Phase change filtering array, preparation method thereof and calculation spectrometer

By using phase change filter arrays in the calculation spectrometer, using alternating deposition of phase change layers and dielectric layers and different annealing temperature designs, the problems of high process requirements and fixed spectral transmittance are solved, low-difficulty manufacturing and spectral coding are achieved, and the improvement of the problem of high quality and high-quality spectral transmission is achieved. The detection effect and filtered pixel count are simplified.

CN118915219APending Publication Date: 2024-11-08HUAZHONG UNIV OF SCI & TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410910781.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Currently, there are problems with high process requirements and fixed spectral transmittance in the current calculation spectrometer, which leads to high production costs and difficulty in achieving continuous changes in spectral transmittance.

Method used

Using a phase change filter array, the phase change layer and dielectric layer are alternately deposited, combined with filter designs with different annealing temperatures, the low-difficulty manufacturing and spectral encoding of the resonant cavity structure are achieved, and the continuity of spectral transmittance is improved.

Benefits of technology

A filter array with low difficulty is realized, with spectral encoding in the visible and near-infrared range, which improves the detection effect and the number of filtered pixels, simplifies the preparation process, and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118915219A_ABST
    Figure CN118915219A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of spectral analysis, in particular to a phase change filtering array, a preparation method thereof and a calculation spectrograph, and the calculation spectrograph comprises the phase change filtering array; the phase change filtering array comprises a plurality of optical filters arranged in an array mode, and each optical filter comprises a transparent substrate. N groups of alternately deposited phase change layers and dielectric layers, wherein the phase change layer at the end part is deposited on the transparent substrate; and the angle reflection suppression layer is deposited on the dielectric layer at the end part. The method has the advantages that the filtering array suitable for being matched with the calculation spectrometer is manufactured with low difficulty, the continuity of the spectral transmittance of the filtering array is improved, the calculation spectrometer based on phase change is achieved by further combining an image sensor and a spectrum reconstruction algorithm, and the calculation efficiency is improved. The problem that the number of filtering pixels obtained by a traditional calculation spectrograph in a working wavelength range is limited is solved, and the performance of the spectrograph is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of spectral analysis, and in particular to a phase-change filter array and a preparation method thereof, and a computational spectrometer. Background Art

[0002] A spectrometer is a device used to study and analyze the spectrum of a substance. It can intuitively display a spectrum (the y-axis is intensity, the x-axis is light wavelength / frequency), which represents the distribution of light intensity with light wavelength. In nature, after a substance interacts with light, its emission, absorption, transmission or scattering spectrum will change in a certain spectral range or at a certain wavelength. This change is highly unique. By analyzing the spectral changes, the type or characteristics of the substance can be qualitatively or quantitatively analyzed. Therefore, spectral information can be regarded as the "fingerprint" of a substance, which is the innate "identity card" of each substance, and the spectrometer is the magical "eye" that helps humans understand the world. It is often used in the fields of intelligent manufacturing, intelligent sensing, and intelligent analysis.

[0003] Therefore, the basic function of a spectrometer is to measure the spectral composition of the absorption, emission, scattering or stimulated emission of the substance under study, including its wavelength and intensity. Spectroscopic technology uses the absorption, reflection and scattering characteristics of light inside the sample to detect sample parameters. It is widely used in environmental monitoring, biomedicine, agricultural science and technology, military analysis, and industrial process monitoring. In particular, the demand for a large number of civilian spectrometers in food safety, environmental and biological monitoring is growing. Therefore, the miniaturization of spectrometers is the only way to promote the development of civilian spectrometers.

[0004] Based on the development of computing power, computational spectrometers use compression coding technology to achieve better spectral measurements while greatly reducing the size and cost of the spectrometer. Currently, this technical solution mainly includes two parts: spectral coding and algorithm-based spectral reconstruction. Among them, spectral coding technology uses a detection structure with different spectral responses to compress and encode the spectrum of the incident light, and algorithm-based spectral reconstruction reversely reconstructs the signal obtained in the encoding process through an algorithm to calculate and restore the input spectrum.

