MXene / CNT composite film self-energized linear pressure sensor and preparation method thereof
Through the preparation of MXene/CNT composite membrane self-energy linear pressure sensor, the problem of nonlinearity and dependence on external power supply of traditional pressure sensors is solved, and a high-precision, environmentally friendly and widely used self-energy pressure sensor is realized, with fast response and low energy consumption characteristics .
Patent Information
- Application Number
- CN202410965466.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
AI Technical Summary
Existing pressure sensors cannot achieve self-energy and their transfer function is nonlinear, resulting in inaccurate measurement results, and traditional linear pressure sensors rely on external power supplies, limiting their use range and increasing maintenance costs and environmental burdens.
The preparation method of the MXene/CNT composite film self-energized linear pressure sensor is adopted. The composite film is prepared by mixing the MXene solution with the CNT solution to form a sandwich structure film, and the electrolyte is filled in the silicon rubber cavity, and self-supply is achieved by using the Ag/AgCl electrode. It can ensure that the sensor output signal is linearly related to the pressure change.
High-precision pressure measurement is achieved, eliminating dependence on traditional power supplies, reducing energy consumption and carbon emissions, extending application range, and improving response speed and linearity.
Smart Images

Figure CN118913485A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of sensors and relates to a self-powered linear pressure sensor and a preparation method thereof, and specifically refers to a MXene / CNT composite film self-powered linear pressure sensor and a preparation method thereof. Background Art
[0002] At present, the booming development of artificial intelligence and the Internet of Things highlights the importance of manufacturing portable electronic devices to realize human-machine interface. As one of the most important electronic devices, pressure sensors play a vital role in signal acquisition. Patent CN116045795A discloses a CNT / MXene nanofiltration film sensor and a preparation method. The prepared CNT / MXene nanofilm sensor can monitor health in real time. However, the sensor cannot achieve self-power supply and the linearity is not ideal. The output signal of the existing pressure sensor is generally nonlinear with the measured pressure, that is, its transfer function has different sensitivities in different detection ranges, resulting in inaccurate measurement results. Generally speaking, a linear transfer function can improve the accuracy of the sensor. A linear pressure sensor is a device that measures pressure changes and converts them into a linear output signal. However, traditional linear pressure sensors usually rely on external power supplies or batteries, which not only limits their scope of use, but also increases maintenance costs and environmental burdens. In order to solve the power supply problem brought about by the rapid development of portable sensors and the Internet of Things, self-powered sensors have been developed. The key to self-powered pressure sensors is to achieve the conversion of mechanical energy to electrical energy, but this is also affected by the problem of nonlinear transfer functions. By utilizing the ion selectivity of the membrane under pressure, a linear relationship between the sensor output signal and the measured pressure can be basically achieved. In addition, the fast response time of pressure also plays an important role in practical applications. Summary of the invention
[0003] In order to solve the above technical problems, the present invention proposes a MXene / CNT composite film self-powered linear pressure sensor and a preparation method thereof. The sensor preparation process is very simple and energy-saving and environmentally friendly, and it has a high accuracy while achieving self-power.
[0004] To achieve the above object, the technical solution of the present invention is implemented as follows:
[0005] A method for preparing a MXene / CNT composite film self-powered linear pressure sensor, the steps are as follows:
[0006] (1) After mixing the MXene solution with the CNT solution, a MXene / CNT composite membrane was prepared by vacuum-assisted filtration;
[0007] (2) placing two polytetrafluoroethylene films with reserved holes on both sides of the MXene / CNT composite film to form a sandwich structure film;
[0008] (3) The sandwich structure film is fixed in two silicone rubber cavities, and the outer side of the silicone rubber cavity is sealed by a flexible film;
[0009] (4) filling the silicone rubber cavity with electrolyte;
[0010] (5) The Ag / AgCl electrode connected to the external circuit was inserted into the silicone rubber cavity to prepare the MXene / CNT composite membrane self-powered linear pressure sensor.
