High-resolution negative photoresist as well as preparation method and application thereof

Through the copolymerization and cross-linking of succinimide-modified epoxy oligomer and photosensitive resin, the problem of low curing reaction rate of negative photoresist is solved, and high resolution and heat resistance are improved, with clear patterns and lines Clear and stable chemical properties, suitable for integrated circuits and semiconductor fields.

CN118915389AInactive Publication Date: 2024-11-08YANCHENG AIKEN TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410958667.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The curing reaction rate of existing negative photoresists is low, making it difficult to meet the needs of high efficiency, deep curing and high precision.

Method used

Copolymerization and cross-linking of succinimide-modified epoxy oligomer with photosensitive resin, and improve the resolution and heat resistance of photoresist by the chemical sensitization of modified epoxy oligomers and the activity of photoacid-producing groups. and achieve deep curing and chemical stability by optimizing the mass ratio of photosensitive resin and modified epoxy oligomer.

Benefits of technology

It significantly improves the resolution and heat resistance of negative photoresist, has clear patterns and clear lines, and has stable chemical properties after film formation, extending the storage cycle and processing resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004949645430000081
    Figure BDA0004949645430000081
  • Figure BDA0004949645430000091
    Figure BDA0004949645430000091
Patent Text Reader

Abstract

The invention provides a negative photoresist with high resolution. The negative photoresist comprises the following raw materials in parts by weight: 1-90 parts of photosensitive resin, 1-99 parts of a modified epoxy oligomer, 3-20 parts of a photoinitiator, 0.5-10 parts of a photoacid generator, 300-400 parts of an organic solvent and 0.5-10 parts of a cross-linking agent, wherein the modified epoxy oligomer is a succinimide modified epoxy oligomer. The negative photoresist provided by the invention has the advantages of excellent heat resistance and high resolution, high curing efficiency and deep curing, and is suitable for application in the fields of integrated circuit design, semiconductors and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of photoresist preparation, and particularly relates to a high-resolution negative photoresist and a preparation method and application thereof. Background Art

[0002] Chips are mainly made through processes such as photolithography doping, etching, packaging and testing. Photolithography is the process of patterning the substrate through light processes such as exposure and development. Light is projected onto the photoresist through a mask to stimulate a chemical reaction in the photoresist, which is then processed through development and other post-processing to form a fine pattern. Photoresist is one of the key materials for fine pattern processing in chip technology. It is also called photoresist. It is a light-sensitive liquid with photosensitive resin, sensitizer and solvent as the main components. In particular, the development of large-scale and ultra-large-scale integrated circuits in recent years has greatly promoted the research, development and application of photoresists.

[0003] According to whether the photoresist in the exposed area is removed or retained during the development process, it can be divided into two categories: positive photoresist and negative photoresist. Among them, the photoresist pattern that is not exposed is dissolved and is opposite to the mask pattern is called negative photoresist. The composition and structure of existing negative photoresists are constantly changing with the exposure wavelength to meet the requirements of integrated circuit process technology, and high-efficiency, deep-curing, and high-precision photoresists are still urgently needed in the market.

[0004] Patent CN 117311092 A discloses a negative photoresist and its preparation method and application. By adding alicyclic epoxy oligomers and cellulose acetate, it can quickly form a film and provide strength support after the solvent evaporates. After the alicyclic epoxy and epoxy oligomers are exposed to ultraviolet light, the polymerization reaction is rapid and a high-precision, high-strength structure is formed. The graphics obtained after development with a developer have clear contours, good stability, and high aspect ratio. However, the problem of low curing reaction rate of alicyclic epoxy resins has not been effectively solved.