[0005] The current spectral encoding strategy of computational spectrometers includes resonant cavity filters. The traditional resonant cavity filtering scheme has very high requirements for the preparation process. Specifically, the photolithography process is required to prepare micron-level or even sub-nanometer-level filters or filters, which has very high requirements for equipment and process. At the same time, this also leads to high preparation costs. And it is difficult to prepare a filter array with continuously changing spectral transmittance using traditional resonant cavity materials.

[0006] Regarding the above-mentioned related technologies, the current computational spectrometer has the problems of high process requirements and fixed spectral transmittance. Summary of the invention

[0007] In order to solve the problems of high process requirements and fixed spectral transmittance of current computational spectrometers, to achieve low-difficulty manufacturing of a filter array that matches the computational spectrometer and to improve the continuity of the spectral transmittance of the filter array, the present application provides a phase change filter array and a preparation method thereof, and a computational spectrometer.

[0008] In the first aspect, the phase change filter array provided in the present application adopts the following technical solution:

[0009] A phase change filter array includes a plurality of filters arranged in an array, each filter including:

[0010] Transparent substrate;

[0011] n groups of alternately deposited phase change layers and dielectric layers, wherein the phase change layers at the ends are deposited on the transparent substrate, wherein the material of the phase change layers is a phase change material with a low K value, n≥3, and the K value is <1;

[0012] An angle reflection suppression layer deposited on the dielectric layer at the end;

[0013] The annealing temperatures of the multiple filters after deposition are different, and the interval between adjacent annealing temperatures is 1 to 20°C.

[0014] By adopting the above technical scheme, on the one hand, the phase change layer and the dielectric layer are alternately arranged to cooperate to form a resonant cavity structure, so as to realize the low-difficulty manufacturing of a resonant cavity filter by using phase change materials; on the other hand, the phase change material of each filter is designed as a multi-layer film system structure, and the multi-layer arrangement improves the continuity of the transmittance in the corresponding band of the filter; further, the annealing temperatures of multiple filters are different, so that the crystallization degrees of the phase change materials of the multiple filters are as different and continuous as possible, even if the multiple filters have different transmittance ranges, they cooperate to realize the filtering requirements of a wide band; furthermore, the material of the phase change layer is limited to a phase change material with a low K value, so as to realize spectral encoding in the visible and near-infrared ranges; in summary, on the basis of the same phase change material, spectral encoding in the visible and near-infrared ranges is realized.

[0015] Optional, n≤7.

[0016] By adopting the above technical solution, the number of phase change layers is limited to 3≤n≤7, so as to maximize the bandwidth on the basis of the same material, control the light absorption, ensure the signal strength detected by the detector, and improve the detection effect.

[0017] Optional, n≤5.

[0018] By adopting the above technical solution, the number of phase change layers is limited to 3≤n≤5, so that on the basis of the same material, it is possible to further improve the bandwidth, control the light absorption, and enhance the detection effect.

[0019] Optionally, the material of the phase change layer is an alloy compound consisting of Sb element and S element or Se element.

[0020] By adopting the above technical solution, SbS alloy compounds and SbSe alloy compounds are both phase change materials with low K values, which can realize spectral encoding in the visible and near-infrared ranges, wherein the percentage of Sb element to S element can be adjusted according to actual needs, and the percentage of Sb element to Se element can be adjusted according to actual conditions.

[0021] Optionally, the material of the phase change layer is Sb2S3, and the thickness of the phase change layer is 10 to 150 nm.

[0022] By adopting the above technical solution, the material of the phase change layer is limited to Sb2S3, and the thickness of the phase change layer is controlled to be no more than 1um, and further limited to 10-150nm, so as to achieve better continuity of transmittance, and at the same time control light absorption and improve detection effect.

[0023] Optionally, the dielectric layer is any one of TiO2, SiO2, Ta2O5, and LaTiO3.