[0011] The MXene solution in the above step (1) refers to the one obtained by selectively etching the precursor MAX phase with HCl and LiF, wherein M is a transition metal, A is mainly a group III element or a group IV element, and X is any one or a combination of two of the C and N elements.
[0012] In the above step (1), the proportion of CNT in the MXene / CNT composite film is 3-9wt%.
[0013] In the above step (3), silicone rubber sealing can be used at the interface of the two silicone rubber cavities.
[0014] Furthermore, in the above step (3), V-705 silicone rubber can be used to seal the interface between the two silicone rubber cavities.
[0015] In the above step (4), the electrolyte is sodium chloride, potassium chloride or magnesium chloride solution.
[0016] In the above step (4), the concentration of the electrolyte is 0.01-0.5M.
[0017] Furthermore, in the above step (4), the concentration of the electrolyte is 0.01-0.3M.
[0018] In step (4), the electrolyte may be filled via a syringe.
[0019] In the above step (5), the Ag / AgCl electrode can be inserted into the silicone rubber cavity through the micropores formed by the syringe, and the gap between the Ag / AgCl electrode and the micropores is sealed.
[0020] In the above step (5), the Ag / AgCl electrode is only placed in the electrolyte and is not in direct contact with the MXene / CNT composite film.
[0021] The MXene / CNT composite film self-powered linear pressure sensor prepared by the above preparation method.
[0022] The MXene / CNT composite membrane self-powered linear pressure sensor comprises a MXene / CNT composite membrane (ion selective membrane), an electrolyte, a polytetrafluoroethylene film, a silicone rubber cavity, a flexible packaging film and an Ag / AgCl electrode. The MXene / CNT composite membrane (ion selective membrane) is provided with polytetrafluoroethylene films with reserved holes on both sides to form a sandwich structure film; silicone rubber cavities are provided outside the polytetrafluoroethylene film, and the silicone rubber cavities are filled with electrolyte for infiltrating the MXene / CNT composite membrane (ion selective membrane) and providing ions; the flexible film is provided outside the silicone rubber cavity to seal the MXene / CNT composite membrane (ion selective membrane), the electrolyte, the polytetrafluoroethylene film and the two silicone rubber cavities in the flexible film; the Ag / AgCl electrode is inserted into the electrolyte in the silicone rubber cavity, which is connected to an external circuit and does not directly contact the MXene / CNT composite membrane (ion selective membrane).
[0023] Since the surface of the MXene / CNT composite membrane is electronegative, it will attract cations in the electrolyte to adhere to the surface. When external pressure is applied, the cations will pass through the composite membrane to form an electrical signal, realizing the conversion of pressure-electrical signal, thereby realizing the self-power supply of the sensor. In addition, by adjusting the ratio of MXene / CNT, the interlayer spacing of the MXene / CNT composite membrane can be regulated, thereby improving the conversion efficiency of pressure-electrical signal (such as output voltage, output current and response time, etc.), and a MXene / CNT composite membrane that is more suitable for cation transmission can be obtained.
[0024] The voltage-pressure linearity of the pressure sensor is 0.999, and the current-pressure linearity is 0.990.
[0025] When the pressure is 6.3 kPa, the current response time is 51.3 ms, and when the pressure is 3.3 kPa, the voltage response time is 70.9 ms.
[0026] The beneficial effects produced by the present invention are:
[0027] (1) The MXene used in the present invention is a member of the two-dimensional material family, and has the characteristics of good flexibility, high mechanical strength, hydrophilic surface, end groups rich in negative charges, and changeable surface charges. The MXene film has a large number of nanochannels with adjustable channel spacing, but its easy stacking property hinders ion diffusion. One-dimensional CNT has excellent mechanical properties, electrical properties, thermal conductivity and chemical stability. By combining MXene with CNT, the characteristics of adjustable interlayer spacing, excellent mechanical properties, and good ion selectivity can be achieved.