[0005] Therefore, the present invention provides a high-resolution negative photoresist and a preparation method and application thereof, which are particularly important. Summary of the invention

[0006] In view of the defects of the prior art, the purpose of the present invention is to provide a high-resolution negative photoresist with excellent heat resistance, high curing efficiency and deep curing, which is suitable for application in fields such as integrated circuit design and semiconductors.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0008] On one hand, the present invention provides a high-resolution negative photoresist, which comprises the following raw materials in parts by weight: 1 to 90 parts of photosensitive resin, 1 to 99 parts of modified epoxy oligomer, 3 to 20 parts of photoinitiator, 0.5 to 10 parts of photoacid generator, 300 to 400 parts of organic solvent and 0.5 to 10 parts of cross-linking agent.

[0009] Wherein, the modified epoxy oligomer is a succinimide modified epoxy oligomer.

[0010] Preferably, the preparation steps of the modified epoxy oligomer are as follows:

[0011] (1) adding a first acrylic monomer and an epoxy resin into a reactor, then adding a catalyst, slowly heating to 80-100° C. and reacting for 2-6 hours to obtain an epoxy compound containing an unsaturated double bond;

[0012] (2) adding a monomer mixture of a second acrylic acid monomer, an acrylic ester monomer and a sulfonium group-containing monomer into another reactor, adding succinimide and an initiator, and stirring the mixture at 80 to 100° C. for 1 to 1.5 hours to obtain a prepolymer;

[0013] (3) Add an epoxy compound containing an unsaturated double bond and a prepolymer into another reactor, mix and stir, and obtain a modified epoxy oligomer.

[0014] More preferably, the mass ratio of the first acrylic monomer to the epoxy resin is (0.3-0.4):1.

[0015] Preferably, the first acrylic monomer is at least one of methacrylic acid and acrylic acid.

[0016] More preferably, the first acrylic monomer is acrylic acid.

[0017] Preferably, the epoxy resin is at least one of E44 epoxy resin and E51 epoxy resin.

[0018] More preferably, the epoxy resin is E44 epoxy resin.

[0019] Preferably, the catalyst is triethanolamine, and the added amount is 0.1-2% of the total mass of the first acrylic monomer and the epoxy resin.

[0020] Preferably, the monomer mixture is obtained by mixing the second acrylic monomer, the acrylic ester monomer and the sulfonium group-containing monomer in a mass ratio of 3: (0.5-2): (0.1-1).

[0021] Further preferably, the second acrylic monomer is acrylic acid, the acrylic ester monomer is polysiloxane methyl propionate, and the sulfonium group-containing monomer is (4-methylphenyl) diphenylsulfonium trifluoromethanesulfonic acid.

[0022] Preferably, the mass ratio of succinimide to the monomer mixture is (0.1-0.8):5.

[0023] Preferably, the initiator is at least one of azobisisoheptanenitrile, dimethyl azobisisobutyrate and benzoyl peroxide.

[0024] Further preferably, the added amount of the initiator is 0.1-1% of the total mass of the acrylate monomer mixture.

[0025] Preferably, the mass ratio of the epoxy compound containing unsaturated double bonds to the prepolymer is (2.5-4):1.

[0026] In the present invention, the applicant copolymerizes and cross-links a monomer mixture containing acrylic acid monomers, acrylate monomers and sulfonium monomers with a substance containing an epoxy group, and uses a compound containing a succinimide group as a modifier for modification, thereby significantly improving the resolution and heat resistance of the negative photoresist. The possible reason is that the modified epoxy oligomer provided by the present invention has an excellent chemical sensitization effect, the preferred photosensitive sulfonium monomer is highly compatible with acrylic acid and acrylate monomers, so that the polymer has a good acid production efficiency, and the sulfonium monomer itself is sensitive to radiation due to its strong ultraviolet light absorption. The large cross-sectional absorption effect of the fluorine atoms coupled to the side chain of the polymer increases the sensitivity and resolution of the modified epoxy oligomer; at the same time, the modifier undergoes a copolymerization and cross-linking reaction with the allyl group through a double bond, and the aromatic ring on the auxiliary main chain jointly increases the heat resistance of the modified epoxy oligomer.

