Carbon-coated 1T / 2H-phase molybdenum disulfide flexible electrode and preparation method and application thereof
By depositing a carbon layer on the surface of molybdenum disulfide using a glucose hydrothermal method, the problem of easy structural damage of molybdenum disulfide materials during charge and discharge was solved, realizing a high-performance flexible electrode and improving electrochemical and mechanical properties.
Patent Information
- Application Number
- CN202411187255.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-08
AI Technical Summary
Existing molybdenum disulfide materials are prone to structural damage during charge and discharge, resulting in poor cycle stability and susceptibility to phase transitions at high temperatures, which limits their application in flexible electrodes.
A carbonaceous layer was deposited on the surface of molybdenum disulfide using a glucose hydrothermal method, avoiding high-temperature treatment, to form a carbon-coated 1T/2H phase molybdenum disulfide flexible electrode, which serves as a conductive network and physical buffer layer, enhancing mechanical and electrochemical stability.
It improves the electrochemical and mechanical properties of flexible electrodes, significantly enhances specific capacitance and cycle stability, and maintains excellent mechanical stability.
Smart Images

Figure CN118919320A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrode materials, and in particular to a carbon-coated 1T / 2H phase molybdenum disulfide flexible electrode and a preparation method and application thereof. Background Art
[0002] With the continuous advancement of electronic technology, electronic devices are gradually developing towards being lighter, thinner, more flexible and wearable. However, traditional rigid energy storage devices are difficult to adapt to the development of flexible electronic devices, and the development of flexible energy storage devices that are compatible with them is considered a considerable challenge. Supercapacitors have excellent electrochemical properties such as high power density, rapid charging and discharging, and high cycle life. They also have the advantages of simple structure, easy assembly, stable properties and no pollution, and are suitable for being developed into safe and reliable flexible energy storage devices. Among them, flexible electrodes are the most important components of flexible supercapacitors. At present, many electrode materials, such as graphene, carbon nanotubes, conductive polymers and metal oxides, have been continuously developed, especially some pseudocapacitive materials with excellent electrochemical properties have attracted people's attention.
[0003] Transition metal disulfides (TMDs) are typical pseudocapacitive electrode materials, among which MoS2 is the most representative transition metal sulfide, which mainly stores energy through the insertion / extraction of ions and has excellent theoretical specific capacity. In addition, MoS2 materials with a two-dimensional nanosheet structure exhibit excellent flexibility due to their special layered crystal structure, and are therefore considered to be potential flexible electrode materials. Typically, MoS2 has a 1T metal phase and a 2H semiconductor phase. Compared with the 2H phase, 1T phase MoS2 has higher conductivity, larger interlayer spacing and hydrophilicity, and is often used as an electrode material for high-performance supercapacitors. However, due to its metastable characteristics, pure 1T phase MoS2 is difficult to prepare, and MoS2 materials mixed with 1T and 2H phases are generally used.
[0004] However, due to its inherent defects, such as severe volume expansion during the charge and discharge process that causes its structure to be destroyed, resulting in capacity attenuation, the application of molybdenum disulfide as a flexible electrode is limited. In order to improve the electrochemical and mechanical properties of molybdenum disulfide materials, coating with carbon materials is the most common modification method. Carbon materials have excellent electrochemical stability and mechanical properties. Coating molybdenum disulfide with carbon materials can effectively alleviate its volume expansion, improve its structural stability and stabilize the electrode interface. However, in the field of electrochemistry, carbon coating mostly adopts high-temperature carbonization, and high temperature will affect the complete transformation of molybdenum disulfide 1T phase to 2H phase, causing a serious decline in its electrochemical performance. Therefore, how to solve the defects of poor cycle stability and easy phase transformation under the influence of high temperature in molybdenum disulfide materials in the prior art is a problem that needs to be solved urgently in this field. Summary of the invention
[0005] The purpose of the present invention is to provide a carbon-coated 1T / 2H phase molybdenum disulfide flexible electrode and a preparation method and application thereof. The flexible electrode prepared by the preparation method solves the problems of poor cycle stability and easy phase transition under high temperature in the prior art.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a method for preparing a carbon-coated 1T / 2H phase molybdenum disulfide flexible electrode, comprising the following steps:
[0008] Placing the 1T / 2H phase molybdenum disulfide-carbon cloth electrode in a glucose solution for hydrothermal reaction to obtain the carbon-coated 1T / 2H phase molybdenum disulfide flexible electrode;
[0009] The 1T / 2H phase molybdenum disulfide-carbon cloth electrode comprises a carbon cloth and a 1T / 2H phase molybdenum disulfide layer distributed on the surface of the carbon cloth.