[0024] By adopting the above technical solution, the dielectric layer is limited to any one of TiO2, SiO2, Ta2O5, and LaTiO3, and the phase change layer is combined to form a resonant cavity filter to improve the filtering effect.

[0025] In a second aspect, the preparation method of the phase change filter array provided in the present application adopts the following technical solution:

[0026] The method for preparing a phase-change filter array is used to prepare the phase-change filter array, wherein after a plurality of filters are deposited, the method comprises the following steps:

[0027] Set the annealing temperature range;

[0028] Multiple annealing temperatures are set based on the annealing temperature range, and the multiple annealing temperatures correspond to multiple filters one by one:

[0029] The multiple filters are heated to corresponding annealing temperatures and then annealed for the same time, wherein the annealing time is 2 to 100 seconds.

[0030] By adopting the above technical solution, the annealing temperature range is set based on the working wavelength range required by the spectrometer, the annealing temperature interval setting when multiple filters are annealed is adjusted, preferably equal interval setting, and then annealing treatment is performed to improve the continuity of the change in the degree of crystallization of multiple filters, thereby improving the continuity of the change in the transmittance of the phase change filter array, so as to solve the problem of the limited number of filter pixels obtained by the traditional computational spectrometer within the working wavelength range.

[0031] Optionally, the starting temperature of the heating of the multiple filters is the same, and the starting temperature range is set to 100 to 240° C.;

[0032] The annealing temperature range is set to 220-500°C, and the difference between the starting temperature and the annealing temperature of the same filter is not less than 120°C.

[0033] By adopting the above technical solution, on the one hand, the starting point temperatures of multiple filters constituting the phase change filter array are set to be the same, thereby further improving the continuity and controllability of the change in the degree of crystallization of the multiple filters; on the other hand, the starting point temperature range is set to 100-240° C., the annealing temperature range is set to 220-500° C., and the difference between the starting point temperature and the annealing temperature is not less than 120° C., which satisfies the continuous change of transmittance while simplifying the number of filters to be set, thereby further simplifying the difficulty of preparing the phase change filter array.

[0034] Optionally, the deposition of each filter includes:

[0035] Set the deposition vacuum to 1*10 -5 ~5*10 -5 Pa, argon flow rate is 40-100 sccm;

[0036] The deposition power of the phase change layer is 15-60W, and the rate is 0.5-5s / nm;

[0037] The deposition power of the dielectric layer is 60-120 W, and the rate is 10-200 s / nm;

[0038] The deposition power of the angle reflection suppression layer is 40-80W, and the deposition rate is 0.2-2s / nm.

[0039] By adopting the above technical solution, the deposition vacuum degree and argon gas flow rate are controlled, and the deposition power and speed are limited to improve the deposition effect of each layer of thin film and improve the quality of the filter.

[0040] In the third aspect, the computational spectrometer provided in this application adopts the following technical solutions:

[0041] A computational spectrometer, comprising:

[0042] Collection agencies;

[0043] The phase-change filter array is attached in front of the lens of the collection mechanism, so that the light is collected by the collection mechanism after passing through the phase-change filter array.

[0044] By adopting the above technical solution, the phase change filter array is attached in front of the lens of the collection mechanism so that the light can be collected by the collection mechanism after passing through the phase change filter array, thereby realizing low-difficulty manufacturing of the computational spectrometer detection structure and having a continuously changing spectral transmittance, while increasing the number of filter pixels obtained within the working wavelength range of the computational spectrometer, thereby improving the performance of the computational spectrometer.

[0045] In summary, the present application includes at least one of the following beneficial technical effects:

[0046] 1. Design a multilayer film structure through phase change materials to realize the spectral encoding structure, and realize the easy manufacture of filter arrays with continuously changing spectral transmittance; further combine image sensors and spectral reconstruction algorithms to realize phase change-based computational spectrometers to solve the problem of limited number of filter pixels obtained by traditional computational spectrometers within the working wavelength range and improve their performance.