[0027] Preferably, each part of the photosensitive resin contains the following raw materials in parts by weight: 10 to 70 parts of a photosensitive resin precursor, 2 to 50 parts of a cross-linking agent, 0.01 to 50 parts of a photoinitiator, 0.01 to 5 parts of an inhibitor, 0.01 to 5 parts of a silane coupling agent, 20 to 80 parts of an organic solvent 1, 50 to 70 parts of a silane-modified inorganic filler, 20 to 100 parts of a solvent 1 and 50 to 200 parts of a solvent 2.

[0028] Preferably, the raw materials of the photosensitive resin precursor include acrylic monomer, acrylic ester monomer, acrylic hydroxyl monomer, initiator, dispersant, organic solvent 2, inhibitor, catalyst, benzene ring-containing ketone compound, dianhydride, acyl chloride reagent, diamine and molecular weight regulator.

[0029] Further preferably, the raw materials of the photosensitive resin precursor include acrylic acid, methyl methacrylate, hydroxyethyl methacrylate, azobisisobutyronitrile, basic magnesium carbonate, propylene glycol methyl ether acetate, p-methoxyphenol, tetraethylammonium bromide, methoxyacetophenone, hexafluorodianhydride, pyridine, diaminodiphenylmethane and tetrahydrophthalic anhydride.

[0030] Preferably, the preparation steps of the photosensitive resin are as follows:

[0031] The photosensitive resin precursor, crosslinking agent, photoinitiator, polymerization inhibitor, silane coupling agent and silane-modified inorganic filler are dissolved in organic solvent 1, fully stirred until uniformly dispersed, added with solvent 1 and mixed, and the precipitated solid is washed with solvent 2 and dried to obtain the photosensitive resin.

[0032] Further preferably, the preparation steps of the photosensitive resin are as follows:

[0033] The photosensitive resin precursor, glycidyl acrylate, benzophenone, 4-methoxyphenol, KH570 and silane-modified inorganic filler are dissolved in N,N-dimethylacetamide, fully stirred until uniformly dispersed, methanol is added and mixed, and the precipitated solid is rinsed with deionized water and dried to obtain a photosensitive resin.

[0034] The present invention prepares a photosensitive resin containing a polyimide structure as a film-forming resin for a negative photoresist, and utilizes the rigidity, polarity and strain protection brought by the aromatic ring-containing polyacrylate of a certain chain length and the asymmetric structure of the main chain of the photosensitive resin to make the negative photoresist have good chemical stability.

[0035] Preferably, the mass ratio of the photosensitive resin to the modified epoxy oligomer is 1:(1.5-2).

[0036] The applicant regulates the mass ratio of the photosensitive resin and the modified epoxy oligomer to release the activity of the acid-generating groups while ensuring that the photosensitive resin protects the functional groups. At the preferred ratio, the photoacid-generating groups bonded to the modified epoxy oligomer greatly increase the compatibility and the resolution of the photoresist; at the same time, the influence of the silane-modified inorganic filler contained in the photosensitive resin on the solubility transformation of the negative photoresist system is avoided, and deep curing of the system is achieved, so that the negative photoresist has good film-forming properties, and the chemical properties are stable after film formation, which is conducive to processing resistance and extended storage period.

[0037] Preferably, the photoinitiator is 1-hydroxycyclohexyl phenyl ketone.

[0038] Preferably, the photoacid generator is an oxime ester initiator.

[0039] Preferably, the organic solvent is propylene glycol monomethyl ether acetate and / or dipropylene glycol methyl ether.

[0040] Preferably, the crosslinking agent is ethoxylated trimethylolpropane triacrylate.

[0041] Another aspect of the present invention provides a method for preparing a high-resolution negative photoresist, comprising the following steps:

[0042] The photosensitive resin, succinimide modified epoxy oligomer, photoinitiator, photoacid generator, organic solvent and crosslinking agent are mixed uniformly in a closed environment by mechanical stirring or ultrasonic treatment, heat treated at a temperature of ≥70°C for 5 to 20 minutes, and exposed to ultraviolet light after film formation to obtain the photoresist.