[0010] Preferably, the dosage ratio of glucose to solvent in the glucose solution is (0.05-1) mol:60 mL.
[0011] Preferably, the temperature of the hydrothermal reaction is 160-180° C., and the time is 2-6 hours.
[0012] Preferably, the preparation method of the 1T / 2H phase molybdenum disulfide-carbon cloth electrode comprises:
[0013] Mixing a soluble molybdenum source, a soluble sulfur source and water to obtain a molybdenum disulfide precursor solution;
[0014] The carbon cloth is placed in the molybdenum disulfide precursor solution to carry out a first hydrothermal reaction to obtain a 1T / 2H phase molybdenum disulfide-carbon cloth electrode.
[0015] Preferably, the mass ratio of the soluble molybdenum source to water is (0.206-0.618):90.
[0016] Preferably, the mass ratio of the soluble sulfur source to water is (0.3806-1.1418):90.
[0017] Preferably, the soluble molybdenum source includes one or more of ammonium molybdate, sodium molybdate and molybdenum chloride;
[0018] The soluble sulfur source includes one or more of thiourea, thioacetamide, ammonium sulfide and sodium sulfide.
[0019] Preferably, the temperature of the first hydrothermal reaction is 180-200° C., and the time is 12-18 hours.
[0020] The present invention also provides a carbon-coated 1T / 2H phase molybdenum disulfide flexible electrode prepared by the preparation method described in the above technical solution, comprising a carbon cloth and a 1T / 2H phase molybdenum disulfide layer and a carbon coating layer sequentially coated on the surface of the carbon cloth.
[0021] The present invention also provides the use of the carbon-coated 1T / 2H phase molybdenum disulfide flexible electrode described in the above technical solution in a supercapacitor.
[0022] The present invention provides a method for preparing a carbon-coated 1T / 2H phase molybdenum disulfide flexible electrode, comprising the following steps: placing a 1T / 2H phase molybdenum disulfide-carbon cloth electrode in a glucose solution, performing a hydrothermal reaction, and obtaining the carbon-coated 1T / 2H phase molybdenum disulfide flexible electrode; the 1T / 2H phase molybdenum disulfide-carbon cloth electrode comprises a carbon cloth and a 1T / 2H phase molybdenum disulfide layer distributed on the surface of the carbon cloth. At present, most carbon-coated composite materials deposit a carbon source on a substrate material, and then convert it into a carbon layer by high-temperature pyrolysis (above 600°C), while the preparation method of the present invention uses hydrothermal carbonization of glucose to deposit a carbonaceous layer on the surface of molybdenum disulfide, and does not require high-temperature treatment, thereby avoiding the influence of high temperature on the phase transformation of molybdenum disulfide, and the method is simpler and energy-saving. At the same time, the carbon coating layer generated by the hydrothermal method has better conductivity and mechanical strength, and can be used as a physical buffer layer to help alleviate the volume expansion of the molybdenum disulfide electrode during the charge and discharge cycle and improve its electrochemical performance; further, the carbon coating layer generated by the hydrothermal method can also be used as a conductive network to fix the electrode fragments together and maintain their mechanical and electrochemical stability. The test results of the embodiment show that the flexible electrode prepared by the present invention has significantly improved specific capacitance and excellent cycle stability; at the same time, it also has good mechanical properties and excellent mechanical stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a SEM image of the 1T / 2H phase molybdenum disulfide-carbon cloth electrode described in Example 1;
[0024] Figure 2 This is a SEM image of the carbon-coated 1T / 2H phase molybdenum disulfide flexible electrode described in Example 1;
[0025] Figure 3 TEM image of the carbon-coated 1T / 2H phase molybdenum disulfide flexible electrode described in Example 1;
[0026] Figure 4 The XPS graph of the carbon-coated 1T / 2H phase molybdenum disulfide flexible electrode described in Examples 1, 2, and 3;
[0027] Figure 5 The charge and discharge curves of the carbon-coated 1T / 2H phase molybdenum disulfide flexible electrode at different current densities described in Example 1;
[0028] Figure 6 The carbon-coated 1T / 2H phase MoS2 flexible electrode described in Example 1 was tested at 10 mA·cm -2 Cycling performance diagram at current density of .
