Cambered surface magnetic ring and manufacturing process thereof
Through the simplified arc-surface magnetic ring manufacturing process, the combination of nano powder and specific auxiliary materials is used to solve the problems of low efficiency and high cost of traditional magnetic ring manufacturing processes, and the efficient and low-cost arc-surface magnetic ring production is achieved, with a strong structure and antioxidant properties.
Patent Information
- Application Number
- CN202410947641.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-16
AI Technical Summary
The traditional magnetic ring manufacturing process has low production efficiency, complex steps and high cost.
A arc-surface magnetic ring manufacturing process including raw material mixing, auxiliary material mixing, sintering raw material preparation, sintering raw material smelting, magnetic ring casting, magnetic ring blank heat treatment, surface grinding and surface spraying is adopted, and nano powder and specific auxiliary materials are used to pass through a vacuum furnace. Smelting and heat treatment form arc-surface magnetic rings.
The manufacturing process is simplified, the production efficiency is improved, and the cost is reduced. The resulting arc-surface magnetic ring structure has high strength, strong oxidation resistance, strong weather resistance and long service life.
Smart Images

Figure CN118919270A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of magnetic ring manufacturing, in particular to a curved magnetic ring and a manufacturing process thereof. Background Art
[0002] The magnetic ring is a ring-shaped magnetic conductor. It is a commonly used anti-interference component in electronic circuits and has a good inhibitory effect on high-frequency noise. The magnetic ring is a commonly used anti-interference component in electronic circuits and has a good inhibitory effect on high-frequency noise. It is generally made of ferrite materials. The magnetic ring has different impedance characteristics at different frequencies. Generally, the impedance is very small at low frequencies. When the signal frequency increases, the impedance of the magnetic ring increases sharply. As we all know, the higher the signal frequency, the easier it is to radiate. Generally, signal lines do not have a shielding layer, so these signal lines become good antennas, receiving various messy high-frequency signals in the surrounding environment. These signals are superimposed on the originally transmitted signals and even change the originally transmitted useful signals. Then, under the action of the magnetic ring, normal and useful signals can pass well, and high-frequency interference signals can be well suppressed, and the cost is low. Therefore, it is not surprising that everyone sees the plastic lump-shaped integrated magnetic ring on the display signal cable, USB cable, and even high-end keyboards and mice.
[0003] However, the traditional magnetic ring manufacturing process, such as the technical solution disclosed in the patent with application number CN202210862169.2 and invention name "A magnetic ring with curved surface and its manufacturing process", has low production efficiency, complex steps and high cost. Summary of the invention
[0004] Based on this, it is necessary to provide a curved magnetic ring manufacturing process to address the technical problems of low production efficiency, complex steps and high cost in the traditional magnetic ring manufacturing process.
[0005] A process for manufacturing a curved magnetic ring, the process comprising the following steps: The raw material mixing step comprises mixing 60 to 70 parts by weight of nano-iron oxide powder, 4 to 8 parts by weight of nano-nickel oxide powder, 10 to 20 parts by weight of nano-zinc oxide powder, 2 to 4 parts by weight of nano-copper oxide powder, 1 to 2 parts by weight of nano-cobalt oxide powder, 10 to 20 parts by weight of nano-manganese oxide powder, 0.5 to 1 part by weight of nano-silicon dioxide powder, 0.05 to 0.2 parts by weight of nano-titanium dioxide powder, and 0.05 to 0.2 parts by weight of nano-zirconium dioxide powder to obtain a raw material powder; Auxiliary material mixing step: 20 to 30 parts by weight of polylaurolactam, 4 to 8 parts by weight of calcium phosphate, 10 to 20 parts by weight of ethyltrimethoxysilane, 15 to 26 parts by weight of sodium metasilicate, 14 to 28 parts by weight of vinyltrimethoxysilane, 10 to 20 parts by weight of polyvinyl alcohol, and 8 to 16 parts by weight of calcium stearate are mixed and stirred to obtain a mixed auxiliary material; Sintering raw material preparation step: adding 10 to 20 parts by mass of a mixed auxiliary material to 100 parts by mass of a raw material powder, mixing and stirring uniformly to obtain a sintering raw material; Sintering raw material smelting step: smelting the sintering raw material in a vacuum furnace under the protection of protective gas to obtain a smelting liquid; Magnetic ring casting steps: pouring the molten liquid into the magnetic ring mold to cast the magnetic ring blank; The magnetic ring blank heat treatment step is: heating the magnetic ring blank at a temperature of 400 degrees Celsius to 600 degrees Celsius for 0.5 hour to 1 hour under the protection of a protective gas; Surface grinding step: Grind the surface of the magnetic ring after heat treatment to remove burrs.