[0047] 2. The multi-layer setting of the phase change layer, combined with the low K value of the material, can meet the requirements of wide-band filtering on the basis of the same phase change material, and realize spectral encoding in the visible and near-infrared ranges; further, by setting the number of layers of the phase change layer, the bandwidth is increased while controlling the light absorption, ensuring the signal strength of the detector and improving the detection effect.

[0048] 3. By regulating the annealing of multiple filters, the continuity of the change in the degree of crystallization of multiple filters is improved, thereby improving the continuity of the change in the transmittance of the phase change filter array. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] Figure 1 is a schematic structural diagram of a phase change filter array according to Example 1 of the present application;

[0050] Figure 2 is a schematic structural diagram of the filter of Example 1 of the present application;

[0051] Figure 3 is a schematic diagram of the transmittance of each filter in the phase change filter array of Example 1 of the present application;

[0052] Figure 4 It is a schematic diagram of the transmittance of each filter in the phase change filter array of Example 2 of the present application.

[0053] Explanation of the reference numerals: 100, phase change filter array; 1, filter; 2, transparent substrate; 3, phase change layer; 4, dielectric layer; 5, angle reflection suppression layer. DETAILED DESCRIPTION

[0054] The following is combined with Figure 1 ~Attached Figure 4 , further details of this application are given.

[0055] <Phase Change Filter Array>

[0056] The present application discloses a phase change filter array, referring to Figure 1 The phase change filter array includes a plurality of filters 1 arranged in an array. The number of filters 1 is set according to the actual spectral analysis requirements. Exemplarily, the number of filters 1 is set to 18, and each filter 1 includes a transparent substrate 2, a phase change layer 3, a dielectric layer 4 and an angle reflection suppression layer 5.

[0057] The transparent substrate 2 is configured to meet the light transmittance requirement and provide rigid support at the same time, and may be any one of quartz glass, crystalline silicon, amorphous silicon or silicon nitride. Exemplarily, the transparent substrate 2 is quartz glass.

[0058] n groups of alternately deposited phase change layers 3 and dielectric layers 4, each group including one phase change layer 3 and one phase change layer 4, n≥3; the phase change layer 3 at the end is deposited on the transparent substrate 2, and the number of phase change layers 3 is set according to the actual requirements for continuity of transmittance, filter band and signal strength and other comprehensive control settings; preferably, the phase change layer 3 is set to 3 to 7 layers, and further preferably, the phase change layer 3 is set to 3 to 5 layers, so as to increase the bandwidth as much as possible on the basis of the same material, and at the same time, avoid the multi-layer setting resulting in a weak signal obtained by the detector, which affects the final detection effect; for example, refer to Figure 2 , the phase change layer 3 is set to 3 layers.

[0059] The material of the phase change layer 3 is a phase change material with a low K value, and the K value is less than 1 and tends to 0; in one embodiment, the material of the phase change layer 3 is an alloy compound composed of Sb elements and S elements, and optionally, the material of the phase change layer 3 is Sb2S3, and the corresponding thickness of the phase change layer 3 is 10 to 150 nm, and the thickness setting is determined according to the specific operating process and materials; in another embodiment, the material of the phase change layer 3 is an alloy compound composed of Sb elements and Se elements.

[0060] The dielectric layer 4 is n-1 layers, that is, the dielectric layer 4 has one less layer than the phase change layer 3, and is deposited alternately on the transparent substrate 2 according to the phase change layer 3, the dielectric layer 4, the phase change layer 3, the dielectric layer 4, ..., the phase change layer 3, the dielectric layer 4; in a possible implementation, the dielectric layer 4 is any one of TiO2, SiO2, Ta2O5, and LaTiO3, and exemplarily, the dielectric layer 4 is TiO2.

[0061] The angle reflection suppression layer 5 is deposited on the dielectric layer at the end to suppress angle reflection. An exemplary angle reflection suppression layer 5 may be MgF2.