[0028] (2) The sensor of the present invention can provide high-precision pressure measurement, and the output signal is linearly related to the pressure change. The relationship between the voltage corresponding to the pressure-converted electrical energy and the corresponding pressure is: Where ε is the dielectric constant of the electrolyte solution, η is the viscosity of the electrolyte solution, is the surface potential of the nanochannel, A is the channel cross-sectional area, and L is the length of the nanochannel. Generally speaking, for a given electrolyte solution and composite membrane, these parameters are constants. Therefore, the corresponding pressure difference value Δp can be obtained from the current I generated by the test, and there is a linear relationship between the two, which enables the sensor to accurately reflect the change of pressure and provide reliable data support for various applications. Due to the high hydrophilicity and surface negative potential of the MXene / CNT composite membrane surface, this sensor has an extremely fast reaction speed. When stimulated by external pressure (pressure of 6.3kPa), the response time of the current can be as low as 51.3ms, and the recovery time is 60.2ms. And when the proportion of CNT in the MXene / CNT composite membrane is 6wt%, the linearity of input pressure-output voltage is 0.999, and the linearity of input pressure-output current is 0.990, which has a good linear relationship and is conducive to high-precision measurement of pressure.
[0029] (3) The sensor of the present invention eliminates the dependence on traditional power supply, so that the sensor can perform long-term stable measurement in places without power supply, especially in remote areas or places where it is difficult to provide stable power supply, which greatly expands its application range. It also reduces the dependence on traditional energy, reduces energy consumption and carbon emissions, and conforms to the development trend of energy conservation and environmental protection. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0031] Figure 1 It is a schematic diagram of the process of preparing the self-powered linear pressure sensor based on MXene / CNT composite film in the present invention.
[0032] Figure 2 The precursor Ti3AlC2 used in the present invention and the prepared Ti3C2T X XRD pattern of .
[0033] Figure 3 This is the XRD pattern of the MXene / CNT composite film prepared in Examples 1-3 of the present invention.
[0034] Figure 4 This is a cross-sectional SEM image of the MXene / CNT composite film prepared in the present invention.
[0035] Figure 5 These are pictures of the mechanical properties of the MXene film and MXene / CNT film prepared in the present invention.
[0036] Figure 6 Zeta potential of MXene and MXene / CNT solutions prepared in the present invention.
[0037] Figure 7 VT diagrams of the self-powered linear pressure sensors prepared in Examples 1-3 of the present invention and the sensor prepared in Comparative Example 1.
[0038] Figure 8 IT diagram of the self-powered linear pressure sensor prepared in Example 2 of the present invention at different pressures.
[0039] Fig. 9 VT diagram of the self-powered linear pressure sensor prepared in Example 2 of the present invention at different pressures.
[0040] Fig.10 VP diagram of the self-powered linear pressure sensor prepared in Example 2 of the present invention.
[0041] Fig.11 This is the IP diagram of the self-powered linear pressure sensor prepared in Example 2 of the present invention.
[0042] Fig.12 Response and recovery time diagram of the self-powered linear pressure sensor 1 prepared in Example 2 of the present invention.
[0043] Fig.13 Response and recovery time diagram of the self-powered linear pressure sensor V prepared in Example 2 of the present invention. DETAILED DESCRIPTION
[0044] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0045] A method for preparing a MXene / CNT composite film self-powered linear pressure sensor, the steps are as follows:
[0046] (1) After mixing the MXene solution and the CNT solution, a MXene / CNT composite membrane was prepared by vacuum assisted filtration;
[0047] (2) placing two polytetrafluoroethylene films with reserved holes on both sides of the MXene / CNT composite film to form a sandwich structure film;
[0048] (3) The sandwich structure film is fixed in two silicone rubber cavities, and the outer side of the silicone rubber cavity is sealed by a flexible film;
[0049] (4) filling the silicone rubber cavity with electrolyte;
[0050] (5) The Ag / AgCl electrode connected to the external circuit was inserted into the silicone rubber cavity to prepare the MXene / CNT composite membrane self-powered linear pressure sensor.
