Method for preparing nitrogen-doped electrode material by coupling pyrolytic oil rich in nitrogen compound with MOFs template method

By combining fungal pretreatment and MOFs template method, nitrogen-doped electrode materials were prepared, which solved the problems of poor thermal stability of pyrolysis oil and high cost of heteroatom doping, and achieved efficient utilization of biomass and high environmental protection. Conversion.

CN118919309APending Publication Date: 2024-11-08SHANDONG UNIV OF TECH

Patent Information

Application Number
CN202410960440.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the existing biomass pyrolysis technology, the thermal stability of the pyrolytic oil is poor and easy to form coke, and the cost of heteroatom doping is high, resulting in equipment corrosion and blockage problems, affecting the efficient utilization of biomass and environmental friendliness.

Method used

Using fungal pretreatment of biomass, the preparation of nitrogen-rich pyrolysis oils and MOFs template method is combined to prepare nitrogen-doped electrode materials, and the quality of pyrolysis oils and nitrogen are improved by using magnetic stirring and non-in-situ pyrolysis technology. Pore ​​structure of doped carbon materials.

Benefits of technology

It significantly improves the thermal stability of pyrolytic oil and the specific capacitance and cyclic stability of nitrogen-doped carbon materials, reduces the negative environmental impact of the activation process, realizes efficient utilization and high-value conversion of biomass, and meets the requirements of circular economy. .

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of biomass pyrolysis, and particularly relates to a method for preparing a nitrogen-doped electrode material by coupling pyrolytic oil rich in nitrogen compounds with an MOFs template method. The preparation method comprises the following steps: carrying out fungus pretreatment on biomass, dipping in a nitrogen-containing solution to prepare nitrogen-containing biomass, and carrying out ex-situ pyrolysis on the nitrogen-containing biomass and a catalyst to prepare pyrolytic oil rich in nitrogen compounds and biochar, pyrolysis oil rich in nitrogen compounds, biochar, a metal organic framework compound and a template agent are subjected to carbonization treatment, a nitrogen-doped carbon material is prepared and obtained, the nitrogen-doped carbon material is subjected to acid pickling to remove the template agent and activated by an activating agent, activated nitrogen-doped biochar is prepared and obtained, and finally the activated nitrogen-doped biochar is used for electrode preparation. According to the method for preparing the nitrogen-doped electrode material by coupling the pyrolytic oil rich in the nitrogen compound with the MOFs template method, efficient utilization of biomass can be realized, and the method has a wide application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of biomass pyrolysis, and specifically relates to a method for preparing nitrogen-doped electrode materials by coupling pyrolysis oil rich in nitrogen compounds with a MOFs template method. Background Art

[0002] The chemical connection and physical arrangement between cellulose, hemicellulose and lignin in biomass hinder the utilization of biomass and greatly affect the pyrolysis behavior of biomass. Pretreatment can improve the pyrolysis process of biomass and increase the selectivity of pyrolysis products. Common biomass pretreatment methods mainly include physical methods (such as densification, grinding, etc.), chemical methods (such as acid, alkali, hydrothermal, steam explosion, etc.), and biological methods (such as bacteria, enzymes, fungi, etc.).

[0003] Compared with physical and chemical pretreatment, biological pretreatment of lignocellulosic biomass is considered to be one of the most economical and environmentally friendly treatment methods. Biological pretreatment technology has many advantages such as mild conditions, low cost, energy saving and environmental friendliness. Fungi can deconstruct and depolymerize the stubborn bonds of lignin and cellulose, making the structure of biomass loose and easier to pyrolyze. Among them, fungal pretreatment reduces the activation energy and reaction temperature of pyrolysis, thereby greatly reducing the difficulty of biomass pyrolysis reaction. On the other hand, biological pretreatment can reduce sulfur content, which is helpful for reducing SO x Emissions are important.

[0004] Biomass is the only renewable carbon source in nature, and its clean, cheap and easily accessible properties make it a carbon precursor with great potential. Pyrolysis oil is a liquid product of thermal conversion of biomass with high content of carbon and oxygen. Compared with primary biomass, the liquid form is more conducive to regulating the carbon structure because pyrolysis oil can form an ordered porous structure without being restricted by the natural biological structure. It is worth noting that the mixing method of the template and the precursor significantly affects the structural properties. MOFs can be used to synthesize materials with catalytic activity. For example, MOFs-derived metal oxide catalysts show excellent performance in organic catalytic reactions. Pyrolysis oil can be uniformly mixed with the template in solution, which can achieve higher specific surface area and specific pore size.

[0005] The N element present in biochar can provide pseudocapacitance, improve the wettability and conductivity of porous carbon, enable the electrolyte to better infiltrate the electrode material, thereby reducing the resulting resistance, further improving the specific capacitance of the multi-electrode material, and at the same time having good chemical stability. Some studies have shown that biochar electrodes treated with nitrogen doping can obtain higher capacitance and better cycle stability than traditional electrodes. In addition, nitrogen-doped biochar can also be used in combination with other materials, such as metal oxides, polymers, and carbon nanotubes, to achieve better supercapacitor performance.

[0006] For example, in CN109574007A, a porous carbon material with high specific surface area is prepared by fungal pretreatment, and a porous carbon material is prepared by fungal treatment and regulation, so that waste biomass is effectively utilized, the preparation process is simple, the production cost is low, and it is environmentally friendly, and microporous, mesoporous or micro-mesoporous porous carbon materials can be obtained. For example, in CN114613612A, a carbon material is prepared by pyrolysis oil obtained by catalytic pyrolysis of biomass. The carbon material has very excellent specific capacitance and can be used to prepare heteroatom-doped carbon electrode materials, thereby improving the energy density of supercapacitors.

[0007] However, the existing activation and modification treatment methods still have some problems, such as poor thermal activation effect, environmental pollution caused by the high oxygen content of pyrolysis oil after disposal, and high heteroatom doping cost; and most of the pyrolysis oil in the carbonization process has high water and oxygen content, which easily leads to equipment corrosion and blockage problems, so the produced pyrolysis oil is discarded.

[0008] Therefore, it is of great significance to study an environmentally friendly and efficient pretreatment and charcoal making method to improve the quality of pyrolysis oil and nitrogen-doped charcoal materials in order to achieve high-value conversion of biomass. Summary of the invention

[0009] The purpose of the present invention is to provide a method for preparing nitrogen-doped electrode materials by coupling pyrolysis oil rich in nitrogen compounds with MOFs template method. This method can not only realize the efficient utilization of biomass, but also overcome the drawbacks existing in the current preparation process of nitrogen-containing chemicals.