[0062] The crystallization degree of the phase change material of multiple filters 1 is not exactly the same, so that the multiple filters 1 correspond to a variety of different transmittances, and the wide-band filtering requirements of multiple peaks required by the calculation spectrometer are realized. To achieve that the crystallization degree of the phase change material of multiple filters 1 is not exactly the same, different annealing conditions can be used to adjust the crystal phase of the phase change material, or different intensities of laser excitation can be used to adjust the crystal phase of the phase change material for different times, or voltage pulses of different lengths and intensities can be applied to change the crystallization degree of the phase change material; in one embodiment, the use of different annealing conditions to adjust the crystal phase of the phase change material can be to set different annealing temperatures, and the interval between adjacent annealing temperatures is 1 to 20°C.

[0063] In one embodiment, the annealing comprises the following steps:

[0064] Setting an annealing temperature range, wherein the annealing temperature range can be set to 220-500° C., that is, when the plurality of filters 1 are annealed, the lowest annealing temperature is not less than 220° C., and the highest annealing temperature is not more than 500° C., and the specific range is determined according to the actual spectral analysis requirements;

[0065] Based on the intervals of the annealing temperature range, multiple annealing temperatures are set, and the multiple annealing temperatures correspond one-to-one to the multiple filters 1. In one embodiment, the multiple filters 1 are set to be m, and the annealing temperature range is approximately equally divided into m-1 segments with the minimum temperature as the starting point and the maximum temperature as the end point, and then the corresponding m endpoint values ​​are obtained, and the m endpoint values ​​correspond one-to-one to constitute the annealing temperatures of the m filters 1, and the annealing temperatures of adjacent filters 1 are spaced 1 to 20°C, preferably at equal intervals, that is, equally divided within the annealing temperature range. Further, in order to facilitate temperature control, the difference between the intervals (the values ​​of each segment in the m-1 segments) is set to be close to 0 and not greater than 1, so as to improve the convenience of temperature control and tend to be equally spaced.

[0066] After the multiple filters 1 are heated to the corresponding annealing temperature, they are annealed for the same time. In one embodiment, the annealing time is 2 to 100 seconds. The specific annealing time is determined according to the actual situation.

[0067] In order to further improve the continuity and controllability of the crystallization degree changes of multiple filters 1 and simplify the number of filters 1, in another embodiment, multiple filters 1 are set to have the same starting temperature for heating in the annealing program, the starting temperature range is set to 100-240°C, the annealing temperature range is set to 220-500°C, and the difference between the starting temperature and the annealing temperature of the same filter is not less than 120°C.

[0068] In one embodiment, the phase change layer 3, the dielectric layer 4 and the angle reflection suppression layer 5 can be deposited on the transparent substrate 2 by magnetron sputtering or electron beam evaporation coating system (EBE). Exemplarily, magnetron sputtering deposition includes:

[0069] Set the deposition vacuum to 1*10 -5 ~5*10 -5 Pa, argon flow rate is 40-100 sccm;

[0070] The deposition power of the phase change layer 3 is 15-60W, and the rate is 0.5-5s / nm;

[0071] The deposition power of the dielectric layer 4 is 60-120 W, and the rate is 10-200 s / nm;

[0072] The deposition power of the angle reflection suppression layer 5 is 40-80 W, and the deposition rate is 0.2-2 s / nm.

[0073] <Computational Spectrometer>

[0074] Embodiment 4 of the present application discloses a computational spectrometer, which includes a collection mechanism and the above-mentioned phase change filter array 100 .

[0075] The collection mechanism may be a camera (exemplarily a CMOS camera) or other photodetector arrays, and the phase change filter array 100 is attached in front of the lens of the collection mechanism to couple the two, so that the light passes through the phase change filter array 100 and is collected by the collection mechanism;

[0076] The computational spectrometer may further include a host computer having a spectrum reconstruction algorithm, which is used to perform spectrum analysis based on the data collected by the collection mechanism through the spectrum reconstruction algorithm.