[0043] Preferably, the wavelength of the ultraviolet light is 200-400 nm, and the exposure energy is ≥80 mJ / mm 2 .

[0044] In another aspect, the present invention provides a high-resolution negative photoresist for use in integrated circuit design and semiconductors.

[0045] Compared with the prior art, the present invention has the following beneficial effects:

[0046] (1) The high-resolution negative photoresist provided by the present invention is obtained by copolymerizing and cross-linking a monomer mixture containing acrylic monomers, acrylate monomers and sulfonium monomers with a substance containing epoxy groups, and using a compound containing succinimide groups as a modifier to modify the negative photoresist. The excellent chemical sensitization effect of the modified epoxy oligomer is utilized to significantly improve the resolution and heat resistance of the negative photoresist.

[0047] (2) The high-resolution negative photoresist provided by the present invention uses a photosensitive resin containing a polyimide structure as the film-forming resin of the negative photoresist, and utilizes the rigidity, polarity and strain protection brought by the main chain containing aromatic rings and polymethyl methacrylate of a certain chain length and the asymmetric structure to increase the chemical stability of the negative photoresist.

[0048] (3) The high-resolution negative photoresist provided by the present invention increases the resolution of the photoresist by adjusting the mass ratio of the photosensitive resin and the modified epoxy oligomer, and utilizing the positive effect of the photoacid-generating groups bonded to the modified epoxy oligomer on the compatibility of the system; at the same time, it avoids the influence of the silane-modified inorganic filler contained in the photosensitive resin on the solubility transformation of the negative photoresist system, realizes deep curing of the system, and makes the negative photoresist have good film-forming properties. The chemical properties after film formation are stable, which is beneficial to improving the processing resistance and extending the storage period. DETAILED DESCRIPTION

[0049] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.

[0050] Unless otherwise specified, the reagents used below can be easily obtained from commercial companies, wherein polysiloxane methyl propionate was purchased from Guangdong Wengjiang Chemical Reagent Co., Ltd., and E44 epoxy resin was purchased from Feicheng Deyuan Chemical Co., Ltd.

[0051] Preparation Example 1

[0052] Preparation of the first modified epoxy oligomer:

[0053] (1) Add 3.5 g of acrylic acid and 10 g of E44 epoxy resin into a reactor, then add 0.2 g of triethanolamine, slowly raise the temperature to 90° C. and react for 4 h to obtain an epoxy compound containing an unsaturated double bond;

[0054] (2) In another reactor, a monomer mixture of 6 g acrylic acid, 2.6 g polysiloxane methyl propionate and 1 g (4-methylphenyl) diphenylsulfonium trifluoromethanesulfonic acid was added, and 0.9 g succinimide and 0.05 g azobisisoheptanenitrile were added, and the mixture was stirred at 90° C. for 1.3 h to obtain a prepolymer;

[0055] (3) In another reactor, 10 g of an epoxy compound containing an unsaturated double bond and 3 g of a prepolymer were added, and the mixture was mixed and stirred to obtain a modified epoxy oligomer.

[0056] Preparation Example 2

[0057] The preparation of the second modified epoxy oligomer is the same as that of Preparation Example 1, except that the amount of succinimide added is 8.6 g.

[0058] Preparation Example 3

[0059] The preparation of the third modified epoxy oligomer is the same as that of Preparation Example 1, except that acrylic acid, polysiloxane methyl propionate and (4-methylphenyl) diphenylsulfonium trifluoromethanesulfonate are added into the reactor and mixed in a mass ratio of 3:1:0.1 to obtain 9.6 g of a monomer mixture.

[0060] Preparation Example 4

[0061] The preparation of the fourth modified epoxy oligomer is the same as that of Preparation Example 1, except that acrylic acid, polysiloxane methyl propionate and (4-methylphenyl) diphenylsulfonium trifluoromethanesulfonate are added into the reactor and mixed in a mass ratio of 3:1:1.1 to obtain 9.6 g of a monomer mixture.