[0010] The method for preparing nitrogen-doped electrode materials by coupling nitrogen-rich compound pyrolysis oil with MOFs template method of the present invention comprises the following steps:

[0011] (1) crushing the biomass to obtain crushed biomass;

[0012] (2) mixing the crushed biomass prepared in step (1) with water and sterilizing it, then inoculating it with a fungal inoculum for pretreatment, and finally washing it with water to remove the hyphae on the surface of the pretreated biomass, drying it, grinding it and screening it, so as to prepare a biomass raw material;

[0013] (3) immersing the biomass raw material prepared in step (2) in a nitrogen-containing solution, performing magnetic stirring, and then filtering and drying to prepare nitrogen-containing biomass;

[0014] (4) subjecting the nitrogen-containing biomass prepared in step (3) to non-in-situ pyrolysis with a catalyst in an oxygen-free atmosphere, and collecting the volatile matter through a condensation system to obtain pyrolysis oil rich in nitrogen compounds, and the remaining solid is biochar produced by the primary pyrolysis;

[0015] (5) mixing the nitrogen compound-rich pyrolysis oil in step (4), the biochar produced by the primary pyrolysis, the metal organic framework compound (MOFs) and the template by magnetic stirring, and then carbonizing the mixture to prepare a nitrogen-doped carbon material;

[0016] (6) acid washing the nitrogen-doped carbon material prepared in step (5) to remove the template, then washing with water until neutral, and drying to obtain inactivated nitrogen-doped biochar;

[0017] (7) mixing the unactivated nitrogen-doped biochar of step (6) with an activating agent for activation treatment to prepare activated nitrogen-doped biochar;

[0018] (8) The activated nitrogen-doped biochar, the conductive material and the polytetrafluoroethylene solution prepared in step (7) are uniformly mixed, and then anhydrous ethanol is added for demulsification to obtain a mixture, and the mixture is coated on a carrier, and then dried, compacted and baked to obtain an electrode.

[0019] in:

[0020] The biomass in step (1) is one or more of crop straw, fruit shell, leaves, bark, aquatic plants or algae; wherein the crop straw is one or more of corn straw, wheat straw, soybean straw, cotton straw or pea straw; and the fruit shell is one or more of walnut shell, peanut shell or coconut shell.

[0021] The particle size of the crushed biomass obtained in step (1) is 40-80 meshes.

[0022] The sterilization treatment in step (2) is performed at 120° C. for 15 min and a pressure of 0.12 MPa.

[0023] In step (2), the fungus is first activated at 28-30° C. for 8-10 days, the generated mycelium is washed with sterile water, filtered and supplemented with sterile water, and homogenized using a vortex oscillator to prepare a fungal inoculum, wherein the fungus is one or more of Trichoderma koningii, Aspergillus niger, Aspergillus kawachii, white rot fungus Trametes versicolor, brown rot fungus or Phanerochaete chrysosporium, preferably Phanerochaete chrysosporium.

[0024] In step (2), the mass ratio of the crushed biomass prepared in step (1) to water is 1:1-1:4.

[0025] The pretreatment in step (2) is carried out in an incubator at 28°C for 7-14 days.

[0026] In step (2), the drying temperature is 105° C. and the drying time is 12-24 hours.

[0027] The amount of the crushed biomass and the fungal inoculum in step (2) is 20-50:6-10, in units of g / mL.

[0028] In step (2), the biomass raw material powder with a size of 60-100 mesh is ground and sieved.

[0029] The nitrogen-containing solution in step (3) is one of ammonia water, urea solution, aniline solution, dicyandiamide solution or melamine solution, and the mass concentration of the nitrogen-containing solution is 1-30%, preferably 20%.

[0030] In step (3), the mass volume ratio of the biomass raw material to the nitrogen-containing solution is 2-4:50-100, in units of g / mL.

[0031] In step (3), the magnetic stirring temperature is room temperature and the magnetic stirring time is 5-10 h.

[0032] In step (3), the drying temperature is 90-105° C. and the drying time is 12-48 hours.

[0033] In step (4), the mass ratio of nitrogen-containing biomass to catalyst is 5:1-6.

[0034] The catalyst in step (4) is one or more of a ZSM-5 molecular sieve catalyst, a MCM-41 molecular sieve catalyst or a ZIF-67 catalyst.

[0035] The oxygen-free atmosphere in step (4) is one of argon, nitrogen, carbon dioxide or ammonia or a mixture thereof.

[0036] The non-in-situ pyrolysis in step (4) is to place the nitrogen-containing biomass and the catalyst in the same quartz boat respectively, separate the nitrogen-containing biomass and the catalyst with quartz wool, heat the temperature to the pyrolysis temperature at a heating rate of 5-10°C / min, and then push the quartz boat to the heating section of the pyrolysis reactor for pyrolysis, the pyrolysis temperature is 400-600°C, and the pyrolysis time is 5-20min.

[0037] The condensation temperature of the condensation system in step (4) is -10-20°C.

[0038] The nitrogen compound-rich pyrolysis oil component in step (4) contains nitrogen-containing compounds such as pyridines, pyrroles, nitriles, amines, hydrazines and pyrazines, and the total nitrogen-containing compounds account for 50-90% of the pyrolysis oil.

[0039] In step (5), the mass ratio of the nitrogen compound-rich pyrolysis oil, the biochar produced by the primary pyrolysis, the metal organic framework compound (MOFs), and the template agent is 1:1-2:0.2-1:1-3.

[0040] In step (5), the metal organic framework compound (MOFs) is one or more mixtures of MOF-5, MOF-74, HKUST-1, ZIF-8, ZIF-67, MIL-100 (Cr), MIL-125, UiO-66 and NU-110.

[0041] In step (5), the magnetic stirring time is 12-24 hours, and the magnetic stirring temperature is room temperature.

[0042] In step (5), the carbonization treatment is to transfer the mixture to a quartz boat, heat it to 700-900°C at a heating rate of 5-10°C / min for carbonization, and the carbonization time is 1-2h. The carbonization atmosphere is one of argon, nitrogen or ammonia or a mixture thereof.

[0043] The template in step (5) is one of magnesium hydroxide, zinc hydroxide or calcium hydroxide.

[0044] The acid used for pickling in step (6) is one of nitric acid, hydrochloric acid or sulfuric acid.

[0045] In step (6), the acid and nitrogen-doped carbon material are magnetically stirred at room temperature for 1-10 hours, the molar ratio of the acid to the template is 1-1.2:1, and then washed with water to neutrality, and dried at 80-110° C. for 6-12 hours to obtain unactivated nitrogen-doped biochar.

[0046] In step (7), the mass ratio of the unactivated nitrogen-doped biochar to the activating agent is 2:1-4.

[0047] In step (7), the activator is one or more of zinc chloride, potassium hydroxide, sodium hydroxide or potassium oxalate.

[0048] In step (7), the activation treatment is performed by heating to 700-900°C at a heating rate of 5-10°C / min, and then keeping the temperature for 0.5-5 hours.

