siloxy hydrophobic modifier dropwise while stirring at 80°C, continue stirring at constant temperature for 12 hours after the addition is completed, filter, remove the filtrate, wash with deionized water, and finally vacuum dry at 60°C until constant weight, and the preparation is completed.

[0074] The particle size of the nano-scale silicon dioxide in step a is 30 nm.

[0075] The aminosilane coupling agent in step a is γ-aminopropyltrimethoxysilane.

[0076] The particle size of the micron-sized silicon dioxide in step b is 0.2 μm.

[0077] The epoxysilane coupling agent in step b is 3-(2,3-epoxypropoxy)propyltrimethoxysilane.

[0078] The dripping rate of step c is controlled at 3 drops / s.

[0079] The pH of the Tris-HCl buffer in step d is 8.5.

[0080] The dripping rate in step e is controlled at 1 drop / s.

[0081] The silaneoxy hydrophobic modifier in step e is dodecyltrimethoxysilane.

[0082] The film-forming aid is dodecyl alcohol ester.

[0083] The coating of step (1) is prepared by the following steps:

[0084] Step X: Add curing agent, modified filler and film-forming aid to epoxy resin, then stir and mix at a speed of 2000 r / min at room temperature for 10 minutes, and finally vacuum degas for 5 minutes to complete the preparation.

[0085] The drying in step (1) refers to drying at 50° C. for 8 hours.

[0086] The forming of a coating in step (1) refers to forming a coating with a thickness of 0.2 mm.

[0087] A water-resistant corrugated packaging material prepared by the preparation method as described above.

[0088] Example 3

[0089] A method for preparing a water-resistant corrugated packaging material, the method comprising the following steps:

[0090] (1) The coating is applied on the surface of the corrugated box, dried, and a coating is formed, and the preparation is completed.

[0091] The coating in step (1) is prepared from 78 parts by weight of epoxy resin, 19 parts by weight of curing agent, 4.5 parts by weight of modified filler and 0.8 parts by weight of film-forming aid.

[0092] The epoxy resin is directly purchased from the market.

[0093] The curing agent is diethylenetriamine.

[0094] The modified filler is prepared by the following steps:

[0095] Step a: adding 6 parts by weight of nano-scale silica, 0.8 parts by weight of deionized water and 0.4 parts by weight of an aminosilane coupling agent to 90 parts by weight of anhydrous ethanol, stirring at 68° C. for 24 hours, filtering, removing the filtrate, washing with anhydrous ethanol, and finally vacuum drying at 55° C. until constant weight, to obtain amino-modified nano-scale silica;

[0096] Step b: adding 6 parts by weight of micron-sized silica, 0.8 parts by weight of deionized water and 0.4 parts by weight of epoxy silane coupling agent to 90 parts by weight of anhydrous ethanol, stirring at 68° C. for 24 hours, filtering, removing the filtrate, washing with anhydrous ethanol, and finally vacuum drying at 55° C. until constant weight, to obtain epoxylated micron-sized silica;

[0097] Step c: adding 6 parts by weight of amino-modified nano-scale silica to 90 parts by weight of anhydrous ethanol, stirring and mixing at room temperature for 8 minutes to obtain dispersion a; adding 11 parts by weight of epoxy-modified micron-scale silica to 145 parts by weight of anhydrous ethanol, stirring and mixing at room temperature for 8 minutes to obtain dispersion b; adding dispersion a dropwise to dispersion b at 35° C. while stirring, continuing to stir at a constant temperature for 2.5 hours after the addition is completed, filtering, removing the filtrate, washing with anhydrous ethanol, and finally vacuum drying at 55° C. until constant weight, to obtain composite micro-nano-scale silica;

[0098] Step d: adding 4 parts by weight of composite micro-nano silica and 5.5 parts by weight of dopamine hydrochloride to 110 parts by weight of Tris-HCl buffer, stirring at 28° C. for 13 hours in contact with air, filtering, removing the filtrate, washing with deionized water, and finally vacuum drying at 55° C. until constant weight, to obtain organic-coated micro-nano silica;

[0099] Step e: Add 6 parts by weight of organically coated micro-nano silica to 90 parts by weight of deionized water, stir at room temperature for 8 minutes to mix, then add 0.8 parts by weight of siloxy hydrophobic modifier dropwise while stirring at 75°C, continue stirring at constant temperature for 11 hours after the addition is completed, filter, remove the filtrate, wash with deionized water, and finally vacuum dry at 55°C until constant weight, and the preparation is completed.

[0100] The particle size of the nano-scale silicon dioxide in step a is 20 nm.

[0101] The aminosilane coupling agent in step a is γ-aminopropyltrimethoxysilane.

[0102] The particle size of the micron-sized silicon dioxide in step b is 0.18 μm.

[0103] The epoxysilane coupling agent in step b is 3-(2,3-epoxypropoxy)propyltrimethoxysilane.

[0104] The dripping rate of step c is controlled at 2 drops / s.