[0006] Surface spraying step: spray the surface treatment liquid evenly on the surface of the magnetic ring blank to obtain a curved magnetic ring.
[0007] In one embodiment, the protective gas is nitrogen.
[0008] In one of the embodiments, in the sintering raw material melting step, the melting temperature is 1400 degrees Celsius to 1600 degrees Celsius.
[0009] In one of the embodiments, in the sintering raw material smelting step, the smelting liquid is uniformly stirred.
[0010] In one embodiment, the surface treatment liquid includes the following components in parts by weight: 30 to 50 parts of epoxy resin, 10 to 20 parts of polypropylene resin, 2 to 5 parts of antioxidant, 20 to 30 parts of filler, 0.4 to 1 part of coupling agent, 8 to 18 parts of silicon micropowder, and 1 to 2 parts of curing agent.
[0011] In one embodiment, the curing agent includes the following components in parts by weight: 30 to 40 parts of 1-cyanoethyl-2-phenylimidazolium-trimellitate, 10 to 20 parts of 2-phenyl-4,5-dihydroxymethylimidazole, and 30 to 50 parts of 2-phenyl-4-methyl-5-hydroxymethylimidazole.
[0012] In one embodiment, the filler includes the following components in parts by weight: 20 to 30 parts of talc powder, 10 to 20 parts of kaolin, 20 to 28 parts of vermiculite powder, 10 to 20 parts of calcium carbonate powder, and 10 to 16 parts of mica powder.
[0013] In one embodiment, the coupling agent is a silane coupling agent.
[0014] In one embodiment, the antioxidant is a mixture of chromium nitrate, sodium phosphite and sodium silicate.
[0015] A curved surface magnetic ring is manufactured by the curved surface magnetic ring manufacturing process in any of the above embodiments.
[0016] The manufacturing process steps of the arc surface magnetic ring are concise and exquisite, easy to control, and each step is carefully and meticulously carried out. In addition, the manufacturing process of the arc surface magnetic ring has high production efficiency and low production cost. The arc surface magnetic ring obtained by the manufacturing process of the arc surface magnetic ring has high structural strength, strong anti-oxidation performance, strong weather resistance and long service life. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 The figure is a schematic diagram of the process of manufacturing a curved magnetic ring in one embodiment. DETAILED DESCRIPTION
[0018] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0019] In order to make the above-mentioned purpose, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth so as to fully understand the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below. In the description of the present invention, it should be understood that the orientation or position relationship indicated by the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like is based on the orientation or position relationship shown in the accompanying drawings, only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation of the present invention.
[0020] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0021] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0022] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0023] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "upper", "lower", "left", "right" and similar expressions used herein are for illustrative purposes only and are not intended to be the only implementation method.
[0024] See also Figure 1 The present invention provides a process for manufacturing a curved magnetic ring, the process comprising the following steps: Step 101: Raw material mixing step: 60 to 70 parts by mass of nano-ferric oxide powder, 4 to 8 parts by mass of nano-nickel oxide powder, 10 to 20 parts by mass of nano-zinc oxide powder, 2 to 4 parts by mass of nano-copper oxide powder, 1 to 2 parts by mass of nano-cobalt trioxide powder, 10 to 20 parts by mass of nano-manganese oxide powder, 0.5 to 1 part by mass of nano-silicon dioxide powder, 0.05 to 0.2 parts by mass of nano-titanium dioxide powder, and 0.05 to 0.2 parts by mass of nano-zirconium dioxide powder are mixed and stirred to uniformly obtain raw material powder.