[0029] Figure 7 The SEM images (a) and TEM images (b) of the carbon-coated 1T / 2H phase MoS2 flexible electrode described in Example 2, the charge-discharge curves at different current densities (c) and the charge-discharge curves at 10 mA·cm -2 Cycling performance diagram at current density of (d).
[0030] Figure 8 The SEM images (a) and TEM images (b) of the carbon-coated 1T / 2H phase MoS2 flexible electrode described in Example 3, the charge-discharge curves at different current densities (c) and the charge-discharge curves at 10 mA·cm -2 Cycling performance diagram at current density of (d). DETAILED DESCRIPTION
[0031] The present invention provides a method for preparing a carbon-coated 1T / 2H phase molybdenum disulfide flexible electrode, comprising the following steps:
[0032] Placing the 1T / 2H phase molybdenum disulfide-carbon cloth electrode in a glucose solution for hydrothermal reaction to obtain the carbon-coated 1T / 2H phase molybdenum disulfide flexible electrode;
[0033] The 1T / 2H phase molybdenum disulfide-carbon cloth electrode comprises a carbon cloth and a 1T / 2H phase molybdenum disulfide layer distributed on the surface of the carbon cloth.
[0034] In the present invention, unless otherwise specified, all preparation raw materials are commercially available products well known to those skilled in the art.
[0035] In the present invention, the preparation method of the 1T / 2H phase molybdenum disulfide-carbon cloth electrode preferably includes:
[0036] Mixing a soluble molybdenum source, a soluble sulfur source and water to obtain a molybdenum disulfide precursor solution;
[0037] The carbon is placed in the molybdenum disulfide precursor solution, and a first hydrothermal reaction is performed to obtain a 1T / 2H phase molybdenum disulfide-carbon cloth electrode.
[0038] The present invention mixes a soluble molybdenum source, a soluble sulfur source and water to obtain a molybdenum disulfide precursor solution.
[0039] In the present invention, the mass ratio of the soluble molybdenum source to water is preferably (0.206-0.618):90, more preferably (0.25-0.50):90, and most preferably (0.3-0.4):90. In the present invention, the mass ratio of the soluble sulfur source to water is preferably (0.3806-1.1418):90, more preferably (0.5-0.8):90, and most preferably (0.6-0.7):90.
[0040] In the present invention, the soluble molybdenum source preferably includes one or more of ammonium molybdate, sodium molybdate and molybdenum chloride, and the ammonium molybdate is preferably ammonium molybdate tetrahydrate; when the soluble molybdenum source is two or more of the above-mentioned specific selections, the present invention has no special restrictions on the ratio of the above-mentioned specific substances, and they can be mixed in any ratio. In the present invention, the soluble sulfur source preferably includes one or more of thiourea, thioacetamide, ammonium sulfide and sodium sulfide, and more preferably includes thiourea; when the soluble sulfur source is two or more of the above-mentioned specific selections, the present invention has no special restrictions on the ratio of the above-mentioned specific substances, and they can be mixed in any ratio. In the present invention, the water is preferably deionized water.
[0041] The present invention does not have any special limitation on the mixing process, and a process well known to those skilled in the art may be used to ensure that the soluble molybdenum source and the soluble sulfur source are fully dissolved in water.
[0042] After obtaining the molybdenum disulfide precursor solution, the present invention arranges carbon in the molybdenum disulfide precursor solution, performs a first hydrothermal reaction, and obtains a 1T / 2H phase molybdenum disulfide-carbon cloth electrode.