[0062] Preparation Example 5

[0063] The preparation steps of the photosensitive resin precursor are as follows:

[0064] (1) In a reactor, 0.3 g of acrylic acid, 15 g of methyl methacrylate and 13 g of hydroxyethyl methacrylate were copolymerized in 55 mL of propylene glycol methyl ether acetate, 0.28 g of azobisisobutyronitrile and 4.2 g of basic magnesium carbonate were added, and the mixture was reacted at 60° C. for 5 h to obtain an acrylic ester polymer;

[0065] (2) First, 95 mL of propylene glycol methyl ether acetate, 0.03 g of p-methoxyphenol and 0.4 g of tetraethylammonium bromide were added to the reactor, and then 50 g of acrylate polymer and 0.55 g of methoxyacetophenone were added to the reactor and mixed, and reacted at 15° C. for 8 h to obtain intermediate 1;

[0066] (3) 60 mL of propylene glycol methyl ether acetate and 0.4 mL of sulfuric acid were added to a reactor, 25.3 g of intermediate 1 and 1.6 g of hexafluorodianhydride were mixed and stirred, and the mixture was reacted at room temperature for 7 h to obtain intermediate 2;

[0067] (4) 250 mL of dichloromethane, 52.5 g of intermediate 2, 0.01 mL of N,N-dimethylformamide and 3.0 g of benzoyl chloride were added to the reactor in sequence, reacted at 6°C for 3 h, and reacted at 24°C for 5 h to obtain intermediate 3;

[0068] (5) 1.9 g of diaminodiphenylmethane and 125 mL of propylene glycol methyl ether acetate were added to the reactor and stirred evenly. Then, 54 g of intermediate 3 and 0.3 g of tetrahydrophthalic anhydride were added and mixed. The mixture was stirred and reacted at room temperature for 13 h. Then, 0.04 g of acetic anhydride and 0.03 g of pyridine were added and reacted at 13° C. for 4 h to obtain a photosensitive resin precursor.

[0069] Preparation Example 6

[0070] Preparation of silane-modified inorganic filler: 2 g of trifluoromethyltrimethylsilane and 50 g of mica powder were mixed at 220° C., and air flow was passed through the mixture to dehydrate the mixture at 120° C. to obtain a silane-modified inorganic filler.

[0071] Preparation Example 7

[0072] Preparation of photosensitive resin: 4 g of photosensitive resin precursor, 2.5 g of glycidyl acrylate, 2.5 g of benzophenone, 0.25 g of 4-methoxyphenol, 0.25 g of KH570 and 6 g of silane-modified inorganic filler were dissolved in 50 mL of N, N-dimethylacetamide, stirred until uniformly dispersed, 8 mL of methanol was added and mixed, and the precipitated solid was rinsed with 10 mL of deionized water and dried to obtain a photosensitive resin.

[0073] Unless otherwise specified, in the following examples, the photoinitiator is 1-hydroxycyclohexyl phenyl ketone, the photoacid generator is oxime ester initiator, the organic solvent is propylene glycol monomethyl ether acetate, and the crosslinking agent is ethoxylated trimethylolpropane triacrylate.

[0074] Example 1

[0075] A high-resolution negative photoresist comprises the following raw materials in parts by weight: 50 parts of photosensitive resin, 90 parts of first modified epoxy oligomer, 6.5 parts of photoinitiator, 5 parts of photoacid generator, 350 parts of organic solvent and 5 parts of crosslinking agent.

[0076] The method for preparing the negative photoresist of this embodiment comprises the following steps:

[0077] The raw materials in parts by weight are mixed uniformly by mechanical stirring in a closed environment, heat treated at 70° C. for 16 minutes, and exposed to ultraviolet light after film formation to obtain the photoresist.

[0078] Example 2

[0079] A high-resolution negative photoresist comprises the following raw materials in parts by weight: 90 parts of photosensitive resin, 90 parts of first modified epoxy oligomer, 20 parts of photoinitiator, 10 parts of photoacid generator, 400 parts of organic solvent and 10 parts of crosslinking agent.

