Screening method of tantalum capacitor and application thereof
By pre-aging the tantalum core of the anode in tantalum capacitors, anode tantalum cores with hidden defects are screened out, solving the problem of high failure rate after packaging and achieving a reduction in material costs and an improvement in production efficiency.
Patent Information
- Application Number
- CN202411167719.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-08
AI Technical Summary
Existing technologies cannot effectively screen out the hidden defective anode tantalum cores in tantalum capacitors, resulting in high failure rates and significant waste of material costs after packaging.
Before encapsulation, the anode tantalum core undergoes a pre-aging treatment. Anode tantalum cores with hidden defects are screened out by applying a rated voltage and electrolyte combination, forming a pre-aging device.
This improved the yield rate of packaged products, reduced material costs, and shortened production time.
Smart Images

Figure CN118919322A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of tantalum capacitor preparation, and in particular to a tantalum capacitor screening method and application thereof. Background Art
[0002] The anode core block in the tantalum capacitor is prepared by oxidizing tantalum metal to form a tantalum pentoxide oxide film. In the process of oxide film formation, there are inevitably more or less, large or small defects. The commonly used screening method is to screen out the anode tantalum core with obvious defects by the leakage current; however, for the anode tantalum core with hidden defects that does not cause leakage, it cannot be screened by whether the current is leaking. Instead, the packaged tantalum capacitor needs to be aged to screen out early failure products. The failure rate is more than 5% and can even reach more than 20% (related to the type of tantalum capacitor).
[0003] However, the raw material cost of tantalum capacitors before packaging is only tantalum powder and tantalum wire. The cost of tantalum core material of chip tantalum capacitor anode accounts for about 40% of the total material cost, while metal package tantalum capacitors only account for about 20%. Regardless of the type of packaging, when tantalum capacitors are aged after packaging, the failure rate will be too high, resulting in a large loss of raw material cost, which means increasing the material cost. Summary of the invention
[0004] To solve the above problems, the present application proposes a tantalum capacitor screening method and its application. The screening method is to directly pre-age the anode tantalum core, screen out the anode tantalum core with hidden defects, and then package it, thereby reducing material costs.
[0005] This application is implemented through the following technical solutions:
[0006] One of the purposes of the present application is to provide a method for screening tantalum capacitors, comprising the following steps:
[0007] Assemble the anode tantalum core pre-aging device to pre-age the anode tantalum core, and age it after packaging it into a tantalum capacitor;
[0008] The pre-aging device comprises an anode tantalum core, a diaphragm, an electrolyte, and a tantalum basin with a cathode layer coated on the inner bottom surface; the diaphragm is arranged between the cathode layer and the anode tantalum core, and the electrolyte is filled in the tantalum basin.
[0009] The screening method of tantalum capacitors provided in the present application directly pre-ages the anode tantalum core before packaging the tantalum capacitor, thereby screening out the anode tantalum cores with hidden defects (anode tantalum cores that show breakdown, flash or surface crystallization during pre-ageing). The screening method reduces production time, improves the qualified rate of products after packaging (more than 90%), and reduces material costs.
[0010] In some possible implementations, the pre-aging step includes:
[0011] The device is pre-aged by applying a voltage of 1.0 to 1.2 times the rated voltage at a temperature of 60° C. to 95° C. In this case, the tantalum anode core that may fail when used at the rated voltage can be effectively screened out.
[0012] In some possible implementations, a water bath is used to maintain the pre-aging temperature at 60° C. to 95° C.
[0013] Preferably, the pre-seasoning step comprises:
[0014] At a temperature of 90° C., the device is subjected to a pre-aging treatment by applying a voltage of 1.0 to 1.2 times the rated voltage. In this case, the pre-aging treatment is performed at 90° C., which is slightly higher than the maximum temperature of 85° C. for the rated voltage use of tantalum capacitors, and effectively eliminates the anode tantalum cores that may fail when used at the rated voltage.