[0043] In the present invention, the volume of the molybdenum disulfide precursor solution used per square centimeter of carbon cloth is preferably 5 to 12 mL, more preferably 8 to 12 mL, and most preferably 10 to 12 mL.
[0044] In the present invention, the temperature of the first hydrothermal reaction is preferably 180-200°C, more preferably 130-180°C, most preferably 140-160°C; the time is preferably 12-18h, more preferably 13-17h, most preferably 14-16h.
[0045] After the first hydrothermal reaction is completed, the present invention also preferably includes washing and drying performed in sequence; the washing is preferably performed by repeatedly washing with deionized water and alcohol in sequence; the drying is preferably vacuum drying. The present invention does not have any special limitation on the vacuum drying process, and the process familiar to those skilled in the art can be used.
[0046] In the present invention, the ratio of glucose to solvent in the glucose solution is preferably (0.05-1) mol:60 mL, more preferably (0.3-0.6) mol:60 mL, and most preferably (0.4-0.5) mol:60 mL.
[0047] In the present invention, the glucose solution is preferably obtained by dissolving glucose in water; the present invention has no special limitation on the dissolution process, and the process well known to those skilled in the art can be used.
[0048] In the present invention, the volume of the glucose solution used per square centimeter of the 1T / 2H phase molybdenum disulfide-carbon cloth electrode is preferably 10 to 15 mL, more preferably 12 to 15 mL, and most preferably 14 to 15 mL.
[0049] In the present invention, the temperature of the hydrothermal reaction is preferably 160-180°C, more preferably 165-175°C, more preferably 168-172°C; the time is preferably 2-6h, more preferably 3-5h, most preferably 3.5-4.5h.
[0050] After the hydrothermal reaction is completed, the present invention also preferably includes washing and drying performed in sequence; the washing is preferably performed by repeatedly washing with deionized water and alcohol in sequence; the drying is preferably vacuum drying. The present invention does not have any special limitation on the vacuum drying process, and the process familiar to those skilled in the art can be used.
[0051] The present invention also provides a carbon-coated 1T / 2H phase molybdenum disulfide flexible electrode prepared by the preparation method described in the above technical solution, comprising a carbon cloth and a 1T / 2H phase molybdenum disulfide layer and a carbon coating layer sequentially coated on the surface of the carbon cloth.
[0052] In the present invention, the carbon in the carbon coating layer is preferably amorphous carbon.
[0053] The present invention also provides the application of the carbon-coated 1T / 2H phase molybdenum disulfide flexible electrode described in the above technical solution in a supercapacitor. The present invention does not have any special limitation on the method of the application, and the method well known to those skilled in the art can be used.
[0054] The carbon-coated 1T / 2H phase molybdenum disulfide flexible electrode provided by the present invention and its preparation method and application are described in detail below in conjunction with the embodiments, but they should not be understood as limiting the scope of protection of the present invention.