[0025] Specifically, 62 to 68 parts by mass of nano-ferric oxide powder, 5 to 7 parts by mass of nano-nickel oxide powder, 12 to 18 parts by mass of nano-zinc oxide powder, 2.5 to 3.5 parts by mass of nano-cobalt oxide powder, 1.2 to 1.8 parts by mass of nano-cobalt oxide powder, 12 to 18 parts by mass of nano-manganese oxide powder, 0.6 to 0.8 parts by mass of nano-silicon dioxide powder, 0.1 to 0.18 parts by mass of nano-titanium dioxide powder, and 0.1 to 0.15 parts by mass of nano-zirconium dioxide powder are mixed and stirred to uniformly obtain a raw material powder. Furthermore, 65 parts by mass of nano-ferric oxide powder, 6 parts by mass of nano-nickel oxide powder, 15 parts by mass of nano-zinc oxide powder, 3 parts by mass of nano-copper oxide powder, 1.5 parts by mass of nano-cobalt oxide powder, 15 parts by mass of nano-manganese oxide powder, 0.7 parts by mass of nano-silicon dioxide powder, 0.15 parts by mass of nano-titanium dioxide powder, and 0.12 parts by mass of nano-zirconium dioxide powder are mixed and stirred to uniformly obtain a raw material powder.
[0026] Step 102: Auxiliary material mixing step: 20 to 30 parts by weight of polylaurolactam, 4 to 8 parts by weight of calcium phosphate, 10 to 20 parts by weight of ethyltrimethoxysilane, 15 to 26 parts by weight of sodium metasilicate, 14 to 28 parts by weight of vinyltrimethoxysilane, 10 to 20 parts by weight of polyvinyl alcohol, and 8 to 16 parts by weight of calcium stearate are mixed and stirred to obtain mixed auxiliary materials.
[0027] Specifically, 22 to 38 parts by mass of polylaurolactam, 5 to 7 parts by mass of calcium phosphate, 12 to 18 parts by mass of ethyltrimethoxysilane, 18 to 24 parts by mass of sodium metasilicate, 16 to 24 parts by mass of vinyltrimethoxysilane, 14 to 18 parts by mass of polyvinyl alcohol, and 10 to 14 parts by mass of calcium stearate are mixed and stirred to obtain a mixed auxiliary material. Further, 32 parts by mass of polylaurolactam, 6 parts by mass of calcium phosphate, 15 parts by mass of ethyltrimethoxysilane, 22 parts by mass of sodium metasilicate, 20 parts by mass of vinyltrimethoxysilane, 16 parts by mass of polyvinyl alcohol, and 12 parts by mass of calcium stearate are mixed and stirred to obtain a mixed auxiliary material.
[0028] Step 103: Sintering raw material preparation step: Add 10 to 20 parts by mass of mixed auxiliary materials to 100 parts by mass of raw material powder, mix and stir evenly to obtain sintering raw materials.
[0029] Specifically, 12 to 18 parts by mass of the mixed auxiliary material are added to 100 parts by mass of the raw material powder, mixed and stirred evenly to obtain the sintering raw material. Further, 15 parts by mass of the mixed auxiliary material are added to 100 parts by mass of the raw material powder, mixed and stirred evenly to obtain the sintering raw material.
[0030] Step 104: Sintering raw material melting step: The sintering raw material is melted in a vacuum furnace under the protection of a protective gas to obtain a molten liquid.
[0031] In this embodiment, the protective gas is nitrogen. The melting temperature is 1400 degrees Celsius to 1600 degrees Celsius.
[0032] Specifically, the sintering raw materials are melted in a vacuum furnace under the protection of nitrogen at a melting temperature of 1400 degrees Celsius to 1600 degrees Celsius to obtain a molten liquid. Further, the molten liquid is uniformly stirred so that the components in the molten liquid are fully mixed.
