Magnetic powder inspection test block for induction current method and use method
By designing a magnetic powder flaw detection test block for the induction current method, using the annular cylinder structure and white paint-resistant grooves, the problem of incomplete sensitivity verification in the existing technology is solved, and efficient and accurate detection without test piece verification is achieved , suitable for a variety of ring-shaped magnetic powder flaw detection systems.
Patent Information
- Application Number
- CN202411243203.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-08
AI Technical Summary
The existing magnetic particle flaw detection detection system cannot guarantee completeness when verifying sensitivity, and requires sensitivity test pieces. The operator has high requirements and the accuracy of the verification results cannot be guaranteed.
Design a magnetic powder flaw detection block for induction current method, adopting an annular cylinder structure, with grooves engraved on the inner, outer and side surfaces, and painted with white paint. It is used to judge the sensitivity of the magnetic powder flaw detection system and polish the surface and hollow structures improve detection accuracy and sensitivity.
The comprehensive sensitivity of the magnetic powder flaw detection system can be verified without the help of sensitivity test pieces, ensuring the integrity and accuracy of the detection results. It is suitable for the magnetic powder flaw detection system of most ring parts induction current method. It has a simple structure, convenient production, low cost and good value of promotion and application.
Smart Images

Figure CN118914346A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of magnetic particle flaw detection, and in particular relates to a magnetic particle flaw detection test block for an induction current method and a use method thereof. Background Art
[0002] The induction current method is mainly used for testing annular parts in magnetic particle testing. Through the coupling induction between the part and the energized coil, an induced current is generated in the part. The magnetic field generated by the induced current is used to detect discontinuities in the part parallel to the direction of the induced current.
[0003] For magnetic particle flaw detection using the induction current method, a sensitivity test piece is usually attached to the inspected annular part to determine whether the surface magnetic field of the inspected part meets the detection requirements. However, there is a lack of means to verify the sensitivity of the entire detection system. For example, Chinese patent document CN103293218B discloses a method for verifying the sensitivity of a magnetic particle detection system for the inner wall of a deep hole annular part. This method involves a method for verifying the sensitivity of a magnetic particle detection system for the inner wall of an annular part. This method uses the annular part to be inspected to cut out the middle of the corresponding deep hole to form a notch that passes through the deep hole and has an axial interface with a regular geometric shape; an insert is processed with a cross-section that matches the notch and has an arc groove that matches the cut-off portion of the deep hole, the sensitivity test piece is attached to the middle of the arc groove of the insert, and the insert is then embedded in the notch of the deep hole annular part and fixed; the insert is removed after magnetization. , observe the display of the sensitivity test piece to determine the surface magnetic field of the inspected part; it can be seen that the above scheme has certain limitations, mainly manifested in that the above method mainly targets the inner wall of the part, not the entire part, and cannot guarantee the integrity of the sensitivity verification; and the annular part to be inspected is only a carrier. In the above method, the sensitivity test piece must be used to realize the verification of the comprehensive sensitivity of the system; and the use of sensitivity test pieces for verification requires certain operating skills and experience. If the operator is not familiar with the use of the test piece and the identification techniques of standard magnetic traces, the accuracy of the verification result cannot be guaranteed.
[0004] It can be seen that the existing sensitivity verification measures cannot guarantee the integrity of the verification because they only verify the inner wall of the part; and they need to be completed with the help of sensitivity test pieces, which has high requirements for operators, and the accuracy of the verification results cannot be guaranteed. Summary of the invention
[0005] The present invention provides a magnetic particle flaw detection test block for an induction current method and a method for using the same, in order to solve the technical problems that in existing sensitivity verification measures, only the inner wall of a part is verified, the integrity of the verification cannot be guaranteed; and the verification needs to be completed with the aid of a sensitivity test piece, which places high demands on operators and the accuracy of the verification result cannot be guaranteed.