[0015] Preferably, the pre-seasoning step comprises:
[0016] At a temperature of 90° C., a voltage of 1.1 times the rated voltage is applied to the device for pre-aging treatment. The pre-aging treatment is performed at this voltage of 1.1 times the rated voltage to further ensure the reliability of the anode tantalum core at a voltage slightly higher than the rated voltage without causing damage to the anode tantalum core.
[0017] In some possible implementations, the voltage lasts for 12 hours to 24 hours.
[0018] In some possible implementations, the power source of the voltage is a DC power source. In this case, the anode tantalum core is connected to the positive electrode of the DC power source through the tantalum wire, and the tantalum basin is connected to the negative electrode of the DC power source, and 1.0 to 1.2 times the rated voltage is applied.
[0019] In some possible implementations, the anode tantalum core includes an anode tantalum core of at least one tantalum electrolytic capacitor of model THC1-100V1900uF, CAK39H-75V330uF, and CAK35-125V100uF.
[0020] In some possible implementations, the electrolyte includes copper sulfate and sulfuric acid solution, and also includes ethylene glycol methyl ether and / or silica sol.
[0021] In some possible implementations, the silica sol has a solid content of 15 wt% to 25 wt% and a particle size of 70 nm to 80 nm.
[0022] In some other possible implementations, the silica sol is a product of Suzhou Silica Electronic Materials Co., Ltd.
[0023] In some possible implementations, the electrolyte is sulfuric acid solution, copper sulfate and ethylene glycol methyl ether; the mass ratio of the sulfuric acid solution, the copper sulfate and the ethylene glycol methyl ether is (70-90):1:(15-25).
[0024] In some possible implementations, the electrolyte is sulfuric acid solution, copper sulfate and silica sol;
[0025] The mass ratio of the sulfuric acid solution, the copper sulfate and the silica sol is (45-60):1:(15-25).
[0026] In some specific possible implementations, the mass fraction of sulfuric acid in the sulfuric acid solution is 38%.
[0027] In some possible implementations, during the pre-aging step, the volume of the electrolyte in the tantalum basin is maintained at 75% to 85% of the volume of the tantalum basin. In this case, the volume of the electrolyte changes slightly during the pre-aging process, which can ensure that the anode tantalum core is immersed and is not easy to overflow.
[0028] In some possible implementations, the thickness of the diaphragm is 0.1 mm to 0.2 mm.
[0029] In some possible implementations, the material of the diaphragm is at least one of polypropylene, polytetrafluoroethylene, and polyvinylidene fluoride.
[0030] In some possible implementations, the size of the diaphragm is larger than the size of the bottom surface of the tantalum basin; preferably, the difference between the length and width of the diaphragm and the tantalum basin is independently 1 mm to 5 mm.
[0031] In some possible implementations, the material of the cathode layer includes ruthenium dioxide, tantalum pentoxide and ultrafine carbon powder; the mass ratio of ruthenium dioxide, tantalum pentoxide and ultrafine carbon powder is (2-5): (1-3): 1. In this case, the cathode layer ensures the stability of charge transfer during the pre-aging process.
[0032] In some possible implementations, the average particle size of the ultrafine carbon powder is 20 nm to 50 nm.
[0033] In some possible implementations, the cathode layer has a thickness of 0.08 mm to 0.15 mm. Within this thickness range, the cathode can be guaranteed to have a large capacitance and not to fall off easily.
[0034] In some possible implementations, the size of the tantalum basin is (20-30)*(30-40)*(10-15).
[0035] The second purpose of the present application is to provide an application of the tantalum capacitor screening method provided in the present application in the field of tantalum capacitors. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] In order to more clearly illustrate the embodiments of the present drawings or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present drawings. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying any creative work.
[0037] Figure 1 Schematic diagram of the structure of the anode tantalum core pre-aging device in the embodiment of the present application.
[0038] Explanation of the reference numerals: 1 - anode tantalum core; 2 - diaphragm; 3 - tantalum basin.