[0080] The preparation method of the negative photoresist in this embodiment is the same as that in Example 1.

[0081] Example 3

[0082] A high-resolution negative photoresist comprises the following raw materials in parts by weight: 1 part of photosensitive resin, 2 parts of first modified epoxy oligomer, 3 parts of photoinitiator, 0.5 parts of photoacid generator, 300 parts of organic solvent and 0.5 parts of crosslinking agent.

[0083] The preparation method of the negative photoresist in this embodiment is the same as that in Example 1.

[0084] Example 4

[0085] A high-resolution negative photoresist comprises the following raw materials in parts by weight: 1.3 parts of photosensitive resin, 1 part of first modified epoxy oligomer, 6.5 parts of photoinitiator, 5 parts of photoacid generator, 350 parts of organic solvent and 5 parts of crosslinking agent.

[0086] The preparation method of the negative photoresist in this embodiment is the same as that in Example 1.

[0087] Example 5

[0088] A high-resolution negative photoresist comprises the following raw materials in parts by weight: 33 parts of photosensitive resin, 99 parts of first modified epoxy oligomer, 6.5 parts of photoinitiator, 5 parts of photoacid generator, 350 parts of organic solvent and 5 parts of crosslinking agent.

[0089] The preparation method of the negative photoresist in this embodiment is the same as that in Example 1.

[0090] Example 6

[0091] A high-resolution negative photoresist and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that the first modified epoxy oligomer is replaced by an equal amount of a second modified epoxy oligomer.

[0092] Example 7

[0093] A high-resolution negative photoresist and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that the first modified epoxy oligomer is replaced by an equal amount of a third modified epoxy oligomer.

[0094] Example 8

[0095] A high-resolution negative photoresist and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that the first modified epoxy oligomer is replaced by an equal amount of a fourth modified epoxy oligomer.

[0096] Performance Test:

[0097] The negative photoresists prepared in the above examples and comparative examples were subjected to the following performance tests. The specific test results are shown in Table 1.

[0098] (1) Development test: The exposed negative photoresist was developed in a 2.38 wt % tetramethylammonium hydroxide solution, rinsed in deionized water, and post-baked. The circuit pattern was observed and evaluated based on pattern clarity or pattern defects.

[0099] (2) Resolution test: The pattern morphology resolution test was carried out under a Hitachi SU8000 ultra-high resolution field emission scanning electron microscope, and the pattern morphology resolution was evaluated based on clear lines, line collapse, and poor morphology.

[0100] (3) Heat resistance test: Measure the film thickness of the cured film obtained by the negative photoresist and record it as t1. Further bake it in an oven at 240°C. Measure the film thickness after baking and record it as t2. Calculate the film thickness change rate ((t2-t1) / t2)*100%. When this value is ≤3%, the heat resistance is good.

[0101] Table 1

[0102]

[0103]

[0104] It can be seen from Table 1 that the negative photoresist prepared in Examples 1 to 3 of the present invention is a negative photoresist with excellent heat resistance and high resolution, high curing efficiency and deep curing, clear development patterns and clear lines.

[0105] Among them, by comparing Example 1 with Examples 4 and 5, it can be seen that Examples 4 and 5 are examples of changing the mass ratio of the photosensitive resin and the modified epoxy oligomer prepolymer, which shows that the modified epoxy oligomer provided by the present invention has excellent chemical sensitization. At the preferred mass ratio, the resin solubility in the negative photoresist system is excellent, the pattern is clear and the lines are clear, and the heat resistance is excellent, which improves the long-term reliability of the negative photoresist application; by comparing Example 1 with Example 6, it can be seen that the proportion of the modifier added to the second modified epoxy oligomer in Example 6 is inappropriate, resulting in excessive polymerization of the modified epoxy oligomer and improper molecular weight distribution. At the same time, the photoacid monomer copolymerized on the main chain of the epoxy oligomer causes the pattern to be over-developed and the resolution to deteriorate; by comparing Example 1 with Examples 7 and 8, it can be seen that Examples 7 and 8 are examples of changing the mass proportion of the photosensitive sulfonium monomer in the monomer mixture, which shows that the modified epoxy oligomer preferably prepared by the present invention can significantly exert the photosensitive acid production efficiency, thereby increasing the sensitivity and resolution of the negative photoresist.