[0051] The MXene solution in the above step (1) refers to the one obtained by selectively etching the precursor MAX phase with HCl and LiF, wherein M is a transition metal, A is mainly a group III element or a group IV element, and X is any one or a combination of two of the C and N elements.
[0052] In the above step (1), the proportion of CNT in the MXene / CNT composite film is 3-9wt%, for example: the proportion of CNT in the MXene / CNT composite film is 3wt%; the proportion of CNT in the MXene / CNT composite film is 6wt%; the proportion of CNT in the MXene / CNT composite film is 9wt%.
[0053] In the above step (4), the electrolyte is sodium chloride, potassium chloride or magnesium chloride solution.
[0054] In the above step (4), the electrolyte concentration is 0.01-0.5M, for example: the electrolyte concentration is 0.01-0.3M; the electrolyte concentration is 0.3-0.5M; the electrolyte concentration is 0.01M; the electrolyte concentration is 0.05M; the electrolyte concentration is 0.1M; the electrolyte concentration is 0.2M; the electrolyte concentration is 0.3M; the electrolyte concentration is 0.4M; the electrolyte concentration is 0.5M.
[0055] In the above step (5), the Ag / AgCl electrode is only placed in the electrolyte and is not in direct contact with the MXene / CNT composite film.
[0056] Example 1
[0057] The preparation method of the MXene / CNT composite film self-powered linear pressure sensor of this embodiment is shown in the flow chart. Figure 1 As shown, the steps are as follows:
[0058] (1) A MXene solution with a concentration of 6.63 mg / mL was obtained by selectively etching the precursor MAX phase with HCl and LiF. Specifically, 1.0 g of LiF powder and 1.0 g of Ti3AlC2 were weighed, and LiF and 20.0 mL of HCl (75 wt.%) were mixed, Ti3AlC2 (MAX phase) was slowly added to the mixed solution, and fully reacted for 24 h at 35 ° C by magnetic stirring. After the reaction was completed, the obtained acidic reactant was placed in a centrifuge tube, deionized water was added, and the centrifuge speed was set to 3500 rpm, and centrifuged for 3 min to obtain a precipitate. Deionized water was added again for a second centrifugal washing, and water molecules were inserted into the interlayer by hand shaking to increase the interlayer spacing of the product. The above process was repeated many times until the pH value of the reactant was neutral. Then, the precipitate was dispersed in a certain amount of deionized water, argon was continuously introduced under water bath conditions below 15 ° C, and ultrasonic peeling was performed for 1.0 h using an ultrasonic machine. Finally, the supernatant was collected by centrifugation at 3500 rpm for 1 h, which was a monolayer of Ti3C2T x Nanosheet colloidal solution, i.e., MXene solution (the concentration is 6.63 mg / mL calculated by taking part of the solution, filtering and drying the mass and the volume of the solution).
[0059] (2) Weigh 40 mg of CNT and 64 mg of SDBS (sodium dodecylbenzene sulfonate) into a beaker, add 20 mL of deionized water, and place the resulting mixed solution into a cell crusher. The cell crusher is operated for 30 min at an interval of 5 s to obtain a CNT solution with a concentration of 2 mg / mL.
[0060] (3) Weigh 0.54 mL of CNT solution into a beaker and add a magnet. Place the beaker on a magnetic stirrer, weigh 5.28 mL of MXene solution, and add it to the beaker while stirring. After stirring for 40 min, a uniform MXene / CNT mixed solution is obtained, which is vacuum-filtered for 2.5 h and left for 24 h. The MXene / CNT composite film with a CNT mass ratio of 3% (denoted as MC-3) is peeled off from the filter paper.
[0061] (4) Place the MXene / CNT composite membrane in two polytetrafluoroethylene films with pre-reserved holes and fix them in two silicone rubber cavities of the same size. The area of the pre-reserved holes is 3 mm 2 The outside of the two silicone rubber cavities is sealed with a flexible film. The entire device consists of two silicone rubber cavities, each of which has an internal size of 20 mm long, 15 mm wide, and 3 mm high, with a circular hole of 10 mm in diameter in the middle.