[0049] In step (8), the carrier is one of nickel mesh, titanium mesh or stainless steel mesh; the conductive material is at least one of acetylene black or graphene; and the mass fraction of the polytetrafluoroethylene solution is 5%.

[0050] In step (8), the mass ratio of activated nitrogen-doped biochar, conductive material and polytetrafluoroethylene solution is 8:1:1, and the volume ratio of polytetrafluoroethylene solution to anhydrous ethanol is 1:1.6.

[0051] In step (8), the drying temperature is 80-83°C, the drying time is 1 hour, the compaction pressure is 20 MPa, the drying temperature is 70-75°C, and the drying time is 12 hours.

[0052] Compared with the prior art, the present invention has the following beneficial effects:

[0053] (1) The method of preparing nitrogen-doped electrode materials by coupling pyrolysis oil rich in nitrogen compounds with MOFs template method described in the present invention affects the quality of pyrolysis oil and biochar through biological pretreatment, solves the problem that pyrolysis oil has poor thermal stability and is easy to form coke, provides a new pyrolysis oil conversion and utilization mode and a method for preparing porous carbon materials, which realizes the efficient utilization of biomass waste.

[0054] (2) The method of preparing nitrogen-doped electrode materials by coupling nitrogen-rich pyrolysis oil with MOFs template method described in the present invention uses biological pretreatment of biomass, which has a significant impact on the physical and chemical properties and pyrolysis behavior of biomass. The selected fungi can selectively degrade hemicellulose and lignin in biomass, significantly changing the physical and chemical properties of biomass. After fungal pretreatment, a large number of pore structures appear on its surface. Fungal pretreatment improves the pyrolysis process of biomass, and the pyrolysis activation energy gradually decreases with the increase of pretreatment time. Biomass pretreated with fungi can be converted into high-quality doped carbon, which has a wide range of application potentials, such as the preparation of catalysts, activated carbon and electrode materials.

[0055] (3) The method for preparing nitrogen-doped biochar by biological pretreatment of biomass described in the present invention, the nitrogen-doped biochar prepared by fungal pretreatment, under the action of an activator, has a significantly increased specific surface area, and the pore structure of the nitrogen-doped porous carbon material is mainly micropores, with a small amount of mesopores and macropores, and partial pseudocapacitance is introduced. The nitrogen-doped carbon material prepared after fungal pretreatment has good cycle stability and improved electrochemical performance.

[0056] (4) The method for preparing nitrogen-doped electrode materials by coupling nitrogen-rich pyrolysis oil with MOFs template method described in the present invention, fungal pretreatment gradually increases the relative content of furfural in the pyrolysis oil, and after impregnation with nitrogen-containing solution, the enrichment of nitrogen-containing chemicals in the nitrogen-rich pyrolysis oil is promoted, thereby realizing the high-value utilization of waste resources. Impregnation with nitrogen-rich pyrolysis oil can effectively reduce the negative impact on the environment and the consumption of energy and resources during the activation process, utilize biomass resources, avoid the environmental problems caused by open-air incineration of biomass, and meet the strategic requirements of circular economy and conservation-oriented society.

[0057] (5) The method of preparing nitrogen-doped electrode materials by coupling nitrogen-rich compound pyrolysis oil with MOFs template method described in the present invention can not only realize the efficient utilization of biomass, but also overcome the drawbacks existing in the current preparation process of nitrogen-containing chemicals, and has broad application prospects.

[0058] (6) In the method for preparing nitrogen-doped electrode materials by coupling nitrogen-rich pyrolysis oil with MOFs template method described in the present invention, the carbon material has been preliminarily carbonized and nitrogen-enriched in the initial carbonization process. The obtained nitrogen-rich pyrolysis oil, metal organic framework compound (MOFs), template agent and biochar material produced by the primary pyrolysis are mixed and carbonized for a secondary time, which will cause the amine substances in the pyrolysis oil to cross-polymerize with the carbon material to produce a carbon material with a higher content. DETAILED DESCRIPTION

[0059] The present invention is further described below with reference to the embodiments.

[0060] Example 1

[0061] The method for preparing nitrogen-doped electrode materials by coupling nitrogen-rich compound pyrolysis oil with MOFs template method described in Example 1 comprises the following steps:

[0062] (1) The collected corn stalks are crushed and sieved using a crusher to obtain corn stalk powder with a particle size of 60 mesh.

[0063] (2) First, activate P. chrysosporium at 29°C for 9 days, wash the generated mycelium with water, filter and add sterile water to 50 mL, and use a vortex oscillator to homogenize the fungal spore inoculum for later use. Put 20g corn straw powder and 50mL of water into a triangular bottle, seal it with a breathable sealing film, and sterilize it at 120°C for 15min at a pressure of 0.12MPa. In the clean bench, inoculate 10mL of homogenized fungal inoculum in each sterilized triangular bottle, place it in a 28°C incubator for 2 weeks, wash the pretreated corn straw powder repeatedly with water to remove the surface mycelium, and then dry it at 105°C for 16 hours, grind and sieve to select 80 mesh, put it into a sample bag, and store it in a desiccator for later use.

[0064] (3) First, a urea solution was prepared, and the mass concentration of the urea solution was controlled to be 8%. The biomass raw material after fungal pretreatment was immersed in the urea solution, that is, 20 g of corn straw powder raw material was added to 500 mL of urea solution, and magnetic stirring was performed at room temperature for 8 hours, and then filtered, and placed in a drying oven at 105° C. for 12 hours to prepare nitrogen-containing biomass.

[0065] (4) The nitrogen-containing biomass and the ZIF-67 molecular sieve catalyst (Nanjing Jichang Nanotechnology Co., Ltd.) were weighed out according to a mass ratio of 5:1, and placed in the same quartz boat respectively. The nitrogen-containing biomass and the ZIF-67 molecular sieve catalyst were separated by quartz wool. The temperature was raised to the pyrolysis temperature at a heating rate of 10°C / min, and then the quartz boat was pushed to the heating section of the pyrolysis reactor for pyrolysis. The pyrolysis atmosphere was argon, the pyrolysis temperature was 500°C, and the pyrolysis time was 10 min. The volatile matter was condensed and collected by a condensation system to obtain a pyrolysis oil rich in nitrogen compounds (9.8% pyridines, 36.2% pyrroles, 6.2% nitriles, 17.9% amines, 5.6% hydrazines and 2.6% pyrazines) (the condensation temperature of the condensation system was -10°C), and the remaining solid was the biochar produced by the primary pyrolysis.

