Device and manufacturing method for non-deformation neodymium-iron-boron sintered blank magnet

By pre-pressing in the mold and maintaining constant pressure during the magnetic filling process, the deformation problem of neodymium iron boron magnet is solved, deformation-free sintered blanks are achieved, grinding rate and production costs are reduced, and it is suitable for all specifications and small-sized cylindrical products. .

CN118919281APending Publication Date: 2024-11-08杨俊林
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411326047.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The powder will deform when the traditional neodymium iron boron magnet is pressed and charged, resulting in a high grinding rate, especially the grinding rate of small-sized products is between 30% and 50%, which increases manufacturing time and resource waste.

Method used

Using a device and production method for sintering blank magnet without deformation, the powder particles are prevented from displaced, and the magnet structure stability is ensured, and the powder structure is sintered. After that, high temperature treatment is carried out.

Benefits of technology

Deformable-free NdFeB sintered blanks are achieved, and the grinding rate is reduced to less than 10%, which significantly saves production costs, improves density uniformity, cancels isostatic pressure processes, and reduces equipment and personnel costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919281A_ABST
    Figure CN118919281A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of sintered neodymium-iron-boron, and particularly discloses a device and a manufacturing method for a non-deformation neodymium-iron-boron sintered blank magnet. The method specifically comprises the working procedures of pre-pressing, magnetizing, pressing and sintering, wherein the pre-pressing working procedure is that magnetizing is started when the designed pre-pressing size is reached; in the magnetizing process, the pressure of an upper pressing head of a pressing machine is kept, so that powder particles can rotate and cannot move in the original position in a mold frame during magnetizing; the upper pressing head of the pressing machine continues to conduct pressurization, pressing is conducted to reach the pressing size, the pressed blank is taken out, and pressing is finished. And meanwhile, in the magnetizing procedure in the manufacturing of the neodymium iron boron sintered blank, the constant pressure of an upper pressing head of a pressing machine is maintained, the displacement phenomenon of powder particles in the magnetizing process is effectively prevented, the density of the manufactured pressed blank is uniform, and the sintered blank does not deform after being sintered. The method is not only suitable for neodymium iron boron sintered blanks of all specifications, but also suitable for small-specification cylindrical products, and the grinding rate of the products can be controlled to be 10% or below.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sintered NdFeB, and in particular relates to a device and a method for manufacturing a deformation-free NdFeB sintered blank magnet. Background Art

[0002] NdFeB magnet products are generally cylindrical, square and special-shaped products. The production process is that NdFeB powder is pressed - isostatically pressed - sintered.

[0003] When the magnets made by traditional technology are pressed and magnetized, the powder will move in two directions toward the pole in the mold. After sintering, the pressed green body will be deformed and needs to be ground to the finished product size required by the product. The grinding rate is high and the waste is large. Especially for small-sized products, such as small-sized cylindrical products of φ3mm to φ6mm, the grinding rate is between 30% and 50%. This undoubtedly increases the manufacturing time of the product, causing unnecessary waste of work resources, and also causes a certain waste of manufacturing resources. Summary of the invention

[0004] The object of the present invention is to provide a device and a method for producing a deformation-free NdFeB sintered blank magnet to solve the problems raised in the above-mentioned background technology.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A device for sintering deformation-free NdFeB blank magnets comprises a workbench, an upper drive assembly and a lower drive assembly, wherein the upper drive assembly comprises an upper pressure head, a connecting piece between the upper pressure head and a lower oil cylinder and an upper oil cylinder of a press; the lower drive assembly comprises a lower pressure head, a lower oil cylinder of a press and a connecting piece between the lower pressure head and a lower oil cylinder, a fixing groove is provided on the middle surface of the workbench, a mold frame is provided on the upper surface of the workbench, left and right magnetizing pole heads are provided on both sides of the mold frame, the lower pressure head is inserted into the inner side of the mold frame, and powder is provided on the inner side of the mold frame.