[0006] In order to achieve the above object, the present invention adopts the following technical contents:
[0007] A magnetic particle flaw detection test block for an induction current method, comprising a test block body;
[0008] The test block body adopts an annular column structure, and the through hole of the test block body is used to be sleeved on the iron core of the magnetic particle flaw detection system;
[0009] At least one groove is engraved on the inner surface, the outer surface and the side surface between the inner surface and the outer surface of the test block body, and the groove is used as an artificial defect for judging the sensitivity of the magnetic particle flaw detection system.
[0010] Furthermore, the inner surface, outer surface and side surfaces of the test block body are all polished surfaces.
[0011] Furthermore, the inner surface, outer surface and side surfaces of the test block body are all coated with paint.
[0012] Furthermore, the paint is white resistant paint.
[0013] Furthermore, the paint layer thickness of the paint is less than or equal to 25 μm.
[0014] Furthermore, the test block body is made of ferromagnetic steel.
[0015] Furthermore, the test block body adopts an internal hollow structure.
[0016] A method for using a magnetic particle flaw detection test block for an induction current method, comprising:
[0017] S1: Polish all surfaces of the annular test block body, and carve at least one groove on the outer surface, inner surface and one side surface of the test block body as an artificial defect;
[0018] S2: coating all surfaces of the test block body with paint to obtain a test block;
[0019] S3: Clean all surfaces of the test block;
[0020] S4: Pass the iron core of the magnetic particle inspection system through the test block, use the continuous method to energize the detection coil of the magnetic particle inspection system, and apply the detection medium to the test block;
[0021] S5: Observe the surface of the test block to verify the sensitivity of the magnetic particle inspection system by checking whether all the artificial defects on the inner surface, outer surface and side of the test block are displayed.
[0022] Furthermore, it also includes:
[0023] S6: After completing the verification of the sensitivity of magnetic particle inspection, the test block is demagnetized, cleaned and rust-proofed in turn.
[0024] Furthermore, in S2, white resistant paint is applied to all surfaces of the test block body, and the thickness of the paint layer is controlled within 25 μm; in S5, artificial defects on the test block are identified under a black light.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] The invention provides a magnetic particle flaw detection test block for an induction current method, the test block comprises a test block body in the form of an annular column, the through hole of the test block body is sleeved on the iron core of a magnetic particle flaw detection system during a test; at least one groove is engraved on the inner surface, the outer surface and the side surface of the test block body, which is used as an artificial defect for judging the sensitivity of the magnetic particle flaw detection system; the positions of the artificial defects cover all detectable parts of the annular part, thereby ensuring the integrity of the sensitivity verification of the magnetic particle flaw detection system; the test block can be applied to the verification of the magnetic particle flaw detection system of the induction current method for most annular parts, and has strong versatility; the system comprehensive sensitivity of the induction current method can be verified without the aid of a sensitivity test piece; the test block has a simple structure, is easy to manufacture, can be repeatedly used, has a low manufacturing cost, and has good popularization and application value.
[0027] Preferably, in the present invention, the polished surface can reduce the surface roughness, improve the accuracy of magnetic particle inspection, and avoid misjudgment or missed inspection due to surface unevenness.
[0028] Preferably, in the present invention, the artificial defects are covered by the coating, simulating near-surface defects, so that the detection sensitivity is high, and the defect location cannot be predicted in advance during the detection process, highly simulating the surface state of the detected part.
[0029] Preferably, in the present invention, the use of white resistant paint is conducive to easier observation of the distribution of magnetic powder and the display of defects during magnetic particle inspection, thereby improving detection efficiency and accuracy.
[0030] Preferably, in the present invention, the paint layer thickness is controlled within 25 μm to ensure that the paint layer is not too thick to affect the adsorption of magnetic powder and the display of defects.
[0031] Preferably, in the present invention, the test block body is made of ferromagnetic steel with high magnetic permeability and small magnetic field loss during use, which can ensure that the test block generates sufficient magnetic field response during magnetic particle testing, thereby accurately simulating the performance of the actual workpiece during testing.
[0032] Preferably, in the present invention, the internal hollow structure reduces the weight of the test block, making it easier to operate and carry; at the same time, the hollow structure may help improve the distribution of the magnetic field and increase the sensitivity of detection.