[0039] The purpose, features and advantages of this figure will be further described in conjunction with the embodiments with reference to the accompanying drawings. DETAILED DESCRIPTION
[0040] In order to make the purpose, technical solutions and advantages of the present application clearer, the present application is described and illustrated below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not intended to limit the present application. Based on the embodiments provided in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application.
[0041] Obviously, the following descriptions are only some examples or embodiments of the present application. For ordinary technicians in this field, the present application can also be applied to other similar scenarios without creative work. In addition, it can also be understood that although the efforts made in this development process may be complicated and lengthy, for ordinary technicians in the field related to the content disclosed in this application, some changes in design, manufacturing or production based on the technical content disclosed in this application are just conventional technical means, and should not be understood as insufficient content disclosed in this application.
[0042] However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repeated descriptions of substantially the same structures may be omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate understanding by those skilled in the art. In addition, the following description is provided for those skilled in the art to fully understand the present application and is not intended to limit the subject matter described in the claims.
[0043] If not otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution, and all technical features and optional technical features of the present application can be combined with each other to form a new technical solution.
[0044] Example 1
[0045] Embodiment 1 proposes a method for screening tantalum capacitors, wherein the tantalum capacitor is a THC1-100V1900uF high-energy tantalum hybrid capacitor; comprising the following steps:
[0046] (1) Figure 1 As shown, assemble the anode tantalum core pre-aging device, Figure 1 In the figure, 1 is the anode tantalum core; 2 is the diaphragm; 3 is the tantalum basin:
[0047] ①Select a tantalum basin with a size of 30*40*10;
[0048] ②Preparing a coating liquid: mixing ruthenium dioxide, ruthenium trichloride, tantalum pentachloride, ultrafine carbon powder and ethanol in a mass ratio of 1:2:2:1:10 to obtain a coating liquid; the average particle size of the ultrafine carbon powder is 30 nm.
[0049] ③ The coating liquid is applied to the inner wall of the tantalum basin and then pyrolyzed to obtain a cathode layer with a thickness of 0.1 mm and a large capacity, that is, a tantalum basin with an inner wall coated with a cathode layer is obtained;
[0050] ④ Lay a 0.1mm thick polypropylene film (diaphragm) with a size of 31*41mm on a tantalum basin with a cathode layer coated on the inner wall, then place a 100v1900uF anode tantalum core on the polypropylene film, add an electrolyte accounting for 80% of the volume, and the anode tantalum core pre-aging device is assembled; wherein, the electrolyte is a mixed electrolyte of sulfuric acid solution, copper sulfate and ethylene glycol methyl ether with a mass ratio of 80:1:20, and the mass fraction of sulfuric acid in the sulfuric acid solution is 38%.
[0051] (2) Pre-aging: A DC power supply is used to supply voltage. The tantalum basin in the device is connected to the negative pole of the DC power supply, and the anode tantalum core is connected to the positive pole of the DC power supply through a tantalum wire. A 110V voltage is applied for pre-aging for 12 hours.
[0052] (3) Packaging: The pre-seasoned qualified anode tantalum core is packaged conventionally to obtain a tantalum capacitor.
[0053] (4) The packaged tantalum capacitor is subjected to conventional aging treatment.
[0054] Example 2
[0055] Embodiment 2 proposes a method for screening tantalum capacitors, wherein the tantalum capacitor is a CAK39H-75V330uF high-energy tantalum hybrid capacitor; the steps are basically the same as those in Embodiment 1, except that:
[0056] (1) Assemble the anode tantalum core pre-aging device:
[0057] ④ The anode tantalum core is a 75v330uF anode tantalum core;
[0058] The electrolyte is a mixed electrolyte of sulfuric acid solution, copper sulfate and silica sol with a mass ratio of 50:1:20.
[0059] (2) Pre-aging: Apply 83 V voltage for 24 h.