[0066] (5) The nitrogen compound-rich pyrolysis oil in step (4), the biochar produced by the primary pyrolysis, the ZIF-67 molecular sieve catalyst (Nanjing Jichang Nanotechnology Co., Ltd.) and the template (magnesium hydroxide) are magnetically stirred and mixed, the magnetic stirring time is 12 hours, and the magnetic stirring temperature is room temperature, wherein the mass ratio of the nitrogen compound-rich pyrolysis oil, the biochar produced by the primary pyrolysis, the ZIF-67 molecular sieve catalyst (Nanjing Jichang Nanotechnology Co., Ltd.) and the template (magnesium hydroxide) is 1:1:1:1; then the mixture is transferred to a quartz boat, and the temperature is increased to 800°C at a heating rate of 8°C / min for carbonization, the carbonization time is 1.5 hours, and the carbonization atmosphere is argon to prepare a nitrogen-doped carbon material.

[0067] (6) The obtained product was acid-washed with nitric acid; the molar ratio of the acid to the template was 1:1, and magnetic stirring was performed at room temperature for 10 hours. The carbonized product was then washed with water to remove impurities such as the template, washed to neutrality, and then dried at 95°C for 9 hours to obtain inactivated nitrogen-doped biochar.

[0068] (7) The unactivated nitrogen-doped biochar obtained in step (6) was mixed with potassium oxalate in a mass ratio of 1:1 and placed in a quartz boat for activation treatment. The activation treatment conditions were heating to 700°C at a heating rate of 8°C / min and maintaining at this temperature for 2.5 hours to prepare activated nitrogen-doped biochar.

[0069] (8) The activated nitrogen-doped biochar, graphene, and polytetrafluoroethylene solution (the mass concentration of the polytetrafluoroethylene solution is 5%) are mixed uniformly in a mass ratio of 8:1:1, and then anhydrous ethanol is added for demulsification. The ratio of the polytetrafluoroethylene solution to anhydrous ethanol is 1:1.6 to obtain a mixture; the mixture is coated on a nickel mesh (size is 1 cm×1 cm), placed in a constant temperature drying oven at 82°C for 1 hour, and then pressed at a pressure of 20 MPa. After pressing, the tablets are continued to be dried at a drying temperature of 73°C and a drying time of 12 hours to obtain an electrode.

[0070] Example 2

[0071] The method for preparing nitrogen-doped electrode materials by coupling nitrogen-rich compound pyrolysis oil with MOFs template method described in Example 2 is composed of the following steps:

[0072] (1) The collected wheat straw is crushed by a crusher to obtain wheat straw powder with a particle size of 40 mesh.

[0073] (2) First, activate P. chrysosporium at 28°C for 10 days, wash the generated mycelium with water, filter and add sterile water to 50 mL, and use a vortex oscillator to homogenize the fungal spore inoculum for later use. Put 20g of wheat straw powder and 20mL of water into a triangular flask, seal it with a breathable sealing film, and sterilize it at 120°C for 15min at a pressure of 0.12MPa. In the clean bench, inoculate 6mL of homogenized fungal inoculum in each sterilized triangular flask, place it in a 28°C incubator for 7 days, wash the pretreated wheat straw powder repeatedly with water to remove the surface mycelium, and then dry it at 105°C for 12 hours, grind and sieve to select 60 mesh, put it into a sample bag, and store it in a desiccator for later use.

[0074] (3) First, an aniline solution is prepared, and the mass concentration of the aniline solution is controlled to be 20%. The biomass raw material pretreated with fungi is immersed in the aniline solution, that is, 20 g of wheat straw powder raw material is added to 800 mL of aniline solution, and magnetic stirring is performed at room temperature for 10 hours, and then the mixture is filtered and placed in a drying oven at 100° C. for 30 hours to prepare nitrogen-containing biomass.

[0075] (4) The above-mentioned nitrogen-containing biomass and MCM-41 molecular sieve catalyst (Jiangsu Xianfeng Nanomaterial Technology Co., Ltd.) were weighed out according to a mass ratio of 5:3, and placed in the same quartz boat respectively. The nitrogen-containing biomass and the MCM-41 molecular sieve catalyst were separated by quartz wool. The temperature was raised to the pyrolysis temperature at a heating rate of 5°C / min, and then the quartz boat was pushed to the heating section of the pyrolysis reactor for pyrolysis. The pyrolysis atmosphere was nitrogen, the pyrolysis temperature was 600°C, and the pyrolysis time was 5 min. The volatile matter was condensed and collected by a condensation system to obtain a pyrolysis oil rich in nitrogen compounds (5.3% pyridines, 26.3% pyrroles, 3.2% nitriles, 12.6% amines, 2.6% hydrazines and 1.6% pyrazines). The condensation temperature of the condensation system was -10°C, and the remaining solid was the biochar produced by the primary pyrolysis.

[0076] (5) The nitrogen-rich pyrolysis oil, the biochar produced by the primary pyrolysis, ZIF-8 (Jiangsu Xianfeng Nanomaterial Technology Co., Ltd.) and the template (calcium hydroxide) in step (4) are magnetically stirred and mixed. The magnetic stirring time is 16 hours and the magnetic stirring temperature is room temperature. The mass ratio of the nitrogen-rich pyrolysis oil, the biochar produced by the primary pyrolysis, and the ZIF-8 template (calcium hydroxide) is 1:1.5:0.2:2. The mixture is then transferred to a quartz boat and heated to 900°C at a heating rate of 10°C / min for carbonization. The carbonization time is 1 hour and the carbonization atmosphere is nitrogen to prepare a nitrogen-doped carbon material.

[0077] (6) The obtained product was acid-washed, and the acid selected for acid washing was hydrochloric acid; the molar ratio of the acid to the template was 1.1:1. After magnetic stirring at room temperature for 5 hours, the carbonized product was washed with water to remove impurities such as the template, and then washed with water until neutral, and then dried at 80°C for 12 hours to obtain unactivated nitrogen-doped biochar.

[0078] (7) The unactivated nitrogen-doped biochar obtained in step (6) was mixed with zinc chloride in a mass ratio of 2:1 and placed in a quartz boat for activation treatment. The activation treatment conditions were heating to 800°C at a heating rate of 5°C / min and maintaining at this temperature for 5 hours to prepare activated nitrogen-doped biochar.

[0079] (8) The activated nitrogen-doped biochar, graphene, and polytetrafluoroethylene solution (the mass concentration of the polytetrafluoroethylene solution is 5%) are mixed uniformly in a mass ratio of 8:1:1, and then anhydrous ethanol is added for demulsification. The ratio of the polytetrafluoroethylene solution to anhydrous ethanol is 1:1.6 to obtain a mixture; the mixture is coated on a nickel mesh (size is 1 cm×1 cm), placed in a constant temperature drying oven at 80°C for 1 hour, and then pressed at a pressure of 20 MPa. After pressing, the tablets are continued to be dried at a drying temperature of 70°C and a drying time of 12 hours to obtain an electrode.