[0055] Example 1
[0056] Dissolve 0.618 g of ammonium molybdate tetrahydrate powder and 1.1418 g of thiourea powder in 90 mL of deionized water to obtain a molybdenum disulfide precursor solution;
[0057] A carbon cloth with a size of 3×3 cm was immersed in 90 mL of the molybdenum disulfide precursor solution, and after hydrothermal reaction at 200° C. for 12 h, it was repeatedly washed with deionized water and alcohol alternately, and vacuum dried to obtain a 1T / 2H phase molybdenum disulfide-carbon cloth electrode;
[0058] Dissolve 1 mol of glucose powder in 60 mL of deionized water to obtain a glucose solution;
[0059] The 1T / 2H phase molybdenum disulfide-carbon cloth electrode with a size of 2×2 cm was immersed in 60 mL of the glucose solution, subjected to hydrothermal reaction at 160° C. for 4 h, repeatedly washed with deionized water and alcohol alternately, and vacuum dried to obtain a carbon-coated 1T / 2H phase molybdenum disulfide flexible electrode;
[0060] The 1T / 2H phase molybdenum disulfide-carbon cloth electrode was subjected to SEM testing, and the test results are as follows Figure 1 As shown by Figure 1 It can be seen that MoS2 presents a thin and curved nanosheet structure, which grows vertically and evenly on the surface of carbon cloth fibers, with almost no nanosheet agglomeration;
[0061] The carbon-coated 1T / 2H phase molybdenum disulfide flexible electrode was subjected to SEM testing. The test results are as follows Figure 2 As shown, the carbon-coated 1T / 2H phase molybdenum disulfide flexible electrode was subjected to TEM test, and the test results are as follows Figure 3 As shown by Figures 2-3 It can be seen that a thin amorphous carbon layer is deposited on the surface of MoS2 nanosheets, and the thickness of the carbon layer is about 4 nm;
[0062] The carbon-coated 1T / 2H phase molybdenum disulfide flexible electrode was subjected to XPS test. The test results are as follows Figure 4 As shown in (a), it can be seen from the figure that the peaks at 228.42 and 231.58 eV correspond to the 1T phase of Mo 3d, while the peaks at 229.01 and 232.25 eV correspond to the 2H phase;
[0063] The area specific capacitance and cycle stability of the carbon-coated 1T / 2H phase molybdenum disulfide flexible electrode were tested using an electrochemical workstation. Figure 5 is a charge and discharge curve diagram of the carbon-coated 1T / 2H phase molybdenum disulfide flexible electrode at different current densities, Figure 6 The carbon-coated 1T / 2H phase MoS2 flexible electrode is -2 The cycling performance diagram at a current density of Figures 5-6 It can be seen that at 1mA·cm -2 At a current density of 1.3 Å, the maximum area specific capacity of the carbon-coated 1T / 2H phase MoS2 flexible electrode is 443 mF·cm-2 , and has excellent cycle stability at 10mA·cm -2 At a current density of 1.34 W, the capacity retention rate after 10,000 cycles is 109%.
[0064] Example 2
[0065] Dissolve 0.618 g of ammonium molybdate tetrahydrate powder and 1.1418 g of thiourea powder in 90 mL of deionized water to obtain a molybdenum disulfide precursor solution;
[0066] A carbon cloth with a size of 3×3 cm was immersed in 90 mL of the molybdenum disulfide precursor solution, and after hydrothermal reaction at 200° C. for 12 h, it was repeatedly washed with deionized water and alcohol alternately, and vacuum dried to obtain a 1T / 2H phase molybdenum disulfide-carbon cloth electrode;
[0067] Dissolve 1 mol of glucose powder in 60 mL of deionized water to obtain a glucose solution;
[0068] The 1T / 2H phase molybdenum disulfide-carbon cloth electrode with a size of 2×2 cm was immersed in 60 mL of the glucose solution, subjected to hydrothermal reaction at 160° C. for 2 h, repeatedly washed with deionized water and alcohol alternately, and vacuum dried to obtain a carbon-coated 1T / 2H phase molybdenum disulfide flexible electrode;
[0069] The carbon-coated 1T / 2H phase MoS2 flexible electrode was subjected to SEM and TEM tests (eg Figure 7 As shown in (a) and (b) in the figure, the test results show that after the hydrothermal reaction time in the glucose aqueous solution is reduced to 2 hours, the amorphous carbon layer deposited on the surface of the MoS2 nanosheets becomes thinner and the thickness is about 1 nm.
[0070] The carbon-coated 1T / 2H phase molybdenum disulfide flexible electrode was subjected to XPS test. The test results are as follows Figure 4 As shown in (b) of Figure 4 It can be seen that the peaks at 228.47 and 231.62 eV correspond to the 1T phase of Mo 3d, while the peaks at 229.07 and 232.32 eV correspond to the 2H phase;
[0071] The area specific capacitance and cycle stability of the carbon-coated 1T / 2H phase molybdenum disulfide flexible electrode were tested using an electrochemical workstation. The test results are as follows: Figure 7 As shown in (c) and (d) in Figure 7 From (c) and (d) in Figure 1, we can see that at 1 mA·cm -2 At a current density of 1.3 Å, the maximum area specific capacity of the carbon-coated 1T / 2H phase MoS2 flexible electrode is 315 mF·cm -2 , and has good cycle stability at 10 mA cm -2At a current density of 1.5 Å, the capacity retention rate after 10,000 cycles is 90%.