[0060] Example 3
[0061] Example 3 proposes a method for screening tantalum capacitors, wherein the tantalum capacitor is a CAK35-125V100uF high-energy tantalum hybrid capacitor; the steps are basically the same as those in Example 1, except that:
[0062] (1) Assemble the anode tantalum core pre-aging device:
[0063] ④ The anode tantalum core is a 125V100uF anode tantalum core;
[0064] The electrolyte is a mixed electrolyte of sulfuric acid solution, copper sulfate and ethylene glycol methyl ether in a mass ratio of 80:1:20, and the mass fraction of sulfuric acid in the sulfuric acid solution is 38%.
[0065] (2) Pre-aging: Apply 135 V voltage for 24 h.
[0066] Example 4
[0067] Example 4 proposes a method for screening tantalum capacitors. The tantalum capacitors are basically the same as those in Example 1, and the steps are also basically the same as those in Example 1, except that the thickness of the polypropylene film (diaphragm) is 0.2 mm.
[0068] Example 5
[0069] Example 5 proposes a method for screening tantalum capacitors. The tantalum capacitors are basically the same as those in Example 1, and the steps are basically the same as those in Example 1, except that the thickness of the cathode layer is 0.15 mm.
[0070] Comparative Example 1
[0071] Comparative Example 1 proposes a method for screening tantalum capacitors, the steps of which are basically the same as those of Example 1, except that the anode tantalum core is directly packaged and aged without going through steps (1) and (2).
[0072] Comparative Example 2
[0073] Comparative Example 2 proposes a method for screening tantalum capacitors, the steps of which are basically the same as those of Example 2, except that the anode tantalum core is directly packaged and aged without going through steps (1) and (2).
[0074] Comparative Example 3
[0075] Comparative Example 3 proposes a method for screening tantalum capacitors, the steps of which are basically the same as those of Example 3, except that the anode tantalum core is directly packaged and aged without going through steps (1) and (2).
[0076] Comparative Example 4
[0077] Comparative Example 4 proposes a method for screening tantalum capacitors. The tantalum capacitors are basically the same as those in Example 1, and the steps are also basically the same as those in Example 1, except that the thickness of the polypropylene film (diaphragm) is 0.08 mm.
[0078] Comparative Example 5
[0079] Comparative Example 5 proposes a method for screening tantalum capacitors. The tantalum capacitors are basically the same as those in Example 1, and the steps are also basically the same as those in Example 1, except that the thickness of the polypropylene film (diaphragm) is 0.25 mm.
[0080] Comparative Example 6
[0081] Comparative Example 6 proposes a method for screening tantalum capacitors. The tantalum capacitors are basically the same as those in Example 1, and the steps are also basically the same as those in Example 1, except that the thickness of the cathode layer is 0.06 mm.
[0082] Comparative Example 7
[0083] Comparative Example 7 proposes a method for screening tantalum capacitors. The tantalum capacitors are basically the same as those in Example 1, and the steps are also basically the same as those in Example 1, except that the thickness of the cathode layer is 0.2 mm.
[0084] In order to verify the progressiveness of the tantalum capacitor screening method provided in the embodiments of the present application, 100 tantalum anode cores made by the same process were tested using the screening methods provided in Examples 1 to 5 and Comparative Examples 1 to 7, and the number of qualified cores after pre-aging, the number of qualified products after aging, and the qualified rate of product packaging are shown in Table 1 below; the material costs are summarized in Table 2 below.
[0085] Table 1
[0086] Number of tantalum anode cores The number of qualified after pre-training Number of qualified candidates after veteranization Packaging qualification rate (%) Example 1 100 95 94 98.9 Example 2 100 94 94 100 Example 3 100 94 92 97.9 Example 4 100 96 93 96.9 Example 5 100 97 95 97.9 Comparative Example 1 100 × 92 90 Comparative Example 2 100 × 91 91 Comparative Example 3 100 × 92 92 Comparative Example 4 100 85 83 83% Comparative Example 5 100 98 90 90% Comparative Example 6 100 98 92 92% Comparative Example 7 100 99 93 93%
[0087] Table 2
[0088]
[0089]
[0090] Note: “×” in Table 1 and Table 2 means that this step is not performed.