[0080] Example 3

[0081] The method for preparing nitrogen-doped electrode materials by coupling nitrogen-rich compound pyrolysis oil with MOFs template method described in Example 3 is composed of the following steps:

[0082] (1) The collected cotton stalks are crushed by a crusher to obtain cotton stalk powder with a particle size of 80 mesh.

[0083] (2) First, activate P. chrysosporium at 30°C for 8 days, wash the generated mycelium with water, filter and add sterile water to 50 mL, and use a vortex oscillator to homogenize the fungal spore inoculum for later use. Put 20g of cotton stalk powder and 80mL of water into a triangular flask, seal it with a breathable sealing film, and sterilize it at 120°C for 15min at a pressure of 0.12MPa. In the clean bench, inoculate 8mL of homogenized fungal inoculum in each sterilized triangular flask, place it in a 28°C incubator for 10 days, wash the pretreated cotton stalk powder repeatedly with water to remove the surface mycelium, and then dry it at 105°C for 24 hours, grind and sieve to select 100 mesh, put it into a sample bag, and store it in a desiccator for later use.

[0084] (3) First, a dicyandiamide solution is prepared, and the mass concentration of the dicyandiamide solution is controlled to be 30%. The biomass raw material pretreated with fungi is immersed in the dicyandiamide solution, that is, 20 g of cotton stalk powder raw material is added to 1000 mL of dicyandiamide solution, and magnetic stirring is performed at room temperature for 5 hours, and then the mixture is filtered and placed in a drying oven at 90° C. for 48 hours to prepare nitrogen-containing biomass.

[0085] (4) The nitrogen-containing biomass and the ZSM-5 molecular sieve catalyst (Jiangsu Xianfeng Nanomaterial Technology Co., Ltd.) were weighed out according to a mass ratio of 5:6, and placed in the same quartz boat respectively. The nitrogen-containing biomass and the ZSM-5 molecular sieve catalyst were separated by quartz wool. The temperature was raised to the pyrolysis temperature at a heating rate of 10°C / min, and then the quartz boat was pushed to the heating section of the pyrolysis reactor for pyrolysis. The pyrolysis atmosphere was ammonia, the pyrolysis temperature was 400°C, and the pyrolysis time was 20min. The volatile matter was condensed and collected by a condensation system to obtain a pyrolysis oil rich in nitrogen compounds (5.4% pyridines, 25.7% pyrroles, 3.6% nitriles, 13.4% amines, 1.9% hydrazines and 2.3% pyrazines) (the condensation temperature of the condensation system was -10°C), and the remaining solid was the biochar produced by the primary pyrolysis.

[0086] (5) The nitrogen compound-rich pyrolysis oil, the biochar produced by the primary pyrolysis, MOF-5 (Jiangsu Xianfeng Nanomaterial Technology Co., Ltd.) and the template (zinc hydroxide) in step (4) are magnetically stirred and mixed. The magnetic stirring time is 24 hours and the magnetic stirring temperature is room temperature. The mass ratio of the nitrogen compound-rich pyrolysis oil, the biochar produced by the primary pyrolysis, MOF-5 (Jiangsu Xianfeng Nanomaterial Technology Co., Ltd.) and the template (zinc hydroxide) is 1:2:0.6:3. The mixture is then transferred to a quartz boat and heated to 700°C at a heating rate of 5°C / min for carbonization. The carbonization time is 2 hours and the carbonization atmosphere is ammonia to prepare a nitrogen-doped carbon material.

[0087] (6) The obtained product was acid-washed, and the acid selected for acid washing was sulfuric acid; the molar ratio of the acid to the template agent was 1.2:1, and magnetic stirring was performed at room temperature for 1 hour. The carbonized product was then washed with water to remove impurities such as the template, and then washed with water until neutral, and then dried at 110°C for 6 hours to obtain unactivated nitrogen-doped biochar.

[0088] (7) The unactivated nitrogen-doped biochar obtained in step (6) was mixed with sodium hydroxide in a mass ratio of 1:2 and placed in a quartz boat for activation treatment. The activation treatment conditions were heating to 900°C at a heating rate of 10°C / min and maintaining at this temperature for 0.5 hours to prepare activated nitrogen-doped biochar.

[0089] (8) The activated nitrogen-doped biochar, graphene, and polytetrafluoroethylene solution (the mass concentration of the polytetrafluoroethylene solution is 5%) are mixed uniformly in a mass ratio of 8:1:1, and then anhydrous ethanol is added for demulsification. The ratio of the polytetrafluoroethylene solution to anhydrous ethanol is 1:1.6 to obtain a mixture; the mixture is coated on a nickel mesh (size is 1 cm×1 cm), placed in a constant temperature drying oven at 83°C for 1 hour, and then pressed at a pressure of 20 MPa. After pressing, the tablets are continued to be dried at a drying temperature of 75°C and a drying time of 12 hours to obtain an electrode.

[0090] Comparative Example 1

[0091] The method for preparing nitrogen-doped electrode materials by coupling nitrogen-rich compound pyrolysis oil with MOFs template method described in Comparative Example 1 is different from that in Example 1 in that the corn stalk powder is not subjected to biological pretreatment. The specific steps are as follows:

[0092] (1) The collected corn stalks were crushed with a crusher, and biomass powder with a particle size of 80 mesh was screened out, and the biomass powder was placed in a drying oven at 105° C. and dried for 16 hours to obtain corn stalk powder.

[0093] (2) First, a urea solution was prepared, and the mass concentration of the urea solution was controlled to be 8%. The biomass raw material after fungal pretreatment was immersed in the urea solution, that is, 20 g of corn straw powder raw material was added to 500 mL of urea solution, and magnetic stirring was performed at room temperature for 8 hours, and then it was filtered and placed in a drying oven at 105° C. for 12 hours to prepare nitrogen-containing biomass.

[0094] (3) The above-mentioned nitrogen-containing biomass and ZIF-67 molecular sieve catalyst (Nanjing Jichang Nanotechnology Co., Ltd.) were weighed out according to a mass ratio of 5:1, and placed in the same quartz boat respectively. The nitrogen-containing biomass and the ZIF-67 molecular sieve catalyst were separated by quartz wool. The temperature was raised to the pyrolysis temperature at a heating rate of 10°C / min, and then the quartz boat was pushed to the heating section of the pyrolysis reactor for pyrolysis. The pyrolysis atmosphere was argon, the pyrolysis temperature was 500°C, and the pyrolysis time was 10 min. The volatile matter was condensed and collected by a condensation system to obtain a pyrolysis oil rich in nitrogen compounds (3.3% pyridines, 15.1% pyrroles, 3.6% nitriles, 11.2% amines, 2.2% hydrazines and 1.7% pyrazines) (the condensation temperature of the condensation system was -10°C), and the remaining solid was the biochar produced by the primary pyrolysis.