[0062] (5) The two silicone rubber cavities are filled with 0.01 M NaCl electrolyte and two Ag / AgCl electrodes are used to connect to the external circuit. In addition, the Ag / AgCl electrodes are only in the electrolyte and are not in direct contact with the composite membrane.
[0063] Example 2
[0064] The preparation method of the MXene / CNT composite film self-powered linear pressure sensor of this embodiment comprises the following steps:
[0065] (1) A MXene solution with a concentration of 6.63 mg / mL was obtained by selectively etching the precursor MAX phase with HCl and LiF. Specifically, 1.0 g of LiF powder and 1.0 g of Ti3AlC2 were weighed, and LiF and 20.0 mL of HCl (75 wt.%) were mixed, Ti3AlC2 (MAX phase) was slowly added to the mixed solution, and fully reacted for 24 h at 35 ° C by magnetic stirring. After the reaction was completed, the obtained acidic reactant was placed in a centrifuge tube, deionized water was added, and the centrifuge speed was set to 3500 rpm, and centrifuged for 3 min to obtain a precipitate. Deionized water was added again for a second centrifugal washing, and water molecules were inserted into the interlayer by hand shaking to increase the interlayer spacing of the product. The above process was repeated many times until the pH value of the reactant was neutral. Then, the precipitate was dispersed in a certain amount of deionized water, argon was continuously introduced under water bath conditions below 15 ° C, and ultrasonic peeling was performed for 1.0 h using an ultrasonic machine. Finally, the supernatant was collected by centrifugation at 3500 rpm for 1 h, which was a monolayer of Ti3C2T x Nanosheet colloidal solution, i.e., MXene solution (the concentration is 6.63 mg / mL calculated by taking part of the solution, filtering and drying the mass and the volume of the solution).
[0066] (2) Weigh 40 mg of CNT and 64 mg of SDBS into a beaker, add 20 mL of deionized water, and place the resulting mixed solution into a cell crusher. The cell crusher is operated for 30 min at a 5 s interval to obtain a CNT solution with a concentration of 2 mg / mL.
[0067] (3) Weigh 1.12 mL of CNT solution into a beaker and add a magnet. Place the beaker on a magnetic stirrer and weigh 5.28 mL of MXene solution. Add the solution into the beaker while stirring. Stir for 40 min to obtain a uniform MXene / CNT mixed solution. Vacuum filter the solution for 2.5 h and place it for 24 h. Peel the solution off the filter paper to obtain a MXene / CNT composite film with a CNT mass ratio of 6% (denoted as MC-6).
[0068] (4) Place the MXene / CNT composite membrane in two polytetrafluoroethylene films with pre-reserved holes and fix them in two silicone rubber cavities of the same size. The area of the pre-reserved holes is 3 mm 2 The outside of the two silicone rubber cavities is sealed with a flexible film. The entire device consists of two silicone rubber cavities, each of which has an internal size of 20 mm long, 15 mm wide, and 3 mm high, with a circular hole of 10 mm in diameter in the middle.
[0069] (5) The two silicone rubber cavities are filled with 0.01 M NaCl electrolyte and two Ag / AgCl electrodes are used to connect to the external circuit. In addition, the Ag / AgCl electrodes are only in the electrolyte and are not in direct contact with the composite membrane.