[0033] Step 105: Magnetic ring casting step: pouring the molten liquid into the magnetic ring mold to cast into a magnetic ring blank.
[0034] Specifically, the molten liquid is poured into the magnetic ring mold, and after being gradually cooled, the mold is demoulded to form a magnetic ring blank. The gradual cooling stage: from 1000 degrees Celsius to room temperature at a cooling rate of 10 degrees per minute.
[0035] Step 106: heat treatment step of the magnetic ring blank: heat the magnetic ring blank at a temperature of 400 degrees Celsius to 600 degrees Celsius for 0.5 hour to 1 hour under the protection of a protective gas.
[0036] Specifically, the magnetic ring blank is heated at a temperature of 450 degrees Celsius to 550 degrees Celsius for 0.6 hours to 0.8 hours under the protection of nitrogen. Further, the magnetic ring blank is heated at a temperature of 500 degrees Celsius for 40 minutes under the protection of nitrogen to remove the stress in the magnetic ring blank.
[0037] Step 107: Surface polishing step: polish the surface of the heat-treated magnetic ring to remove burrs.
[0038] Specifically, the surface of the magnetic ring after heat treatment is polished with a polishing device to remove burrs, and a vacuum cleaner is used during the polishing process to effectively absorb the dust generated during the polishing process to avoid dust pollution to the processing environment.
[0039] Step 108: Surface spraying step: spray the surface treatment liquid evenly on the surface of the magnetic ring blank to obtain a curved magnetic ring.
[0040] Specifically, a surface treatment liquid is evenly sprayed on the surface of the magnetic ring blank by using a spraying device to obtain a curved magnetic ring.
[0041] In order to improve the anti-oxidation performance of the arc surface magnetic ring, in one embodiment, the surface treatment liquid includes the following components in parts by mass: 30 to 50 parts of epoxy resin, 10 to 20 parts of polypropylene resin, 2 to 5 parts of antioxidant, 20 to 30 parts of filler, 0.4 to 1 part of coupling agent, 8 to 18 parts of silicon powder, and 1 to 2 parts of curing agent. In this embodiment, the filler includes the following components in parts by mass: 20 to 30 parts of talc, 10 to 20 parts of kaolin, 20 to 28 parts of vermiculite powder, 10 to 20 parts of calcium carbonate powder, and 10 to 16 parts of mica powder. In one embodiment, the coupling agent is a silane coupling agent to increase the mixing uniformity of the components in the surface treatment liquid. In one embodiment, the antioxidant is a mixture of chromium nitrate, sodium phosphite and sodium silicate to increase the anti-oxidation performance of the surface treatment liquid, thereby further increasing the anti-oxidation performance of the arc surface magnetic ring. In this way, the surface treatment liquid can adhere well to the surface of the arc-surface magnetic ring to form a good protective layer, so as to increase the anti-oxidation performance of the arc-surface magnetic ring.
[0042] In order to accelerate the drying of the surface treatment liquid, in one embodiment, the curing agent includes the following components by weight: 30 to 40 parts of 1-cyanoethyl-2-phenylimidazolium-trimellitate, 10 to 20 parts of 2-phenyl-4,5-dihydroxymethylimidazole, and 30 to 50 parts of 2-phenyl-4-methyl-5-hydroxymethylimidazole. In this way, the curing agent composed of the above components can accelerate the drying of the surface treatment liquid, thereby improving production efficiency.
[0043] The present invention also provides a curved surface magnetic ring, which is made by the curved surface magnetic ring manufacturing process in any of the above embodiments.