[0072] Example 3
[0073] Dissolve 0.618 g of ammonium molybdate tetrahydrate powder and 1.1418 g of thiourea powder in 90 mL of deionized water to obtain a molybdenum disulfide precursor solution;
[0074] A carbon cloth with a size of 3×3 cm was immersed in 90 mL of the molybdenum disulfide precursor solution, and after hydrothermal reaction at 200° C. for 12 h, it was repeatedly washed with deionized water and alcohol alternately, and vacuum dried to obtain a 1T / 2H phase molybdenum disulfide-carbon cloth electrode;
[0075] Dissolve 1 mol of glucose powder in 60 mL of deionized water to obtain a glucose solution;
[0076] The 1T / 2H phase molybdenum disulfide-carbon cloth electrode with a size of 2×2 cm was immersed in 60 mL of the glucose solution, subjected to hydrothermal reaction at 160° C. for 6 h, repeatedly washed with deionized water and alcohol alternately, and vacuum dried to obtain a carbon-coated 1T / 2H phase molybdenum disulfide flexible electrode;
[0077] The carbon-coated 1T / 2H phase MoS2 flexible electrode was subjected to SEM and TEM tests (eg Figure 7 As shown in (a) and (b) in the figure, the test results show that after the hydrothermal reaction time in the glucose aqueous solution is increased to 6 h, the amorphous carbon layer deposited on the surface of the MoS2 nanosheets becomes significantly thicker, with a thickness of about 9 nm.
[0078] The carbon-coated 1T / 2H phase molybdenum disulfide flexible electrode was subjected to XPS test. The test results are as follows Figure 4 As shown in (c), the peaks at 228.45 and 231.58 eV correspond to the 1T phase of Mo 3d, while the peaks at 229.03 and 232.26 eV correspond to the 2H phase;
[0079] The area specific capacitance and cycle stability of the carbon-coated 1T / 2H phase molybdenum disulfide flexible electrode were tested using an electrochemical workstation. The test results are as follows: Figure 7 As shown in (c) and (d) in Figure 7 From (c) and (d) in Figure 1, we can see that at 1 mA·cm -2 At a current density of 1.3 Å, the maximum area specific capacity of the carbon-coated 1T / 2H phase MoS2 flexible electrode decreased significantly to about 163 mF·cm -2 , while maintaining excellent cycle stability at 10 mA cm -2 At a current density of 1.34 W, the capacity retention rate after 10,000 cycles is 100%.
[0080] Comparative Example 1
[0081] Dissolve 0.618 g of ammonium molybdate tetrahydrate powder and 1.1418 g of thiourea powder in 90 mL of deionized water to obtain a molybdenum disulfide precursor solution;
[0082] A carbon cloth with a size of 3×3 cm was immersed in 90 mL of the molybdenum disulfide precursor solution, and after hydrothermal reaction at 200° C. for 12 h, it was repeatedly washed with deionized water and alcohol alternately, and vacuum dried to obtain a 1T / 2H phase molybdenum disulfide-carbon cloth electrode;
[0083] The 1T / 2H phase molybdenum disulfide-carbon cloth electrode was subjected to XPS testing, and the test results were as follows: the peaks at 228.54 and 231.61 eV corresponded to the 1T phase of Mo 3d, and the peaks at 229.04 and 232.32 eV corresponded to the 2H phase;
[0084] The area specific capacitance and cycle stability of the 1T / 2H phase MoS2-carbon cloth electrode were tested using an electrochemical workstation. The test results were as follows: -2 At a current density of 1.3 Å, the maximum area specific capacity of the 1T / 2H phase MoS2-carbon cloth electrode is 240 mF·cm -2 , at 10 mA cm -2 At a current density of 1.34 W, the capacity retention rate after 5000 cycles is 78%.