[0070] Example 3
[0071] The preparation method of the MXene / CNT composite film self-powered linear pressure sensor of this embodiment comprises the following steps:
[0072] (1) A MXene solution with a concentration of 6.63 mg / mL was obtained by selectively etching the precursor MAX phase with HCl and LiF. Specifically, 1.0 g of LiF powder and 1.0 g of Ti3AlC2 were weighed, and LiF and 20.0 mL of HCl (75 wt.%) were mixed, Ti3AlC2 (MAX phase) was slowly added to the mixed solution, and fully reacted for 24 h at 35 ° C by magnetic stirring. After the reaction was completed, the obtained acidic reactant was placed in a centrifuge tube, deionized water was added, and the centrifuge speed was set to 3500 rpm, and centrifuged for 3 min to obtain a precipitate. Deionized water was added again for a second centrifugal washing, and water molecules were inserted into the interlayer by hand shaking to increase the interlayer spacing of the product. The above process was repeated many times until the pH value of the reactant was neutral. Then, the precipitate was dispersed in a certain amount of deionized water, argon was continuously introduced under water bath conditions below 15 ° C, and ultrasonic peeling was performed for 1.0 h using an ultrasonic machine. Finally, the supernatant was collected by centrifugation at 3500 rpm for 1 h, which was a monolayer of Ti3C2T x Nanosheet colloidal solution, i.e., MXene solution (the concentration is 6.63 mg / mL calculated by taking part of the solution, filtering and drying the mass and the volume of the solution).
[0073] (2) Weigh 40 mg of CNT and 64 mg of SDBS into a beaker, add 20 mL of deionized water, and place the resulting mixed solution into a cell crusher. The cell crusher is operated for 30 min at a 5 s interval to obtain a CNT solution with a concentration of 2 mg / mL.
[0074] (3) Weigh 1.73 mL of CNT solution into a beaker and add a magnet. Place the beaker on a magnetic stirrer and weigh 5.28 mL of MXene solution. Add the solution into the beaker while stirring. Stir for 40 min to obtain a uniform MXene / CNT mixed solution. Vacuum filter the solution for 2.5 h and place it for 24 h. Peel the solution off the filter paper to obtain a MXene / CNT composite film with a CNT mass ratio of 9% (denoted as MC-9).
[0075] (4) Place the MXene / CNT composite membrane in two polytetrafluoroethylene films with pre-reserved holes and fix them in two silicone rubber cavities of the same size. The area of the pre-reserved holes is 3 mm 2 The outside of the two silicone rubber cavities is sealed with a flexible film. The entire device consists of two silicone rubber cavities, each of which has an internal size of 20 mm long, 15 mm wide, and 3 mm high, with a circular hole of 10 mm in diameter in the middle.
[0076] (5) The two silicone rubber cavities are filled with 0.01 M NaCl electrolyte and two Ag / AgCl electrodes are used to connect to the external circuit. In addition, the Ag / AgCl electrodes are only in the electrolyte and are not in direct contact with the composite membrane.
[0077] Comparative Example 1
[0078] This comparative example is a method for preparing a MXene film sensor, and the preparation method is as follows:
[0079] (1) A MXene solution with a concentration of 6.63 mg / mL was obtained by selectively etching the precursor MAX phase with HCl and LiF. Specifically, 1.0 g of LiF powder and 1.0 g of Ti3AlC2 were weighed, and LiF and 20.0 mL of HCl (75 wt.%) were mixed, Ti3AlC2 (MAX phase) was slowly added to the mixed solution, and fully reacted for 24 h at 35 ° C by magnetic stirring. After the reaction was completed, the obtained acidic reactant was placed in a centrifuge tube, deionized water was added, and the centrifuge speed was set to 3500 rpm, and centrifuged for 3 min to obtain a precipitate. Deionized water was added again for a second centrifugal washing, and water molecules were inserted into the interlayer by hand shaking to increase the interlayer spacing of the product. The above process was repeated many times until the pH value of the reactant was neutral. Then, the precipitate was dispersed in a certain amount of deionized water, argon was continuously introduced under water bath conditions below 15 ° C, and ultrasonic peeling was performed for 1.0 h using an ultrasonic machine. Finally, the supernatant was collected by centrifugation at 3500 rpm for 1 h, which was a monolayer of Ti3C2T x Nanosheet colloidal solution, i.e., MXene solution (the concentration is 6.63 mg / mL calculated by taking part of the solution, filtering and drying the mass and the volume of the solution).