[0033] The present invention also provides a method for using a magnetic particle flaw detection test block for an induction current method. Based on the above-mentioned magnetic particle flaw detection test block for an induction current method, the method first performs polishing, groove engraving, paint coating and other processes on the test block body in sequence to obtain the test block, then passes the iron core through the test block and adopts a continuous method to energize the detection coil of the magnetic particle flaw detection system, and completes the sensitivity detection of the magnetic particle flaw detection system by applying a detection medium to the test block. Finally, the sensitivity of the magnetic particle flaw detection is verified by whether all the artificial defects on the inner surface, outer surface and side of the test block are displayed; if all are displayed, it proves that the magnetic particle flaw detection system is sensitive, otherwise it is judged that the magnetic particle flaw detection system does not meet the sensitivity requirements. The method provides a standardized operating procedure for magnetic particle flaw detection to ensure the accuracy and repeatability of the detection results.
[0034] Preferably, in the present invention, after completing the magnetic particle inspection, the test block is demagnetized, cleaned and rust-proofed, so as to restore the original state of the test block, extend its service life, and prepare for the next use.
[0035] Preferably, in the present invention, the control of white paint resistance and paint layer thickness is specifically specified when applying paint, as well as the identification of artificial defects under a black light. The above operations further improve the accuracy and reliability of magnetic particle inspection. The use of a black light helps to more clearly observe the distribution of magnetic particles and the display of defects under dark field conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 A schematic diagram of the structure of a magnetic particle flaw detection test block for an induction current method provided by an embodiment of the present invention;
[0037] Figure 2 A side view of a magnetic particle flaw detection test block for an induction current method provided by an embodiment of the present invention;
[0038] Figure 3 A schematic diagram of a test block connection of a closed induction current method for a magnetic particle flaw detection test using an induction current method provided by an embodiment of the present invention;
[0039] Figure 4 A schematic diagram of test block connection for an open induction current method for a magnetic particle flaw detection test using an induction current method is provided in an embodiment of the present invention.
[0040] Reference numerals:
[0041] 1-test block body; 2-detection coil; 3-iron core; 4-magnetizing current. DETAILED DESCRIPTION
[0042] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail in the following specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0043] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.
[0044] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0045] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.
[0046] In the description of the embodiments of the present invention, it should be noted that if the terms "upper", "lower", "horizontal", "inner", etc. indicate an orientation or positional relationship based on the orientation or positional relationship shown in the drawings, or the orientation or positional relationship in which the product of the invention is usually placed when in use, it is only for the convenience of describing the present invention and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. In addition, the terms "first", "second", etc. are only used to distinguish the description, and cannot be understood as indicating or implying relative importance.
[0047] In addition, if the term "horizontal" appears, it does not mean that the component must be absolutely horizontal, but can be slightly tilted. For example, "horizontal" only means that its direction is more horizontal than "vertical", which does not mean that the structure must be completely horizontal, but can be slightly tilted.
[0048] In the description of the embodiments of the present invention, it is also necessary to explain that, unless otherwise clearly specified and limited, the terms "set", "install", "connect", and "connect" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal connection of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0049] Example 1
[0050] As mentioned in the background technology, the existing sensitivity verification measures cannot guarantee the integrity of the verification because only the inner wall of the part is verified; and it needs to be completed with the help of sensitivity test pieces, which has high requirements for operators, and the accuracy of the verification results cannot be guaranteed.
[0051] In order to solve the above problems, the present invention provides a magnetic particle flaw detection test block for an induction current method. The test block can realize efficient detection of the sensitivity of the detection system without the aid of a sensitivity test piece.
[0052] The present invention is further described in detail below with reference to the accompanying drawings and embodiments:
[0053] like Figure 1 and Figure 2 As shown, this test block provides a standardized evaluation tool to verify the sensitivity of the flaw detection system.