[0007] A method for manufacturing a deformation-free NdFeB sintered blank magnet comprises the following steps:

[0008] S1, pre-pressing stage:

[0009] First, start the press and assemble the upper pressure head of the mold, then pour the powder evenly into the mold frame, and use a scraper tool to ensure that the surface of the powder is flush with the upper edge of the mold frame to eliminate unevenness. The powder is neodymium iron boron powder;

[0010] Next, the upper pressing head of the mold is slowly pre-pressed into the mold frame until it reaches the preset pre-pressing size, and magnetization begins;

[0011] S2, magnetization stage:

[0012] After the pre-pressing size is in place, magnetization is carried out. During this process, the pressure of the pressing head on the press is maintained constant. The magnetic field generated at the beginning of magnetization is transmitted to the powder through the pole head of the clamping mold frame to magnetize the powder. During the magnetization process, the powder particles will not move, and the powder particles will rotate in the original position to ensure the stability of the magnet structure;

[0013] In S3, the suppression phase:

[0014] After the magnetization is completed, the pressing process begins immediately. The pressure head on the press continues to increase the pressure until the predetermined pressing size is reached. After the pressing is completed, the blank is taken out and checked to confirm that its density distribution is uniform.

[0015] S4, sintering stage:

[0016] Finally, the pressed blank is directly transferred to the sintering furnace for high-temperature sintering treatment; the sintered blank needs to undergo quality inspection to confirm that its various performance indicators meet the established standards before it can be considered a finished product.

[0017] Preferably, the pre-pressing size is 0%-60% of the pressing size.

[0018] Preferably, the dimensions of the pressed blank and the sintered blank after sintering in the sintering process are A→A1, B→B1 with a shrinkage ratio of 1.2, and C→C1 with a shrinkage ratio of 1.4.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The present invention aims at maintaining a constant pressure of a pressing head on a press during the magnetization process in the manufacture of NdFeB sintered blanks, thereby effectively preventing the displacement of powder particles during the magnetization process. This method is not only applicable to NdFeB sintered blanks of all specifications, but is also particularly applicable to small-sized cylindrical products, and can control the grinding rate of the product to below 10%.

[0021] At the same time, the cylinders, blocks and special-shaped blanks produced by this technology can remain in a deformation-free state, thereby significantly reducing the grinding rate of the products and achieving substantial cost savings. Due to the improvement in the uniformity of the blank density, the isostatic pressing process is eliminated, which not only saves the isostatic pressing equipment and its related personnel costs, but also further reduces the overall production cost.

[0022] Under the current background that rare earth raw materials are becoming increasingly precious and scarce, this innovative method for producing deformation-free NdFeB sintered blank magnets has shown broad application prospects and huge market potential. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a schematic diagram of the pressing die and pre-pressing position of the present invention;

[0024] Figure 2It is a schematic diagram of the pressed powder of the present invention;

[0025] Figure 3 It is a schematic diagram of the pressed blank of the present invention;

[0026] Figure 4 It is a schematic diagram of the sintered blank of the present invention.

[0027] Figures: 1. Upper pressure head; 2. Powder; 3. Mould frame; 4. Lower pressure head; 5. Lower oil cylinder of press machine; 6. Connecting piece between lower pressure head and lower oil cylinder; 7. Workbench; 8. Left and right magnetizing pole heads; 9. Connecting piece between upper pressure head and lower oil cylinder; 10. Upper oil cylinder of press machine; 11. Pressed blank; 12. Sintered blank. a refers to pre-pressing size; b refers to the distance from the upper pressure head to the end of pressing; c refers to pressing size; d refers to the diameter of magnetizing pole head. DETAILED DESCRIPTION

[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] refer to Figure 1-Figure 4 As shown, a device for sintering a non-deformed NdFeB blank magnet comprises a workbench 7, an upper drive assembly and a lower drive assembly, wherein the upper drive assembly comprises an upper pressure head 1, a connection piece 9 between the upper pressure head and the lower oil cylinder and an upper oil cylinder 10 of a press; the lower drive assembly comprises a lower pressure head 4, a lower oil cylinder 5 of the press and a connection piece 6 between the lower pressure head and the lower oil cylinder, a fixing groove is provided on the middle surface of the workbench 7, a mold frame 3 is provided on the upper surface of the workbench 7, left and right magnetizing pole heads 8 are provided on both sides of the mold frame 3, the lower pressure head 4 is inserted into the inner side of the mold frame 3, and a powder 2 is provided on the inner side of the mold frame 3

[0030] A method for manufacturing a deformation-free NdFeB sintered blank magnet comprises the steps of pre-pressing, magnetizing, pressing and sintering.