[0106] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.

Claims

1. A high-resolution negative photoresist, characterized in that: The negative photoresist comprises the following raw materials in parts by weight: 1 to 90 parts of photosensitive resin, 1 to 99 parts of modified epoxy oligomer, 3 to 20 parts of photoinitiator, 0.5 to 10 parts of photoacid generator, 300 to 400 parts of organic solvent and 0.5 to 10 parts of crosslinking agent; Wherein, the modified epoxy oligomer is a succinimide modified epoxy oligomer.

2. The high-resolution negative photoresist according to claim 1, characterized in that: The preparation steps of the modified epoxy oligomer are as follows: (1) adding a first acrylic monomer and an epoxy resin into a reactor, then adding a catalyst, slowly heating to 80-100° C. and reacting for 2-6 hours to obtain an epoxy compound containing an unsaturated double bond; (2) adding a monomer mixture of a second acrylic acid monomer, an acrylic ester monomer and a sulfonium group-containing monomer into another reactor, adding succinimide and an initiator, and stirring the mixture at 80 to 100° C. for 1 to 1.5 hours to obtain a prepolymer; (3) Add an epoxy compound containing an unsaturated double bond and a prepolymer into another reactor, mix and stir, and obtain a modified epoxy oligomer.

3. The high-resolution negative photoresist according to claim 2, characterized in that: The monomer mixture is obtained by mixing the second acrylic monomer, the acrylic ester monomer and the sulfonium group-containing monomer in a mass ratio of 3: (0.5-2): (0.1-1).

4. The high-resolution negative photoresist according to claim 2, characterized in that: The acrylic monomer is acrylic acid, the acrylic ester monomer is polysiloxane methyl propionate, and the sulfonium group-containing monomer is (4-methylphenyl) diphenylsulfonium trifluoromethane sulfonate.

5. The high-resolution negative photoresist according to claim 2, characterized in that: The mass ratio of the succinimide to the monomer mixture is (0.1-0.8):

5.

6. The high-resolution negative photoresist according to claim 1, characterized in that: Each portion of the photosensitive resin contains the following raw materials in parts by weight: 10 to 70 parts of a photosensitive resin precursor, 2 to 50 parts of a crosslinking agent, 0.01 to 50 parts of a photoinitiator, 0.01 to 5 parts of an inhibitor, 0.01 to 5 parts of a silane coupling agent, 20 to 80 parts of an organic solvent 1, 50 to 70 parts of a silane-modified inorganic filler, 20 to 100 parts of a solvent 1 and 50 to 200 parts of a solvent 2.

7. The high-resolution negative photoresist according to claim 1, characterized in that: The mass ratio of the photosensitive resin to the modified epoxy oligomer is 1:(1.5-2).

8. The method for preparing a high-resolution negative photoresist according to any one of claims 1 to 7, characterized in that: The following steps are involved: The photosensitive resin, modified epoxy oligomer, photoinitiator, photoacid generator, organic solvent and crosslinking agent are mixed uniformly in a closed environment by mechanical stirring or ultrasonic treatment, heat treated at a temperature of ≥70°C for 5 to 20 minutes, and exposed to ultraviolet light after film formation to obtain the photoresist.

9. The method for preparing a high-resolution negative photoresist according to claim 8, characterized in that: The wavelength of the ultraviolet light is 200-400nm, and the exposure energy is ≥80mJ / mm 2 .

10. Application of the high-resolution negative photoresist according to any one of claims 1 to 7 in integrated circuit design and semiconductors.