[0054] The test block mainly includes a test block body 1, wherein the test block body 1 adopts a unique annular column design, and a through hole design running through the center thereof is convenient for seamless fitting on the core component (i.e., the iron core 3) of the magnetic particle flaw detection system (magnetic particle detection system) to achieve precise positioning and testing.
[0055] In this embodiment, the test block is not only polished to achieve a mirror effect on the outer surface and the inner surface in contact with the iron core 3, but also finely polished on the side surface between the outer surface and the inner surface. This design not only improves the aesthetics, but also ensures the accuracy of the test.
[0056] In this embodiment, at least one groove is engraved on the inner surface, outer surface and side surface of the test block body 1 , and these grooves are set as artificial defects and serve as standard reference points for detection sensitivity.
[0057] In this embodiment, in order to facilitate the observation of the aggregation of magnetic powder, a layer of resistant paint is coated on the inner surface, outer surface and side surface, that is, all surfaces of the test block body 1, preferably white resistant paint. The artificial defects are covered by the coating, simulating near-surface defects, so that the detection sensitivity is high, and the defect location cannot be predicted in advance during the detection process, and the surface state of the inspected parts is highly simulated; and the use of white resistant paint is conducive to easier observation of the distribution of magnetic powder and the display of defects during magnetic particle inspection, thereby improving detection efficiency and accuracy.
[0058] In this embodiment, the thickness of the above coating is precisely controlled to ensure that it does not exceed 25 microns, which not only protects the test block substrate, but also does not affect the magnetic field distribution and magnetic powder aggregation effect during the magnetic particle inspection process, and can ensure that the paint layer is not too thick to affect the adsorption of magnetic powder and the display of defects.
[0059] In this embodiment, the test block body 1 is made of ferromagnetic steel. This material not only has good magnetic conductivity to ensure the effective transmission of the magnetic field during the flaw detection process, but also ensures the long-term service life of the test block due to its high strength and stability.
[0060] In this embodiment, the test block body 1 adopts an internal hollow structure design, which not only reduces the weight of the test block and facilitates operation and carrying, but also optimizes the magnetic field distribution, making the flaw detection effect more accurate and reliable.
[0061] like Figure 3 and Figure 4 As shown, this embodiment also provides a specific implementation process of a magnetic particle flaw detection test block for an induction current method, which is as follows:
[0062] S1: polishing all surfaces of the annular test block body 1, and engraving at least one groove on the outer surface, inner surface and one side surface of the test block body 1 as an artificial defect.
[0063] S2: Paint is applied to all surfaces of the test block body 1 to obtain a test block.
[0064] S3: Clean all surfaces of the test block.
[0065] S4: Pass the iron core 3 of the magnetic particle flaw detection system through the test block, use the continuous method to energize the detection coil 2 of the magnetic particle flaw detection system, and apply the detection medium to the test block.
[0066] S5: Observe the surface of the test block to verify the sensitivity of the magnetic particle inspection system by checking whether all the artificial defects on the inner surface, outer surface and side of the test block are displayed.
[0067] S6: After completing the verification of the sensitivity of magnetic particle inspection, the test block is demagnetized, cleaned and rust-proofed in turn.
[0068] like Figure 3 As shown, Figure 3 This is a schematic diagram of using the closed induction current method to detect system sensitivity. Figure 3 In the figure, the iron core 3 is in the shape of a U, the through hole of the test block is sleeved on one side of the iron core 3, and the side opposite to the test block is sleeved with a detection coil 2. When the power is on, a magnetizing current 4 is generated at both ends of the detection coil 2, and a detection medium is applied to the test block. Under suitable lighting, artificial defects on the test block can be observed. When all the artificial defects on the inner surface, outer surface and side surface are observed and identified, it proves that the sensitivity of the system is qualified; if the artificial defects on one side cannot be identified, it proves that the sensitivity of the system is unqualified.