[0095] (4) The nitrogen compound-rich pyrolysis oil in step (3), the biochar produced by the primary pyrolysis, the ZIF-67 molecular sieve catalyst (Nanjing Jichang Nanotechnology Co., Ltd.) and the template (magnesium hydroxide) are magnetically stirred and mixed, the magnetic stirring time is 12 hours, and the magnetic stirring temperature is room temperature, wherein the mass ratio of the nitrogen compound-rich pyrolysis oil, the biochar produced by the primary pyrolysis, the ZIF-67 molecular sieve catalyst (Nanjing Jichang Nanotechnology Co., Ltd.) and the template (magnesium hydroxide) is 1:1:1:1; then the mixture is transferred to a quartz boat, and the temperature is increased to 700°C at a heating rate of 8°C / min for carbonization, the carbonization time is 1.5 hours, and the carbonization atmosphere is argon to prepare a nitrogen-doped carbon material.

[0096] (5) The obtained product was acid-washed with nitric acid; the molar ratio of the acid to the template was 1:1, and magnetic stirring was performed at room temperature for 10 hours. The carbonized product was then washed with water to remove impurities such as the template, washed to neutrality, and then dried at 95°C for 9 hours to obtain inactivated nitrogen-doped biochar.

[0097] (6) The unactivated nitrogen-doped biochar obtained in step (5) was mixed with potassium oxalate in a mass ratio of 1:1 and placed in a quartz boat for activation treatment. The activation treatment conditions were heating to 800°C at a heating rate of 8°C / min and maintaining at this temperature for 2.5 hours to prepare activated nitrogen-doped biochar.

[0098] (7) The activated nitrogen-doped biochar, graphene, and polytetrafluoroethylene solution (the mass concentration of the polytetrafluoroethylene solution is 5%) are mixed uniformly in a mass ratio of 8:1:1, and then anhydrous ethanol is added for demulsification. The ratio of the polytetrafluoroethylene solution to anhydrous ethanol is 1:1.6 to obtain a mixture; the mixture is coated on a nickel mesh (size is 1 cm×1 cm), placed in a constant temperature drying oven at 82°C for 1 hour, and then pressed at a pressure of 20 MPa. After pressing, the tablets are continued to be dried at a drying temperature of 73°C and a drying time of 12 hours to obtain an electrode.

[0099] Comparative Example 2

[0100] The method for preparing nitrogen-doped electrode materials by coupling nitrogen-rich pyrolysis oil with MOFs template method described in Comparative Example 2 is different from that in Example 1 in that no catalyst is added during the preparation of pyrolysis oil. The specific steps are as follows:

[0101] (1) The collected corn stalks are crushed by a crusher to obtain corn stalk powder with a particle size of 60 mesh.

[0102] (2) First, activate P. chrysosporium at 29°C for 9 days, wash the generated mycelium with water, filter and add sterile water to 50 mL, and use a vortex oscillator to homogenize the fungal spore inoculum for later use. Put 20g corn straw powder and 50mL of water into a triangular bottle, seal it with a breathable sealing film, and sterilize it at 120°C for 15min at a pressure of 0.12MPa. In the clean bench, inoculate 10mL of homogenized fungal inoculum in each sterilized triangular bottle, place it in a 28°C incubator for 2 weeks, wash the pretreated corn straw powder repeatedly with water to remove the surface mycelium, and then dry it at 105°C for 16 hours, grind and sieve to select 80 mesh, put it into a sample bag, and store it in a desiccator for later use.

[0103] (3) First, a urea solution was prepared, and the mass concentration of the urea solution was controlled to be 8%. The biomass raw material after fungal pretreatment was immersed in the urea solution, that is, 20 g of corn straw powder raw material was added to 500 mL of urea solution, and magnetic stirring was performed at room temperature for 8 hours, and then filtered, and placed in a drying oven at 105° C. for 12 hours to prepare nitrogen-containing biomass.

[0104] (4) The nitrogen-containing biomass is placed in a quartz boat, and the temperature is increased to the pyrolysis temperature at a heating rate of 10°C / min. The quartz boat is then pushed to the heating section of the pyrolysis reactor for pyrolysis. The pyrolysis atmosphere is argon, the pyrolysis temperature is 500°C, and the pyrolysis time is 10 min. The volatile matter is condensed and collected by a condensation system to obtain a pyrolysis oil rich in nitrogen compounds (5.1% pyridines, 22.2% pyrroles, 3.4% nitriles, 15.7% amines, 2.5% hydrazines, and 1.8% pyrazines) (the condensation temperature of the condensation system is -10°C), and the remaining solid is the biochar produced by the primary pyrolysis.

[0105] (5) The nitrogen compound-rich pyrolysis oil in step (4), the biochar produced by the primary pyrolysis, the ZIF-67 molecular sieve catalyst (Nanjing Jichang Nanotechnology Co., Ltd.) and the template (magnesium hydroxide) are magnetically stirred and mixed, the magnetic stirring time is 12 hours, and the magnetic stirring temperature is room temperature, wherein the mass ratio of the nitrogen compound-rich pyrolysis oil, the biochar produced by the primary pyrolysis, the ZIF-67 molecular sieve catalyst (Nanjing Jichang Nanotechnology Co., Ltd.) and the template (magnesium hydroxide) is 1:1:1:1; then the mixture is transferred to a quartz boat, and the temperature is increased to 800°C at a heating rate of 8°C / min for carbonization, the carbonization time is 1.5 hours, and the carbonization atmosphere is argon to prepare a nitrogen-doped carbon material.

[0106] (6) The obtained product was acid-washed with nitric acid; the molar ratio of the acid to the template was 1:1, and magnetic stirring was performed at room temperature for 10 hours. The carbonized product was then washed with water to remove impurities such as the template, washed to neutrality, and then dried at 95°C for 9 hours to obtain inactivated nitrogen-doped biochar.

[0107] (7) The unactivated nitrogen-doped biochar obtained in step (6) was mixed with potassium oxalate in a mass ratio of 1:1 and placed in a quartz boat for activation treatment. The activation treatment conditions were heating to 700°C at a heating rate of 8°C / min and maintaining at this temperature for 2.5 hours to prepare activated nitrogen-doped biochar.

[0108] (8) The activated nitrogen-doped biochar, graphene, and polytetrafluoroethylene solution (the mass concentration of the polytetrafluoroethylene solution is 5%) are mixed uniformly in a mass ratio of 8:1:1, and then anhydrous ethanol is added for demulsification. The ratio of the polytetrafluoroethylene solution to anhydrous ethanol is 1:1.6 to obtain a mixture; the mixture is coated on a nickel mesh (size is 1 cm×1 cm), placed in a constant temperature drying oven at 82°C for 1 hour, and then pressed at a pressure of 20 MPa. After pressing, the tablets are continued to be dried at a drying temperature of 73°C and a drying time of 12 hours to obtain an electrode.