[0080] (2) Weigh 5.28 mL of MXene solution, vacuum filter it for 2.5 h and leave it for 24 h, and peel it off from the filter paper to obtain the MXene membrane.
[0081] (4) Place the MXene membrane in two polytetrafluoroethylene films with pre-reserved holes and fix them in two silicone rubber cavities of the same size. The area of the pre-reserved holes is 3 mm 2 The outside of the two silicone rubber cavities is sealed with a flexible film. The entire device consists of two silicone rubber cavities, each of which has an internal size of 20 mm long, 15 mm wide, and 3 mm high, with a circular hole of 10 mm in diameter in the middle.
[0082] (5) The two silicone rubber cavities were filled with 0.01 M NaCl electrolyte and two Ag / AgCl electrodes were used to connect to the external circuit. In addition, the Ag / AgCl electrodes were only in the electrolyte and not in direct contact with the MXene film.
[0083] Test Case
[0084] Figure 2 The precursor Ti3AlC2 used in the present invention and the prepared Ti3C2T X From the XRD pattern, it can be seen that the Al in the precursor (Ti3AlC2) was successfully etched away.
[0085] Figure 3 The XRD diagram of the MXene / CNT composite film prepared in Example 1-3 of the present invention shows that CNT intercalation into MXene will change the diffraction peak angle of the composite film, thereby changing its interlayer spacing. From the formula 2dsinθ=0.15406, it can be seen that the interlayer spacing of the MXene film is 1.315nm, MC-3 is 1.369nm, MC-6 is 1.489nm, and MC-9 is 1.546nm.
[0086] Figure 4 This is a cross-sectional SEM image of the MXene / CNT composite film prepared in the present invention. It can be seen that the composite film has an obvious layered structure.
[0087] Figure 5 The mechanical properties of the MXene film and MXene / CNT film (MC-6) prepared by the present invention are shown in the figure. It can be seen that with the addition of CNT, the composite film has better mechanical properties. Specifically, the tensile fracture strength of the MXene film is 11.20Mpa, and the elongation at break is 5.0%; the tensile fracture strength of the MXene / CNT film (MC-6) is 17.85Mpa, and the elongation at break is 7.5%.
[0088] Figure 6The surface potential of the MXene film and the MXene / CNT film prepared in the present invention. It can be seen from the figure that the Zeta potential of the MXene and MXene / CNT solutions are -32.22 mV and -29.92 mV, respectively. The MXene / CNT composite film is the same as the MXene film. Its negative surface potential can adsorb more cations, which is beneficial to improve the sensitivity and response time of the sensor. Moreover, the interlayer channel of the composite film is adjustable, and the optimal ion transport performance can be controlled.
[0089] In order to further detect the performance of the sensor, VT test was performed on the sensors prepared in Examples 1-3 and Comparative Example 1. The specific steps are as follows: the pressure-electrical signal conversion test system consists of a motion control axis, a force gauge and a source meter. The motion control axis applies pressure to the sensor through the propulsion distance, the force gauge tests the pressure, and the source meter records the output electrical signal.
[0090] Figure 7 The VT diagrams of the self-powered linear pressure sensors prepared in Examples 1-3 of the present invention and the MXene film sensor prepared in Comparative Example 1 show that when the CNT doping mass ratio is 6%, the composite film has the best performance and the output voltage is 3.05 mV.
[0091] In order to test the sensing performance of the sensor prepared in Example 2 under different pressures, its IT and VT under different pressures were tested, and the results are as follows:
[0092] Figure 8 The IT diagram of the self-powered linear pressure sensor prepared in Example 2 of the present invention at different pressures shows that as the pressure increases, the output current increases accordingly. When the pressure is 8.6 kPa, the output current density is 160.58 nA / cm 2 .