[0085] Comparative Example 2
[0086] Dissolve 0.618 g of ammonium molybdate tetrahydrate powder and 1.1418 g of thiourea powder in 90 mL of deionized water to obtain a molybdenum disulfide precursor solution;
[0087] A carbon cloth with a size of 3×3 cm was immersed in 90 mL of the molybdenum disulfide precursor solution, and after hydrothermal reaction at 200° C. for 12 h, it was repeatedly washed with deionized water and alcohol alternately, and vacuum dried to obtain a 1T / 2H phase molybdenum disulfide-carbon cloth electrode;
[0088] 0.1 g of dopamine hydrochloride was dispersed in a Tris buffer solution (50 mL, 10 mM, pH = 8.5). The obtained 1T / 2H phase molybdenum disulfide-carbon cloth electrode was then immersed in the above solution for 24 h. It was then washed alternately with deionized water and alcohol and dried in vacuo. The obtained sample was heated to 800 ° C in a tube furnace under an argon atmosphere and maintained for 2 h at a heating rate of 5 ° C / min. A carbon-coated molybdenum disulfide flexible electrode was obtained.
[0089] The carbon-coated molybdenum disulfide flexible electrode was subjected to XPS testing, and the test results showed that the peaks at 229.14 and 232.38 eV corresponded to the 2H phase of molybdenum disulfide, and no obvious 1T phase peak appeared.
[0090] The area specific capacitance of the carbon-coated molybdenum disulfide flexible electrode was tested using an electrochemical workstation. The test results were as follows: -2 At a current density of 1.3 Å, the maximum area specific capacity of the carbon-coated MoS2 flexible electrode decreased significantly to about 31 mF·cm -2 .
[0091] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a carbon-coated 1T / 2H phase molybdenum disulfide flexible electrode, characterized in that: The following steps are involved: Placing the 1T / 2H phase molybdenum disulfide-carbon cloth electrode in a glucose solution for hydrothermal reaction to obtain the carbon-coated 1T / 2H phase molybdenum disulfide flexible electrode; The 1T / 2H phase molybdenum disulfide-carbon cloth electrode comprises a carbon cloth and a 1T / 2H phase molybdenum disulfide layer distributed on the surface of the carbon cloth.
2. The preparation method according to claim 1, characterized in that The dosage ratio of glucose to solvent in the glucose solution is (0.05-1) mol:60 mL.
3. The preparation method according to claim 2, characterized in that: The temperature of the hydrothermal reaction is 160-180° C. and the time is 2-6 hours.
4. The preparation method according to any one of claims 1 to 3, characterized in that: The preparation method of the 1T / 2H phase molybdenum disulfide-carbon cloth electrode comprises: Mixing a soluble molybdenum source, a soluble sulfur source and water to obtain a molybdenum disulfide precursor solution; The carbon cloth is placed in the molybdenum disulfide precursor solution to carry out a first hydrothermal reaction to obtain a 1T / 2H phase molybdenum disulfide-carbon cloth electrode.
5. The preparation method according to claim 4, characterized in that: The mass ratio of the soluble molybdenum source to water is (0.206-0.618):
90.
6. The preparation method according to claim 5, characterized in that: The mass ratio of the soluble sulfur source to water is (0.3806-1.1418):
90.
7. The preparation method according to claim 6, characterized in that: The soluble molybdenum source includes one or more of ammonium molybdate, sodium molybdate and molybdenum chloride; The soluble sulfur source includes one or more of thiourea, thioacetamide, ammonium sulfide and sodium sulfide.
8. The preparation method according to claim 4, characterized in that: The temperature of the first hydrothermal reaction is 180-200° C., and the time is 12-18 hours.
9. The carbon-coated 1T / 2H phase molybdenum disulfide flexible electrode prepared by the preparation method according to any one of claims 1 to 8, characterized in that: It comprises a carbon cloth and a 1T / 2H phase molybdenum disulfide layer and a carbon coating layer which are sequentially coated on the surface of the carbon cloth.
10. Use of the carbon-coated 1T / 2H phase molybdenum disulfide flexible electrode according to claim 9 in a supercapacitor.
Citation Information
Cited By
Two-dimensional 1T / 2H mixed-phase MoS2 / TiO2 nano composite catalyst as well as preparation and application thereof
CN122441461A