[0031] The pre-pressing process refers to starting magnetization when the designed pre-pressing size is reached; during the magnetization process, the pressure of the upper ram of the press is maintained so that the powder particles do not move during magnetization and can only rotate at their position; after magnetization, the pressing process begins: the upper ram of the press continues to pressurize, and the pressing reaches the pressing size, and the pressed blank is taken out. The density of the pressed blank is uniform, and the pressing is completed; the pressed blank is sent to the sintering furnace for sintering. The sintering process is the same as the traditional process. The shrinkage ratio in the A→A1 and B→B1 directions is 1.2, and the shrinkage ratio in the C→C1 direction is 1.4. Among them, A and A1 refer to the length direction of the product; B and B1 refer to the width direction of the product; C and C1 refer to the orientation direction of the product. a refers to the pre-pressing size; b refers to the distance from the upper ram pre-pressing to the end of pressing; c refers to the pressing size.

[0032] Embodiment 1:

[0033] The cylindrical specification is φ5mm*20mm (the designed sintered blank size is φ5.1mm*20.2mm), the diameter shrinkage ratio is 1.2, and the height (orientation) shrinkage ratio is 1.4. The die pressure head diameter is 6.1mm, the height is 28.3mm, the pressing size is 6.1mm, the pre-pressing size is 3mm, and the pre-pressing is magnetized after the pre-pressing is in place, and the upper pressure head is pressed to the pressing size. The actual sintering size is φ5.06mm-φ5.1mm. The grinding rate is 2.4%-4.0%.

[0034] Embodiment 2:

[0035] The cylindrical specification is φ10mm*34mm (the designed sintered blank size is φ10.1mm*34.2mm), the diameter shrinkage ratio is 1.2, and the height (orientation) shrinkage ratio is 1.4. The die pressure head has a diameter of 12.1mm, a height of 48mm, a pressing size of 12.1mm, and a pre-pressing size of 6mm. After the pre-pressing is in place, magnetization is performed, and the upper pressure head is pressed to the pressing size. The actual sintering size is φ10.08mm-φ10.14mm. The grinding rate is 1.6%-2.8%.

[0036] Embodiment 3:

[0037] The cylindrical specification is φ16mm*30mm (the designed sintered blank size is φ16.1mm*30.2mm), the diameter shrinkage ratio is 1.2, and the height (orientation) shrinkage ratio is 1.4. The die pressure head diameter is 19.3mm, the height is 42.3mm, the pressing size is 19.3mm, the pre-pressing size is 9mm, and the pre-pressing is magnetized after the pre-pressing is in place, and the upper pressure head is pressed to the pressing size. The actual sintering size is φ16.1mm-16.16mm. The grinding rate is 1.2%-2.0%.

[0038] Embodiment 4:

[0039] The cylindrical specification is φ26mm*34mm (the designed sintered blank size is φ26.1mm*34.2mm), the diameter shrinkage ratio is 1.2, and the height (orientation) shrinkage ratio is 1.4. The die pressure head has a diameter of 31.3mm, a height of 48mm, a pressing size of 31.3mm, and a pre-pressing size of 15mm. After the pre-pressing is in place, magnetization is performed, and the upper pressure head is pressed to the pressing size. The actual sintering size is φ26.12mm-φ26.18mm. The grinding rate is 0.9%-1.4%.

[0040] Embodiment 5:

[0041] The cylindrical specification is φ50mm*30mm (the designed sintered blank size is φ50.2mm*30.3mm), the diameter shrinkage ratio is 1.2, and the height (orientation) shrinkage ratio is 1.4. The die pressure head diameter is 60.2mm, the height is 42.4mm, the pressing size is 60.2mm, the pre-pressing size is 30mm, and the pre-pressing is magnetized after the pre-pressing is in place, and the upper pressure head is pressed to the pressing size. The actual sintering size is φ50.16mm-φ50.28mm. The grinding rate is 0.6%-1.1%.