[0093] Fig. 9 The VT diagram of the self-powered linear pressure sensor prepared in Example 2 of the present invention at different pressures shows that as the pressure increases, the output voltage increases accordingly. When the pressure is 8.6 kPa, the output voltage is 0.18 mV.
[0094] Fig.10 The VP diagram of the self-powered linear pressure sensor prepared in Example 2 of the present invention shows that the linearity of input pressure-output voltage is 0.999.
[0095] Fig.11 The IP diagram of the self-powered linear pressure sensor prepared in Example 2 of the present invention shows that the linearity of input pressure-output current is 0.990.
[0096] Fig.12The response and recovery time diagram of the self-powered linear pressure sensor 1 prepared in Example 2 of the present invention shows that the sensor has an extremely fast reaction speed. When stimulated by external pressure (6.3 kPa), the response time is 51.3 ms and the recovery time is 60.2 ms.
[0097] Fig.13 The response and recovery time diagram of the self-powered linear pressure sensor V prepared in Example 2 of the present invention shows that the sensor has an extremely fast reaction speed. When stimulated by external pressure (3.3 kPa), the response time is 70.9 ms and the recovery time is 101.8 ms.
[0098] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a MXene / CNT composite film self-powered linear pressure sensor, characterized in that: Here are the steps: (1) After mixing the MXene solution with the CNT solution, the MXene / CNT composite membrane was prepared by vacuum-assisted filtration; (2) Placing two polytetrafluoroethylene films with pre-reserved holes on both sides of the MXene / CNT composite film to form a sandwich structure film; (3) The sandwich structure film is fixed in two silicone rubber cavities, and the outside of the silicone rubber cavity is sealed by a flexible film; (4) Filling the silicone rubber cavity with electrolyte; (5) The Ag / AgCl electrode connected to the external circuit was inserted into the silicone rubber cavity to prepare a MXene / CNT composite membrane self-powered linear pressure sensor.
2. The method for preparing the MXene / CNT composite film self-powered linear pressure sensor according to claim 1, characterized in that: The MXene solution in step (1) is obtained by selectively etching the precursor MAX phase with HCl and LiF, wherein M is a transition metal, A is mainly a group III element or a group IV element, and X is any one or a combination of two of C and N elements.
3. The method for preparing the MXene / CNT composite film self-powered linear pressure sensor according to claim 2, characterized in that: In the step (1), the proportion of CNT in the MXene / CNT composite film is 3-9 wt%.
4. The method for preparing the MXene / CNT composite film self-powered linear pressure sensor according to claim 3, characterized in that: The electrolyte in step (4) is sodium chloride, potassium chloride or magnesium chloride solution.
5. The method for preparing the MXene / CNT composite film self-powered linear pressure sensor according to claim 4, characterized in that: The electrolyte concentration in step (4) is 0.01-0.5M.
6. The method for preparing the MXene / CNT composite film self-powered linear pressure sensor according to claim 5, characterized in that: The electrolyte concentration in step (4) is 0.01-0.3M.
7. The method for preparing the MXene / CNT composite film self-powered linear pressure sensor according to claim 6, characterized in that: In the step (5), the Ag / AgCl electrode is only placed in the electrolyte and is not in direct contact with the MXene / CNT composite film.
8. A MXene / CNT composite film self-powered linear pressure sensor prepared by the preparation method according to any one of claims 1 to 7.
9. The MXene / CNT composite film self-powered linear pressure sensor according to claim 8, characterized in that: The pressure sensor has a voltage-pressure linearity of 0.999 and a current-pressure linearity of 0.
990.
10. The MXene / CNT composite film self-powered linear pressure sensor according to claim 8, characterized in that: When the pressure is 6.3 kPa, the current response time is 51.3 ms, and when the pressure is 3.3 kPa, the voltage response time is 70.9 ms.
Citation Information
Cited By
All-solid-state ionic liquid-MXene composite film self-energized linear pressure sensor and preparation method thereof
CN120507066A
Nanometer sensor monitoring method for laying pressure of fiber prepreg
CN120992066A