[0109] Comparative Example 3

[0110] The method for preparing nitrogen-doped electrode materials with nitrogen-rich compounds described in this comparative example 3 is different from that in Example 1 in that pyrolysis oil impregnation and MOFs template carbonization treatment are not performed, and the specific steps are as follows:

[0111] (1) The collected corn stalks are crushed by a crusher to obtain corn stalk powder with a particle size of 60 mesh.

[0112] (2) First, activate P. chrysosporium at 29°C for 9 days, wash the generated mycelium with water, filter and add sterile water to 50 mL, and use a vortex oscillator to homogenize the fungal spore inoculum for later use. Put 20g corn straw powder and 50mL of water into a triangular bottle, seal it with a breathable sealing film, and sterilize it at 120°C for 15min at a pressure of 0.12MPa. In the clean bench, inoculate 10mL of homogenized fungal inoculum in each sterilized triangular bottle, place it in a 28°C incubator for 2 weeks, wash the pretreated corn straw powder repeatedly with water to remove the surface mycelium, and then dry it at 105°C for 16 hours, grind and sieve to select 80 mesh, put it into a sample bag, and store it in a desiccator for later use.

[0113] (3) First, a urea solution was prepared, and the mass concentration of the urea solution was controlled to be 8%. The biomass raw material after fungal pretreatment was immersed in the urea solution, that is, 20 g of corn straw powder raw material was added to 500 mL of urea solution, and magnetic stirring was performed at room temperature for 8 hours, and then filtered, and placed in a drying oven at 105° C. for 12 hours to prepare nitrogen-containing biomass.

[0114] (4) The nitrogen-containing biomass and the ZIF-67 molecular sieve catalyst (Nanjing Jichang Nanotechnology Co., Ltd.) were weighed out according to a mass ratio of 5:1, and placed in the same quartz boat respectively. The nitrogen-containing biomass and the ZIF-67 molecular sieve catalyst were separated by quartz wool. The temperature was raised to the pyrolysis temperature at a heating rate of 10°C / min, and then the quartz boat was pushed to the heating section of the pyrolysis reactor for pyrolysis. The pyrolysis atmosphere was argon, the pyrolysis temperature was 500°C, and the pyrolysis time was 10 min. The volatile matter was condensed and collected by a condensation system to obtain a pyrolysis oil rich in nitrogen compounds (9.8% pyridines, 36.2% pyrroles, 6.2% nitriles, 17.9% amines, 5.6% hydrazines and 2.6% pyrazines) (the condensation temperature of the condensation system was -10°C), and the remaining solid was the biochar produced by the primary pyrolysis.

[0115] (5) The biochar produced by the primary pyrolysis was transferred to a quartz boat, and the pyrolysis reactor was set up and heated to 800°C at a heating rate of 8°C / min for carbonization. The carbonization time was 1.5 hours, and the carbonization atmosphere was argon.

[0116] (6) The biochar obtained in step (5) was mixed with potassium oxalate in a mass ratio of 1:1, and placed in a quartz boat for activation treatment. The activation treatment conditions were heating to 700°C at a heating rate of 8°C / min and maintaining at this temperature for 2.5 hours to prepare activated nitrogen-doped biochar.

[0117] (7) The activated nitrogen-doped biochar, graphene, and polytetrafluoroethylene solution (the mass concentration of the polytetrafluoroethylene solution is 5%) are mixed uniformly in a mass ratio of 8:1:1, and then anhydrous ethanol is added for demulsification. The ratio of the polytetrafluoroethylene solution to anhydrous ethanol is 1:1.6 to obtain a mixture; the mixture is coated on a nickel mesh (size is 1 cm×1 cm), placed in a constant temperature drying oven at 82°C for 1 hour, and then pressed at a pressure of 20 MPa. After pressing, the tablets are continued to be dried at a drying temperature of 73°C and a drying time of 12 hours to obtain an electrode.

[0118] The performance tests were performed on the activated nitrogen-doped biochar and electrodes prepared in Examples 1-3 and Comparative Examples 1-3. The results are shown in Table 1 below:

[0119] Table 1 Activated nitrogen-doped biochar prepared in Examples 1-3 and Comparative Examples 1-3 and electrode performance test results

[0120] Serial number Yield of nitrogen-containing porous carbon / % <![CDATA[Specific surface area / m 2 / g]]> Specific capacitance / F / g Example 1 46.1 2034.7 657.1 Example 2 44.5 1936.4 540.5 Example 3 45.2 1975.9 568.8 Comparative Example 1 30.2 1705.2 267.3 Comparative Example 2 32.5 1836.6 294.6 Comparative Example 3 26.5 1685.6 182.5

Claims

1. A method for preparing nitrogen-doped electrode materials by coupling pyrolysis oil rich in nitrogen compounds with MOFs template method, characterized in that: It consists of the following steps: (1) crushing the biomass to obtain crushed biomass; (2) mixing the crushed biomass prepared in step (1) with water and sterilizing it, then inoculating it with a fungal inoculum for pretreatment, and finally washing it with water to remove the hyphae on the surface of the pretreated biomass, drying it, grinding it and screening it, so as to prepare a biomass raw material; (3) immersing the biomass raw material prepared in step (2) in a nitrogen-containing solution, performing magnetic stirring, and then filtering and drying to prepare nitrogen-containing biomass; (4) subjecting the nitrogen-containing biomass prepared in step (3) to non-in-situ pyrolysis with a catalyst in an oxygen-free atmosphere, and collecting the volatile matter through a condensation system to obtain pyrolysis oil rich in nitrogen compounds, and the remaining solid is biochar produced by the primary pyrolysis; (5) mixing the nitrogen compound-rich pyrolysis oil in step (4), the biochar produced by the primary pyrolysis, the metal organic framework compound and the template by magnetic stirring, and then carbonizing the mixture to prepare a nitrogen-doped carbon material; (6) acid washing the nitrogen-doped carbon material prepared in step (5) to remove the template, then washing with water until neutral, and drying to obtain inactivated nitrogen-doped biochar; (7) mixing the unactivated nitrogen-doped biochar of step (6) with an activating agent for activation treatment to prepare activated nitrogen-doped biochar; (8) The activated nitrogen-doped biochar, the conductive material and the polytetrafluoroethylene solution prepared in step (7) are uniformly mixed, and then anhydrous ethanol is added for demulsification to obtain a mixture, and the mixture is coated on a carrier, and then dried, compacted and baked to obtain an electrode.