[0042] Embodiment 6:

[0043] The block size is 40mm*35mm*33mm (the designed sintered blank size is 40.1mm*35.1mm33.2mm), the shrinkage ratio in the A and C directions is 1.2, and the shrinkage ratio in the B direction (orientation) is 1.4. The pressing size is 42.1mm, the pre-pressing size is 21mm, and the magnetization is performed after the pre-pressing is in place, and the upper pressing head is pressed to the pressing size. The actual sintering size is 40.08mm--40.16mm*35.1mm—35.22mm*33.2mm—33.3mm. The grinding rate is 1.1%--1.9%.

[0044] Embodiment 7:

[0045] Block size is 52mm*52mm*33mm (designed sintered blank size is 52.1mm*52.1mm33.2mm), shrinkage ratio in A and C directions is 1.2, shrinkage ratio in B direction (orientation) is 1.4. Pressing size is 62.5mm, pre-pressing size is 31mm, magnetization is performed after pre-pressing, and the upper pressing head is pressed to the pressing size. The actual sintering size is 52.1mm--52.18mm*52.12mm--52.2mm*33.2mm—33.3mm. Grinding rate is 1.0%--1.6%.

[0046] Embodiment 8:

[0047] Block size is 62mm*40mm*32mm (designed sintered blank size is 62.1mm*40.1mm32.2mm), shrinkage ratio in A and C directions is 1.2, and shrinkage ratio in B direction (orientation) is 1.4. Pressing size is 48.1mm, pre-pressing size is 24mm, magnetization is performed after pre-pressing, and the upper press head is pressed to the pressing size. The actual sintering size is 62.1mm—62.18mm*40.08mm—40.12mm*32.2mm—32.3mm. Grinding rate is 1.0%--1.5%.

[0048] Embodiment 9:

[0049] The block size is 83mm*63mm*20mm (the designed sintered blank size is 83.2mm*63.2mm20.3mm), the shrinkage ratio in the A and C directions is 1.2, and the shrinkage ratio in the B direction (orientation) is 1.4. The pressing size is 75.8mm, the pre-pressing size is 37mm, and the magnetization is performed after the pre-pressing is in place, and the upper pressing head is pressed to the pressing size. The actual sintering size is 83.24mm—83.3mm*63.18mm—63.3mm*20.2mm—20.28mm. The grinding rate is 1.6%--2.3%.

[0050] Embodiment 10:

[0051] The block size is 100mm*45mm*30mm (the designed sintered blank size is 100.2mm*45.2mm30.2mm), the shrinkage ratio in the A and C directions is 1.2, and the shrinkage ratio in the B direction (orientation) is 1.4. The pressing size is 54.2mm, the pre-pressing size is 27mm, and the magnetization is performed after the pre-pressing is in place, and the upper pressing head is pressed to the pressing size. The actual sintering size is 100.2mm—100.3mm*45.12mm—45.2mm*30.18mm—30.26mm. The grinding rate is 1.1%--1.6%.

[0052] The above embodiments are specifically shown in Table 1:

[0053] Table 1

[0054]

[0055]

[0056] The products produced by the current NdFeB magnet preparation process, such as cylindrical, square and special-shaped products, will have different degrees of deformation, and the product grinding rate is relatively high.

[0057] The most critical part of the present invention is the method of pre-pressing powder. Pre-pressing starts from the time when the upper pressure head enters the upper surface of the mold frame. Among them, magnetization is carried out after the pre-pressing size is in place, and pre-pressing means that the powder is poured into the mold frame in a loose state, and the gap between the powder particles is large. As the upper pressure head continues to press in, the gap between the powder particles gradually decreases. Due to the different particle sizes of the powder, the pre-pressing size will also be different. When the pre-pressing size is reached, the powder particles in the mold frame only rotate in the original position without moving, and the pressed blank produced will not be deformed.