[0091] From Table 1 and Table 2 above, at least the following conclusions can be drawn:
[0092] 1) As shown in Table 1, pre-aging can screen out most of the unqualified tantalum anode cores and improve the qualified rate of the packaging process. A small number of them fail in the subsequent aging due to potential hidden dangers caused during the assembly process, making it impossible to screen them out through pre-aging and can only be screened through the aging step after packaging.
[0093] 2) It can be seen from Table 2 that after pre-aging to remove the anode tantalum cores with hidden dangers, the packaging materials invested in the bad anode tantalum cores in the packaging process are reduced, so that the total material cost is greatly reduced.
[0094] 3) Comparison conclusions of Examples 4 and 5 and Comparative Examples 4 to 7. Too thin an isolation film will cause the anode tantalum core and the cathode to be insufficiently isolated, resulting in a short circuit in the core blocks and a large number of failures. Too thick an isolation film will not achieve the screening effect, and it will not be possible to remove bad core blocks in advance to reduce costs. The thickness of the cathode layer also affects the screening effect. When it is too thin or too thick, the screening effect is not good.
[0095] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A method for screening tantalum capacitors, characterized in that: The steps include: Assemble the anode tantalum core pre-aging device to pre-age the anode tantalum core, and age it after packaging it into a tantalum capacitor; The pre-aging device comprises an anode tantalum core, a diaphragm, an electrolyte, and a tantalum basin with a cathode layer coated on the inner bottom surface; the diaphragm is arranged between the cathode layer and the anode tantalum core, and the electrolyte is filled in the tantalum basin.
2. The method for screening tantalum capacitors according to claim 1, characterized in that: The pre-seasoning treatment step comprises: A voltage of 1.0 to 1.2 times the rated voltage is applied to the device at a temperature of 60° C. to 95° C. to perform a pre-aging treatment.
3. The method for screening tantalum capacitors according to claim 2, characterized in that: The voltage lasts for 12 hours to 24 hours.
4. The method for screening tantalum capacitors according to any one of claims 1 to 3, characterized in that: The electrolyte includes copper sulfate and sulfuric acid solution, and also includes ethylene glycol methyl ether and / or silica sol; And / or, the thickness of the diaphragm is 0.1 mm to 0.2 mm; And / or, the cathode layer has a thickness of 0.08 mm to 0.15 mm.
5. The method for screening tantalum capacitors according to claim 4, characterized in that: In the pre-aging step, the volume of the electrolyte in the tantalum basin is maintained at 78% to 81% of the volume of the tantalum basin.
6. The method for screening tantalum capacitors according to any one of claims 1 to 3, characterized in that: The electrolyte is sulfuric acid solution, copper sulfate and ethylene glycol methyl ether; the mass ratio of the sulfuric acid solution, the copper sulfate and the ethylene glycol methyl ether is (70-90):1:(15-25).
7. The method for screening tantalum capacitors according to any one of claims 1 to 3, characterized in that: The electrolyte is a sulfuric acid solution, copper sulfate and silica sol; the mass ratio of the sulfuric acid solution, the copper sulfate and the silica sol is (45-60):1:(15-25).
8. The method for screening tantalum capacitors according to claim 4, characterized in that: The material of the diaphragm is at least one of polypropylene, polytetrafluoroethylene and polyvinylidene fluoride.
9. The method for screening tantalum capacitors according to claim 4, characterized in that: The material of the cathode layer includes ruthenium dioxide, tantalum pentoxide, and ultrafine carbon powder; The mass ratio of ruthenium dioxide, tantalum pentoxide and ultrafine carbon powder is (2-5):(1-3):
1.
10. Application of the tantalum capacitor screening method according to any one of claims 1 to 9 in the field of tantalum capacitors.