[0077] Embodiment 1:

[0078] Embodiment 1 of the present application discloses a method for preparing a phase change filter array, comprising the following steps:

[0079] Step 1: Preparation of multiple filters

[0080] In this embodiment, 18 filters are prepared, and the preparation of each filter includes multi-layer thin film deposition. Specifically, Sb2S3, TiO2, Sb2S3, TiO2, Sb2S3, TiO2, and MgF2 multi-layer thin films are sequentially deposited on a quartz glass substrate, and the deposition thicknesses are 43nm, 97nm, 89nm, 43nm, 92nm, 10nm, and 22nm, respectively. The multi-layer thin film deposition can be deposited by magnetron sputtering or electron beam evaporation coating system (EBE). In this embodiment, magnetron sputtering deposition is used. Specifically:

[0081] Set the deposition vacuum to 3*10 -5 Pa, argon flow rate is 70 sccm;

[0082] The deposition power of the phase change layer is 40W and the rate is 2.5s / nm;

[0083] The deposition power of the dielectric layer is 90W and the rate is 10 5 s / nm;

[0084] The deposition power of the angle reflection suppression layer is 60 W, and the deposition rate is 1.1 s / nm.

[0085] Step 2: Preparation of phase change filter array

[0086] Set the annealing temperature range to 240-420°C;

[0087] 18 annealing temperatures are set at equal intervals of 10°C based on the annealing temperature range, and the 18 annealing temperatures are determined to be 240°C, 250°C, 260°C, ..., 400°C, 410°C, and 420°C respectively;

[0088] Set the starting temperature to 120°C and the annealing time to 20s;

[0089] The (starting point temperature, annealing temperature, annealing time) of the 18 filters were annealed in the following correspondence: [(120°C, 240°C, 20s), (120°C, 250°C, 20s), (120°C, 260°C, 20s), ..., (120°C, 400°C, 20s), (120°C, 410°C, 20s), (120°C, 420°C, 20s)];

[0090] The 18 filter arrays after annealing are arranged to form a phase change filter array.

[0091] Example 2

[0092] Embodiment 2 of the present application discloses a method for preparing a phase change filter array, comprising the following steps:

[0093] Step 1: Preparation of multiple filters

[0094] In this embodiment, 7 filters are prepared, and the preparation of each filter includes multi-layer thin film deposition. Specifically, Sb2S3, TiO2, Sb2S3, TiO2, Sb2S3, TiO2, Sb2S3, TiO2, Sb2S3, TiO2, and MgF2 multi-layer thin films are deposited in sequence on a quartz glass substrate, and the deposition thicknesses are 15nm, 40nm, 43nm, 153nm, 40nm, 43nm, 107nm, 11nm, and 72nm, respectively. The multi-layer thin film deposition can be deposited by magnetron sputtering or electron beam evaporation coating system (EBE). In this embodiment, magnetron sputtering deposition is adopted. Specifically:

[0095] Set the deposition vacuum to 3*10 -5Pa, argon flow rate is 70 sccm;

[0096] The deposition power of the phase change layer is 40W and the rate is 2.5s / nm;

[0097] The deposition power of the dielectric layer is 90W and the rate is 10 5 s / nm;

[0098] The deposition power of the angle reflection suppression layer is 60 W, and the deposition rate is 1.1 s / nm.

[0099] Step 2: Preparation of phase change filter array

[0100] Set the annealing temperature range to 220-320°C;

[0101] Seven annealing temperatures are set based on the annealing temperature range, and the seven annealing temperatures are determined to be 220° C., 240° C., 260° C., 270° C., 290° C., 300° C., and 320° C.;

[0102] Set the starting temperature to 120°C and the annealing time to 15s;

[0103] The (starting point temperature, annealing temperature, annealing time) of the 18 filters were annealed according to [(120°C, 220°C, 15s), (120°C, 240°C, 15s), (120°C, 260°C, 15s), (120°C, 270°C, 15s), (120°C, 290°C, 15s), (120°C, 300°C, 15s), (120°C, 320°C, 15s)] respectively;

[0104] The 7 filter arrays after annealing are arranged to form a phase change filter array.