[0069] like Figure 4 As shown, Figure 3 This is a schematic diagram of using the open induction current method to detect system sensitivity. Figure 3 In the figure, the iron core 3 is in the shape of an elongated strip, the through hole of the test block is sleeved on the iron core 3, and a detection coil 2 is sleeved on the outside of the test block. Similarly, the detection coil 2 will generate a magnetizing current 4 when powered on, and a detection medium is applied to the test block. Artificial defects on the test block can be observed under suitable lighting. When all the artificial defects on the inner surface, outer surface and side surface are observed and identified, it proves that the sensitivity of the system is qualified; if the artificial defects on one side cannot be identified, it proves that the sensitivity of the system is unqualified.
[0070] It can be seen that the method first polishes, grooves, and paints the test block body in sequence to obtain the test block, then passes the iron core through the test block and uses the continuous method to energize the detection coil of the magnetic particle flaw detection system, and completes the sensitivity detection of the magnetic particle flaw detection system by applying the detection medium to the test block. Finally, the sensitivity of the magnetic particle flaw detection is verified by whether all the artificial defects on the inner surface, outer surface and side of the test block are displayed; if all are displayed, it proves that the magnetic particle flaw detection system is sensitive, otherwise it is judged that the magnetic particle flaw detection system does not meet the sensitivity requirements. The method provides a standardized operating procedure for magnetic particle flaw detection to ensure the accuracy and repeatability of the test results.
[0071] Example 2
[0072] This embodiment also provides another method for using a magnetic particle inspection test block for an induction current method. The test block includes a test block body 1. The test block body 1 is made of ferromagnetic steel, or a material that is the same or similar to the material and heat treatment state of the inspected part, and is an internal hollow ring structure. Artificial defects are made in the circumferential direction on the inner surface, the outer surface and one side. The size of the artificial defects can be made in proportion to the defect length, width, depth, etc. of the QQI test piece, and can also be determined by the defect size of other traceable test blocks or test pieces, the specific situation of the inspected ring part, customer requirements, etc.
[0073] After the groove is engraved (the artificial defect is made), the entire surface of the test block body 1 is coated with resistant paint. In this embodiment, white resistant paint is preferably used, and the thickness of the paint layer is controlled within 25μm; since the test block material is ferromagnetic steel with high magnetic permeability, the magnetic field loss during use is small; the artificial defect positions cover all detectable parts; the artificial defects are covered by the coating, simulating near-surface defects, with high detection sensitivity, and the defective parts cannot be predicted in advance during the detection process, highly simulating the surface state of the detected parts, and the white coating makes it easier to identify defects under a black light, with high detection reliability; it can be mostly used for magnetic particle flaw detection of ring-shaped parts by the induction current method, and has strong applicability; the system comprehensive sensitivity of the induction current method can be verified; the structure is simple, the production is convenient, it can be reused, and the manufacturing cost is low.
[0074] The specific steps are as follows:
[0075] (1) A surface of a test block body 1 is polished, and an artificial defect is made on the outer surface, inner surface and one side surface of the annular test block body 1. The size of the artificial defect can be made with reference to the proportion of the QQI test piece, or it can be determined according to the user's requirements.
[0076] (2) All surfaces of the grooved annular test block body 1 are coated with white resistant paint, and the thickness of the paint layer is controlled within 25 μm, so that the artificial defects are completely covered and cannot be visually detected, thereby obtaining a test block.
[0077] (3) Pre-treat the finished test block to ensure that the surface is clean and free of impurities that may affect the test.
[0078] (4) Figure 3 and Figure 4 As shown, the detection system is installed, that is, the induction current device is installed, the iron core 3 passes through the test block, the detection coil 2 is energized using the continuous method, and the detection medium is applied to the test block;
[0079] (5) Under a suitable light source, observe the surface of the test block until all the artificial defects on the inner surface, outer surface and side surface are identified, indicating that the sensitivity of the system is qualified; otherwise, it is unqualified.
[0080] (6) Demagnetize and clean the test block, and store it using oil seals or other anti-rust treatments.