[0044] The manufacturing process steps of the arc surface magnetic ring are concise and exquisite, easy to control, and each step is carefully and meticulously carried out. In addition, the manufacturing process of the arc surface magnetic ring has high production efficiency and low production cost. The arc surface magnetic ring obtained by the manufacturing process of the arc surface magnetic ring has high structural strength, strong anti-oxidation performance, strong weather resistance and long service life. The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0045] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A process for manufacturing a curved magnetic ring, characterized in that: The process comprises the following steps: The raw material mixing step comprises mixing 60 to 70 parts by weight of nano-iron oxide powder, 4 to 8 parts by weight of nano-nickel oxide powder, 10 to 20 parts by weight of nano-zinc oxide powder, 2 to 4 parts by weight of nano-copper oxide powder, 1 to 2 parts by weight of nano-cobalt oxide powder, 10 to 20 parts by weight of nano-manganese oxide powder, 0.5 to 1 part by weight of nano-silicon dioxide powder, 0.05 to 0.2 parts by weight of nano-titanium dioxide powder, and 0.05 to 0.2 parts by weight of nano-zirconium dioxide powder to obtain a raw material powder; Auxiliary material mixing step: 20 to 30 parts by weight of polylaurolactam, 4 to 8 parts by weight of calcium phosphate, 10 to 20 parts by weight of ethyltrimethoxysilane, 15 to 26 parts by weight of sodium metasilicate, 14 to 28 parts by weight of vinyltrimethoxysilane, 10 to 20 parts by weight of polyvinyl alcohol, and 8 to 16 parts by weight of calcium stearate are mixed and stirred to obtain a mixed auxiliary material; Sintering raw material preparation step: adding 10 to 20 parts by mass of a mixed auxiliary material to 100 parts by mass of a raw material powder, mixing and stirring uniformly to obtain a sintering raw material; Sintering raw material smelting step: smelting the sintering raw material in a vacuum furnace under the protection of protective gas to obtain a smelting liquid; Magnetic ring casting steps: pouring the molten liquid into the magnetic ring mold to cast the magnetic ring blank; The magnetic ring blank heat treatment step is: heating the magnetic ring blank at a temperature of 400 degrees Celsius to 600 degrees Celsius for 0.5 hour to 1 hour under the protection of a protective gas; Surface grinding step: Grind the surface of the heat-treated magnetic ring to remove the burrs; Surface spraying step: spray the surface treatment liquid evenly on the surface of the magnetic ring blank to obtain a curved magnetic ring.
2. The process according to claim 1, characterized in that The protective gas is nitrogen.
3. The process according to claim 1, characterized in that In the sintering raw material smelting step, the smelting temperature is 1400 degrees Celsius to 1600 degrees Celsius.
4. The process according to claim 1, characterized in that In the sintering raw material smelting step, the smelting liquid is uniformly stirred.
5. The process according to claim 1, characterized in that The surface treatment liquid includes the following components in parts by weight: 30 to 50 parts of epoxy resin, 10 to 20 parts of polypropylene resin, 2 to 5 parts of antioxidant, 20 to 30 parts of filler, 0.4 to 1 part of coupling agent, 8 to 18 parts of silicon powder, and 1 to 2 parts of curing agent.
6. The process according to claim 5, characterized in that The curing agent includes the following components in parts by mass: 30 to 40 parts of 1-cyanoethyl-2-phenylimidazolium trimellitate, 10 to 20 parts of 2-phenyl-4,5-dihydroxymethylimidazole, and 30 to 50 parts of 2-phenyl-4-methyl-5-hydroxymethylimidazole.
7. The process according to claim 5, characterized in that The filler includes the following components in parts by mass: 20 to 30 parts of talc powder, 10 to 20 parts of kaolin, 20 to 28 parts of vermiculite powder, 10 to 20 parts of calcium carbonate powder, and 10 to 16 parts of mica powder.
8. The process according to claim 5, characterized in that The coupling agent is a silane coupling agent.
9. The process according to claim 5, characterized in that The antioxidant is a mixture of chromium nitrate, sodium phosphite and sodium silicate.
10. A curved magnetic ring, characterized in that: The invention is manufactured by the arc surface magnetic ring manufacturing process of any one of claims 1 to 9.
Citation Information
Patent Citations
Magnetic ring with cambered surface and manufacturing process thereof
CN115295300A
Nickel zinc soft magnetic ferrite material
CN106252016A
High saturation magnetization soft magnetic ferrite material and preparation method thereof
CN106278225A
Power type nickel-zinc ferrite material and preparation method thereof
CN106587977A
High-strength magnetic core and preparation method thereof