[0105] test

[0106] Test Example 1 obtains the transmittance of 18 filters corresponding to the phase change filter array. The results are as follows: Figure 3 As shown, according to Figure 3 It can be seen that the transmittance of the phase-change filter array changes continuously in a wide spectrum of 400 to 800 nm, and it is possible to manufacture a filter array with continuously changing spectral transmittance with low difficulty.

[0107] Test Example 2 obtains the transmittance of the seven filters corresponding to the phase change filter array. The results are as follows: Figure 4 As shown, according to Figure 4 It can be seen that the transmittance of the phase-change filter array changes continuously in a wide spectrum of 1000 to 1700 nm, and it is possible to manufacture a filter array with continuously changing spectral transmittance with low difficulty.

[0108] In summary, by further combining image sensors and spectral reconstruction algorithms, a phase-change based computational spectrometer can be obtained to solve the problem of the limited number of filter pixels obtained by traditional computational spectrometers within the working wavelength range and improve their performance.

[0109] The embodiments of this specific implementation are all preferred embodiments of the present application, and are not intended to limit the protection scope of the present application. The same components are represented by the same figure marks. Therefore, any equivalent changes made based on the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A phase change filter array, characterized in that: The invention comprises a plurality of filters arranged in an array, each filter comprising: Transparent substrate; n groups of alternately deposited phase change layers and dielectric layers, wherein the phase change layers at the ends are deposited on the transparent substrate, wherein the material of the phase change layers is a phase change material with a low K value, n≥3, and the K value is <1; An angle reflection suppression layer deposited on the dielectric layer at the end; The annealing temperatures of the multiple filters after deposition are different, and the interval between adjacent annealing temperatures is 1 to 20°C.

2. The phase change filter array according to claim 1, characterized in that: n≤7。 3. The phase change filter array according to claim 1, characterized in that: n≤5。 4. The phase change filter array according to claim 1, characterized in that: The material of the phase change layer is an alloy compound composed of Sb element and S element or Se element.

5. The phase change filter array according to claim 4, characterized in that: The material of the phase change layer is Sb2S3, and the thickness of the phase change layer is 10-150nm.

6. The phase change filter array according to claim 1, characterized in that: The dielectric layer is any one of TiO2, SiO2, Ta2O5, and LaTiO3.

7. A method for preparing a phase change filter array, characterized in that: Used to prepare the phase change filter array according to any one of claims 1 to 6, wherein after the deposition of multiple filters is completed, the following steps are included: Set the annealing temperature range; Multiple annealing temperatures are set based on the annealing temperature range, and the multiple annealing temperatures correspond to multiple filters one by one: The multiple filters are heated to corresponding annealing temperatures and then annealed for the same time, wherein the annealing time is 2 to 100 seconds.

8. The method for preparing a phase change filter array according to claim 7, characterized in that: The starting point temperature of the heating of multiple filters is the same, and the starting point temperature range is set to 100-240°C; The annealing temperature range is set to 220-500°C, and the difference between the starting temperature and the annealing temperature of the same filter is not less than 120°C.

9. The method for preparing a phase change filter array according to claim 8, characterized in that: The deposition of each filter includes: Set the deposition vacuum to 1*10 -5 ~5*10 -5 Pa, argon flow rate is 40-100 sccm; The deposition power of the phase change layer is 15-60W, and the rate is 0.5-5s / nm; The deposition power of the dielectric layer is 60-120 W, and the rate is 10-200 s / nm; The deposition power of the angle reflection suppression layer is 40-80W, and the deposition rate is 0.2-2s / nm.

10. A computational spectrometer, characterized in that include: Collection agencies; The phase change filter array according to any one of claims 1 to 6 is attached in front of the lens of the collection mechanism so that light can be collected by the collection mechanism after passing through the phase change filter array.

Citation Information

Cited By

  • Computational spectrometer based on photochromic microcavity coupling and spectral reconstruction method thereof

    CN122835557A