[0105] The pH of the Tris-HCl buffer in step d is 8.3.

[0106] The dripping rate in step e is controlled at 1 drop / s.

[0107] The silaneoxy hydrophobic modifier in step e is dodecyltrimethoxysilane.

[0108] The film-forming aid is dodecyl alcohol ester.

[0109] The coating of step (1) is prepared by the following steps:

[0110] Step X: Add curing agent, modified filler and film-forming aid to epoxy resin, then stir and mix at a speed of 1800 r / min at room temperature for 8 minutes, and finally vacuum degas for 5 minutes to complete the preparation.

[0111] The drying in step (1) refers to drying at 50° C. for 7.5 hours.

[0112] The forming of a coating in step (1) refers to forming a coating with a thickness of 0.15 mm.

[0113] A water-resistant corrugated packaging material prepared by the preparation method as described above.

[0114] Comparative Example 1

[0115] On the basis of Example 1, the aminosilane coupling agent in step a was replaced by an equal weight of deionized water, and the epoxysilane coupling agent in step b was replaced by an equal weight of deionized water, and the rest remained unchanged.

[0116] Comparative Example 2

[0117] Based on Example 1, the siloxy hydrophobic modifier in step e was replaced by an equal weight of deionized water, and the rest remained unchanged.

[0118] Comparative Example 3

[0119] On the basis of Example 1, step e is not performed, and step d is changed to adding 5 parts by weight of composite micro-nano silica, 0.5 parts by weight of deionized water, 0.3 parts by weight of dodecyltrimethoxysilane and 0.3 parts by weight of γ-aminopropyltrimethoxysilane to 100 parts by weight of anhydrous ethanol, and then stirring at 70°C for 23 hours, filtering, removing the filtrate, washing with anhydrous ethanol, and finally vacuum drying at 50°C until constant weight, that is, the preparation is completed; the rest remains unchanged.

[0120] Comparative Example 4

[0121] On the basis of Example 1, step e is changed to adding 5 parts by weight of organic-coated micro-nano silica to 80 parts by weight of deionized water, stirring for 5 minutes at room temperature, and then adding 0.5 parts by weight of siloxy hydrophobic modifier dropwise while stirring at 70°C, and continuing to stir at a constant temperature for 10 hours after the addition is completed, filtering, removing the filtrate, washing with deionized water, and finally vacuum drying at 50°C until constant weight to obtain a material; adding 100 parts by weight of anhydrous ethanol and 5 parts by weight of 1,2-epoxyhexane to the material, and then stirring at 40°C for 12 hours, filtering, removing the filtrate, washing with anhydrous ethanol, and finally vacuum drying at 50°C until constant weight, that is, the preparation is completed; the rest remains unchanged.

[0122] Test Example 1

[0123] Water resistance test:

[0124] The static contact angle and rolling contact angle of the water-resistant corrugated packaging materials prepared in Examples 1-3 and Comparative Examples 1-4 were tested respectively.

[0125] Table 1. Water resistance test results

[0126] Static contact angle / degree Rolling contact angle / degree Example 1 157.4 7.3 Example 2 159.6 6.8 Example 3 159.5 7.0 Comparative Example 1 141.8 23.5 Comparative Example 2 105.2 64.9 Comparative Example 3 157.0 7.2 Comparative Example 4 157.9 7.2

[0127] Test Example 2

[0128] Durability test:

[0129] Sandpaper with a mesh size of 600 was placed on the surface of the water-resistant corrugated packaging materials prepared in Examples 1-3 and Comparative Examples 1-4, respectively. The sandpaper was then dragged 10 times under the pressure of a 400 g weight, with each dragging distance being 20 cm. Finally, the static contact angle and rolling contact angle after dragging were retested.

[0130] Table 2. Durability test results

[0131]

[0132]

[0133] Comparison between Example 1 and Comparative Examples 1-4 shows that:

[0134] The difference between Comparative Example 1 and Example 1 is that no nano-scale silicon dioxide is compounded on the surface of the micro-scale silicon dioxide.

[0135] The difference between Comparative Example 2 and Example 1 is that no silaneoxy hydrophobic modifier is added to form low surface energy for the micro-nano structure.

[0136] The difference between Comparative Example 3 and Example 1 is that the micro-nano structure is not self-polymerized and encapsulated with dopamine hydrochloride, but the amino groups are still modified and the low surface energy is formed.

[0137] The difference between Comparative Example 4 and Example 1 is that 1,2-epoxyhexane is added to consume the surface amino groups of the modified filler.

[0138] From the comparison between Example 1 and Comparative Examples 1-4 in Test Example 1, it can be seen that the water-resistant corrugated packaging material prepared by the present invention has super hydrophobic properties and excellent water resistance.

[0139] From the comparison between Example 1 and Comparative Examples 1-4 in Test Example 2, it can be seen that the water-resistant corrugated packaging material prepared by the present invention has excellent super-hydrophobic durability. Even after friction and wear, its static contact angle still decreases very little, and still exhibits super-hydrophobic properties.