[0081] In summary, the present invention provides a magnetic particle flaw detection test block for an induction current method and a method for using the same, which has the following advantages over existing sensitivity detection measures:
[0082] Firstly, by designing a test block body with an annular cylindrical structure and engraving grooves on its inner surface, outer surface and side as artificial defects, the test block can comprehensively and accurately evaluate the sensitivity of the magnetic particle inspection system and ensure the accuracy and reliability of the test results; secondly, the test block body adopts a polished surface treatment, which not only improves the surface quality of the test block, but also enhances the clarity of the test results; further, the paint coated on the surface of the test block, especially the white paint, and the strict control of the paint layer thickness, effectively reduce external interference, improve the detection efficiency, and can more clearly identify artificial defects under the black light, enhancing the visibility of the detection; in addition, the test block body is made of ferromagnetic steel, which ensures its magnetization effect during the magnetic particle inspection process, and the design of the internal hollow structure reduces the weight of the test block and facilitates operation; finally, the technical scheme also provides a method for using the test block, including subsequent steps such as demagnetization, cleaning and rust prevention treatment, which ensures the long-term use effect of the test block and reduces maintenance costs. It can be seen that this technical solution has shown obvious advantages in detection sensitivity, surface quality, detection efficiency, visibility, material selection, structural design and subsequent maintenance, and is an important innovation in magnetic particle flaw detection technology.
[0083] The above embodiment is only one of the implementation methods that can realize the technical solution of the present invention. The scope of protection claimed by the present invention is not limited only to this embodiment, but also includes changes, replacements and other implementation methods that can be easily thought of by any technician familiar with the technical field within the technical scope disclosed by the present invention.
Claims
1. A magnetic particle testing test block for induction current method, characterized in that: It comprises a test block body (1); The test block body (1) adopts an annular column structure, and the through hole of the test block body (1) is used to be sleeved on the iron core (3) of the magnetic particle flaw detection system; At least one groove is engraved on the inner surface, the outer surface and the side surface between the inner surface and the outer surface of the test block body (1), and the groove serves as an artificial defect for judging the sensitivity of the magnetic particle flaw detection system.
2. A magnetic particle testing test block for induction current method according to claim 1, characterized in that: The inner surface, outer surface and side surfaces of the test block body (1) are all polished surfaces.
3. A magnetic particle testing test block for induction current method according to claim 1 or 2, characterized in that: The inner surface, outer surface and side surfaces of the test block body (1) are all coated with paint.
4. A magnetic particle testing test block for induction current method according to claim 3, characterized in that: The paint is white resistant paint.
5. The magnetic particle testing test block for induction current method according to claim 3, characterized in that: The paint layer thickness of the paint is less than or equal to 25 μm.
6. The magnetic particle testing test block for induction current method according to claim 1, characterized in that: The test block body (1) is made of ferromagnetic steel.
7. The magnetic particle testing test block for induction current method according to claim 1, characterized in that: The test block body (1) adopts an internal hollow structure.
8. A method for using a magnetic particle testing test block for an induction current method, characterized in that: include: S1: polishing all surfaces of the annular test block body (1), and engraving at least one groove as an artificial defect on the outer surface, the inner surface and one side surface of the test block body (1); S2: coating all surfaces of the test block body (1) with paint to obtain a test block; S3: Clean all surfaces of the test block; S4: passing the iron core (3) of the magnetic particle inspection system through the test block, energizing the detection coil (2) of the magnetic particle inspection system using a continuous method, and applying a detection medium to the test block; S5: Observe the surface of the test block to verify the sensitivity of the magnetic particle inspection system by checking whether all the artificial defects on the inner surface, outer surface and side of the test block are displayed.
9. The method for using a magnetic particle flaw detection test block for an induction current method according to claim 8, characterized in that: Also includes: S6: After completing the verification of the sensitivity of magnetic particle inspection, the test block is demagnetized, cleaned and rust-proofed in turn.
10. The method for using a magnetic particle flaw detection test block for an induction current method according to claim 8, characterized in that: In S2, white resistant paint is applied to all surfaces of the test block body (1), and the thickness of the paint layer is controlled within 25 μm; in S5, artificial defects on the test block are identified under a black light.
Citation Information
Cited By
Test block for assessing detection sensitivity of alternating electromagnetic field instruments
CN224744888U