[0058] The sintered blank produced by the method of the present invention has a good appearance and no deformation, and the grinding rate can be controlled below 10%. Since the density of the pressed blank is uniform, the isostatic pressing process is omitted, the magnetic powder utilization rate is high, the process flow is short, the cost is reduced, the benefit is high, the market is wide, and it has good market value.

[0059] This method is not only applicable to all specifications of NdFeB sintered blanks, but is also particularly suitable for small-sized cylindrical products (diameter range φ3-φ10), and can control the grinding rate of the products to below 10%.

[0060] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A device for sintering a deformation-free NdFeB blank magnet, characterized in that: The invention comprises a workbench (7), an upper driving assembly and a lower driving assembly, wherein the upper driving assembly comprises an upper pressing head (1), a connecting piece (9) between the upper pressing head and the lower oil cylinder and an upper oil cylinder (10) of a press; the lower driving assembly comprises a lower pressing head (4), a lower oil cylinder (5) of a press and a connecting piece (6) between the lower pressing head and the lower oil cylinder, a fixing groove is provided on the middle surface of the workbench (7), a mold frame (3) is provided on the upper surface of the workbench (7), left and right magnetizing pole heads (8) are provided on both sides of the mold frame (3), the lower pressing head (4) is inserted into the inner side of the mold frame (3), and powder (2) is provided on the inner side of the mold frame (3).

2. A method for producing a deformation-free NdFeB sintered blank magnet, characterized in that: The following steps are involved: S1, pre-pressing stage: First, the press is started and the upper pressure head (1) of the mold is assembled, and then the powder (2) is evenly poured into the mold frame (3). The powder (2) is arranged between the upper pressure head (1) and the lower pressure head (4). A scraper tool is used to ensure that the surface of the powder is flush with the upper edge of the mold frame (3) to eliminate unevenness. The powder is neodymium iron boron powder; the mold frame (3) is arranged on a workbench (7), and a through hole is opened in the middle of the workbench (7). Next, the upper pressing head (1) of the mold is slowly pre-pressed into the mold frame (3) until a preset pre-pressing size is reached, and magnetization begins; left and right magnetizing pole heads (8) are provided at the left and right ends of the mold frame (3), and the left and right magnetizing pole heads (8) are electrically connected to conductive wires; the upper pressing head (1) is connected to the upper oil cylinder (10) of the press through the upper pressing head and lower oil cylinder connecting piece (9), and the lower pressing head (4) is connected to the lower oil cylinder (5) of the press through the lower pressing head and lower oil cylinder connecting piece (6); S2, magnetization stage: After the pre-pressing size is in place, magnetization is performed. During this process, the pressure of the pressing head (1) on the press is maintained constant. The magnetic field generated at the beginning of magnetization is transmitted to the powder by clamping the left and right magnetizing pole heads (8) to magnetize the powder. During the magnetization process, the powder particles will not move in position, but rotate in the original position to ensure the stability of the magnet structure. S3, Suppression stage: After the magnetization is completed, the pressing process begins immediately. The pressing head (1) on the press continues to increase the pressure until the predetermined pressing size is reached. After the pressing is completed, the blank (11) is taken out to check and confirm that its density distribution is uniform. S4, sintering stage: Finally, the pressed blank (11) is directly transferred to a sintering furnace for high-temperature sintering. The sintered blank needs to undergo quality inspection to confirm that all performance indicators meet the established standards and is considered a finished sintered blank (12).

3. The method for manufacturing a deformation-free NdFeB sintered blank magnet according to claim 2, characterized in that: The pre-pressing size is 0%-60% of the pressing size.

4. The method for manufacturing a deformation-free NdFeB sintered blank magnet according to claim 2, characterized in that: The dimensions of the pressed blank (11) and the sintered blank (12) after sintering are A→A1, B→B1 with a shrinkage ratio of 1.2, and C→C1 with a shrinkage ratio of 1.4.

Citation Information

Cited By

  • Method for improving one-time forming rate of large-size neodymium iron boron product and rapid verification device

    CN122252603A