2. The method for preparing nitrogen-doped electrode materials by coupling nitrogen-rich compound pyrolysis oil with MOFs template method according to claim 1, characterized in that: The biomass in step (1) is one or more of crop straw, fruit shell, leaves, bark, aquatic plants or algae; wherein the crop straw is one or more of corn straw, wheat straw, soybean straw, cotton straw or pea straw; the fruit shell is one or more of walnut shell, peanut shell or coconut shell; The particle size of the crushed biomass obtained in step (1) is 40-80 meshes.

3. The method for preparing nitrogen-doped electrode materials by coupling nitrogen-rich compound pyrolysis oil with MOFs template method according to claim 1, characterized in that: The sterilization treatment in step (2) is performed at 120° C. for 15 min and a pressure of 0.12 MPa; In step (2), the fungus is first activated at 28-30° C. for 8-10 days, the generated mycelium is washed with sterile water, filtered and supplemented with sterile water, and homogenized using a vortex oscillator to prepare a fungal inoculum, wherein the fungus is one or more of Trichoderma koningii, Aspergillus niger, Aspergillus kawachii, white rot fungus Trametes versicolor, brown rot fungus or Phanerochaete chrysosporium, preferably Phanerochaete chrysosporium.

4. The method for preparing nitrogen-doped electrode materials by coupling nitrogen-rich compound pyrolysis oil with MOFs template method according to claim 1, characterized in that: In step (2), the mass ratio of the crushed biomass prepared in step (1) to water is 1:1-1:4; The pretreatment in step (2) is carried out in an incubator at 28° C. for 7-14 days; In step (2), the drying temperature is 105° C. and the drying time is 12-24 hours; The amount of the crushed biomass and the fungal inoculum in step (2) is 20-50:6-10, in g / mL; In step (2), the biomass raw material powder with a size of 60-100 mesh is ground and sieved.

5. The method for preparing nitrogen-doped electrode materials by coupling nitrogen-rich compound pyrolysis oil with MOFs template method according to claim 1, characterized in that: The nitrogen-containing solution in step (3) is one of aqueous ammonia, urea solution, aniline solution, dicyandiamide solution or melamine solution, and the mass concentration of the nitrogen-containing solution is 1-30%; In step (3), the mass volume ratio of the biomass raw material to the nitrogen-containing solution is 2-4:50-100, in units of g / mL; In step (3), the magnetic stirring temperature is room temperature and the magnetic stirring time is 5-10 h; In step (3), the drying temperature is 90-105° C. and the drying time is 12-48 hours.

6. The method for preparing nitrogen-doped electrode materials by coupling nitrogen-rich compound pyrolysis oil with MOFs template method according to claim 1, characterized in that: In step (4), the mass ratio of nitrogen-containing biomass to catalyst is 5:1-6; The catalyst in step (4) is one or more of a ZSM-5 molecular sieve catalyst, an MCM-41 molecular sieve catalyst or a ZIF-67 catalyst; In step (4), the oxygen-free atmosphere is one of argon, nitrogen, carbon dioxide or ammonia or a mixture thereof; The non-in-situ pyrolysis in step (4) is to place the nitrogen-containing biomass and the catalyst in the same quartz boat, respectively, with the nitrogen-containing biomass and the catalyst separated by quartz wool, and heat the mixture to the pyrolysis temperature at a heating rate of 5-10°C / min, and then push the quartz boat to the heating section of the pyrolysis reactor for pyrolysis, wherein the pyrolysis temperature is 400-600°C and the pyrolysis time is 5-20min; The condensation temperature of the condensation system in step (4) is -10-20°C.

7. The method for preparing nitrogen-doped electrode materials by coupling nitrogen-rich compound pyrolysis oil with MOFs template method according to claim 1, characterized in that: In step (5), the mass ratio of the nitrogen compound-rich pyrolysis oil, the biochar produced by the primary pyrolysis, the metal organic framework compound, and the template agent is 1:1-2:0.2-1:1-3; In step (5), the metal organic framework compound is one or more mixtures of MOF-5, MOF-74, HKUST-1, ZIF-8, ZIF-67, MIL-100, MIL-125, UiO-66 and NU-110; In step (5), the magnetic stirring time is 12-24 h, and the magnetic stirring temperature is room temperature; In step (5), the carbonization treatment is to transfer the mixture to a quartz boat, heat it to 700-900°C at a heating rate of 5-10°C / min for carbonization, the carbonization time is 1-2h, and the carbonization atmosphere is one of argon, nitrogen or ammonia or a mixture thereof; The template in step (5) is one of magnesium hydroxide, zinc hydroxide or calcium hydroxide.

8. The method for preparing nitrogen-doped electrode materials by coupling nitrogen-rich compound pyrolysis oil with MOFs template method according to claim 1, characterized in that: The acid used for pickling in step (6) is one of nitric acid, hydrochloric acid or sulfuric acid; In step (6), the acid and nitrogen-doped carbon material are magnetically stirred at room temperature for 1-10 hours, the molar ratio of the acid to the template is 1-1.2:1, and then washed with water to neutrality, and dried at 80-110° C. for 6-12 hours to obtain unactivated nitrogen-doped biochar.

9. The method for preparing nitrogen-doped electrode materials by coupling nitrogen-rich compound pyrolysis oil with MOFs template method according to claim 1, characterized in that: In step (7), the mass ratio of the unactivated nitrogen-doped biochar to the activating agent is 2:1-4; In step (7), the activator is one or more of zinc chloride, potassium hydroxide, sodium hydroxide or potassium oxalate; The activation treatment in step (7) is performed by heating to 700-900°C at a heating rate of 5-10°C / min, and then keeping the temperature for 0.5-5 hours.

10. The method for preparing nitrogen-doped electrode materials by coupling nitrogen-rich compound pyrolysis oil with MOFs template method according to claim 1, characterized in that: In step (8), the carrier is one of a nickel mesh, a titanium mesh or a stainless steel mesh; the conductive material is at least one of acetylene black or graphene; the mass fraction of the polytetrafluoroethylene solution is 5%; In step (8), the mass ratio of activated nitrogen-doped biochar, conductive material and polytetrafluoroethylene solution is 8:1:1, and the volume ratio of polytetrafluoroethylene solution to anhydrous ethanol is 1:1.6; In step (8), the drying temperature is 80-83°C, the drying time is 1 hour, the compaction pressure is 20 MPa, the drying temperature is 70-75°C, and the drying time is 12 hours.

Citation Information

Patent Citations

  • Porous carbon material with high specific surface area prepared by virtue of fungal pretreatment as well as method and application thereof

    CN109574007A

  • Carbon material prepared from bio-oil obtained by catalytic pyrolysis of biomass and method of carbon material

    CN114613612A

Cited By

  • Method for preparing capacitor carbon by taking cotton stalks as raw material and capacitor carbon

    CN121790188A