[0140] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A method for preparing a water-resistant corrugated packaging material, characterized in that: The preparation method comprises the following steps: (1) Applying a coating on the surface of the corrugated box and drying it to form a coating, the preparation is completed; The coating in step (1) is prepared from 75-80 parts by weight of epoxy resin, 18-20 parts by weight of curing agent, 4-5 parts by weight of modified filler and 0.5-1 parts by weight of film-forming aid.

2. The method for preparing a water-resistant corrugated packaging material according to claim 1, characterized in that: The curing agent is at least one of diethylenetriamine and triethylenetetramine.

3. The method for preparing a water-resistant corrugated packaging material according to claim 1, characterized in that: The modified filler is prepared by the following steps: Step a: adding 5-7 parts by weight of nano-scale silica, 0.5-1 parts by weight of deionized water and 0.3-0.5 parts by weight of an aminosilane coupling agent to 80-100 parts by weight of anhydrous ethanol, stirring at 65-70° C. for 23-25 ​​hours, filtering, removing the filtrate, washing with anhydrous ethanol, and finally vacuum drying at 50-60° C. until constant weight, to obtain amino-modified nano-scale silica; Step b: adding 5-7 parts by weight of micron-sized silica, 0.5-1 parts by weight of deionized water and 0.3-0.5 parts by weight of epoxy silane coupling agent to 80-100 parts by weight of anhydrous ethanol, stirring at 65-70° C. for 23-25 ​​hours, filtering, removing the filtrate, washing with anhydrous ethanol, and finally vacuum drying at 50-60° C. until constant weight, to obtain epoxylated micron-sized silica; Step c: adding 5-7 parts by weight of amino-modified nano-scale silica to 80-100 parts by weight of anhydrous ethanol, stirring and mixing at room temperature for 5-10 minutes to obtain dispersion a; adding 10-12 parts by weight of epoxy-modified micron-scale silica to 140-150 parts by weight of anhydrous ethanol, stirring and mixing at room temperature for 5-10 minutes to obtain dispersion b; adding dispersion a dropwise to dispersion b at 30-40° C. while stirring, continuing to stir at a constant temperature for 2-3 hours after the addition is completed, filtering, removing the filtrate, washing with anhydrous ethanol, and finally vacuum drying at 50-60° C. until constant weight is obtained to obtain composite micro-nano-scale silica; Step d: adding 3-5 parts by weight of composite micro-nano silica and 5-6 parts by weight of dopamine hydrochloride to 100-120 parts by weight of Tris-HCl buffer, stirring at 25-30° C. for 12-14 hours in contact with air, filtering, removing the filtrate, washing with deionized water, and finally vacuum drying at 50-60° C. until constant weight, to obtain organically coated micro-nano silica; Step e: add 5-7 parts by weight of organically coated micro-nano silica to 80-100 parts by weight of deionized water, stir for 5-10 minutes at room temperature to mix, then add 0.5-1 parts by weight of siloxy hydrophobic modifier dropwise while stirring at 70-80°C, continue stirring at constant temperature for 10-12 hours after the addition is completed, filter, remove the filtrate, wash with deionized water, and finally vacuum dry at 50-60°C until constant weight, and the preparation is completed.

4. The method for preparing a water-resistant corrugated packaging material according to claim 3, characterized in that: The aminosilane coupling agent in step a is at least one of γ-aminopropyltrimethoxysilane and γ-aminopropyltriethoxysilane.

5. The method for preparing a water-resistant corrugated packaging material according to claim 3, characterized in that: In step b, the epoxysilane coupling agent is at least one of 3-(2,3-epoxypropoxy)propyltrimethoxysilane and 3-[(2,3)-epoxypropoxy]propylmethyldimethoxysilane.

6. The method for preparing a water-resistant corrugated packaging material according to claim 3, characterized in that: In step e, the silaneoxy hydrophobic modifier is at least one of dodecyltrimethoxysilane, dodecyltriethoxysilane and hexadecyltrimethoxysilane.

7. The method for preparing a water-resistant corrugated packaging material according to claim 1, characterized in that: The drying in step (1) refers to drying at 50° C. for 7-8 hours.

8. The method for preparing a water-resistant corrugated packaging material according to claim 1, characterized in that: The forming of a coating in step (1) refers to forming a coating with a thickness of 0.1-0.2 mm.

9. A water-resistant corrugated packaging material prepared by the preparation method according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Tensioning ground and rock anchoring bolt

    EP0006520A1

  • Nano-coated waterproof and anti-fouling corrugated carton

    CN106882468A

  • Preparation method of persistent icing-resistant superhydrophobic coating

    CN106883650A

  • Super-hydrophobic nano SiO2 modified epoxy acrylic resin coating and preparation method thereof

    CN111410887A

  • Micro-nano composite SiO2 particles, micro-nano composite structure super-hydrophobic coating layer and preparation methods and applications of micro-nano composite SiO2 particles and micro-nano composite structure super-hydrophobic coating layer

    CN113088123A