HEMT device and preparation method thereof

By adopting the structure of annular isolation layer and cap layer in GaN HEMT devices, the device isolation process is simplified, the problem of complex process steps and high cost in the prior art is solved, and the device performance is improved and cost reduction is achieved.

CN118919550APending Publication Date: 2024-11-08CHINA RESOURCES MICROELECTRONICS (CHONGQING) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310506533.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-06
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the prior art, the process steps for making GaN HEMT devices individually have complex processes, resulting in increased costs.

Method used

Using a structure of multiple annular isolation layers and cap layers, the annular isolation layer is formed to etch and surround the main device area, and a voltage lower than the substrate is applied on the isolation electrode to achieve isolation between devices, simplify process steps and reduce costs. .

Benefits of technology

The mask or ion implantation isolation process that separates the device isolation structure is eliminated, simplifies the production steps, reduces costs and thermal budgets, and improves device performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919550A_ABST
    Figure CN118919550A_ABST
Patent Text Reader

Abstract

The invention provides an HEMT device and a preparation method thereof, the HEMT device comprises a semiconductor structure, an annular isolation layer, a cap layer, a source electrode, a drain electrode, a grid electrode and an isolation electrode, the semiconductor structure comprises a substrate, a channel layer and a barrier layer which are stacked in sequence, the annular isolation layer is located on the upper surface of the barrier layer, and an area surrounded by the annular isolation layer serves as a main body device area; the cap layer is located on the upper surface of the barrier layer in the main body device region and is spaced from the annular isolation layer by a preset distance; the source electrode and the drain electrode are electrically connected with the barrier layer of the main body device region; the cap layer is located between the source electrode and the drain electrode and is spaced from the source electrode and the drain electrode by a preset distance; the grid electrode is located on the upper surface of the cap layer and electrically connected with the cap layer. The isolation electrode is located on the upper surface of the annular isolation layer and electrically connected with the annular isolation layer. According to the invention, the main body device region is defined by arranging the annular isolation layer which is synchronously formed with the cap layer, so that the process steps are simplified while device isolation is realized, and the cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of semiconductor integrated circuit manufacturing and relates to a HEMT device and a preparation method thereof. Background Art

[0002] The third-generation semiconductor material gallium nitride (GaN) has become an ideal candidate for high-voltage and high-frequency applications due to its wide bandgap and high electron saturation velocity. Gallium nitride semiconductors can withstand stronger currents and higher voltages than silicon semiconductors, and can achieve higher power density, thus showing ample market potential in radars, base stations, cable TV, fast charging, and DC-DC converters, and will become a new generation of cost-competitive consumer power electronics products.

[0003] High-power devices and their integrated circuits are often made up of many small devices connected together. Usually, the devices need to be isolated to block the flow of carriers between the devices so that each device can work independently. For GaN devices, there are two common methods for device isolation, such as Figure 1 As shown, it is a schematic diagram of a cross-sectional structure of a high electron mobility transistor (HEMT) device, including a semiconductor structure 01, a substrate 011, a channel layer 012, a barrier layer 013, an isolation channel 014, a cap layer 02, a source 03, a drain 04 and a gate 05. A mesa is formed by etching GaN, and a two-dimensional electron gas channel is cut to achieve device isolation; Figure 2 , which is another schematic diagram of the cross-sectional structure of a HEMT device, including a semiconductor structure 01, a substrate 011, a channel layer 012, a barrier layer 013, a high-resistance isolation region 015, a cap layer 02, a source 03, a drain 04 and a gate 05. A high-resistance region is formed in the barrier layer by ion implantation to cut off the flow of the two-dimensional electron gas, thereby achieving device isolation.

[0004] For enhancement-mode GaN devices, PGaN-gate GaN devices (PGaN devices for short) are usually manufactured by growing a GaN epitaxial layer on a substrate, growing an AlGaN barrier layer on the GaN epitaxial layer, and then growing a P-type GaN layer on the AlGaN barrier layer. Device isolation is formed by mesa etching or ion implantation, and then a PGaN gate is formed by etching PGaN. The isolation structure of the device is manufactured separately, which makes the process steps more complicated and increases the manufacturing cost.

[0005] Therefore, there is an urgent need to find a HEMT device that simplifies the manufacturing process and reduces the manufacturing cost. Summary of the invention

[0006] In view of the above-mentioned shortcomings of the prior art, an object of the present invention is to provide a HEMT device and a method for manufacturing the same, so as to solve the problem that the isolation structure of the HEMT device is separately manufactured in the prior art, resulting in an increase in the number of process steps and an increase in the manufacturing cost of the device.

[0007] To achieve the above-mentioned object and other related objects, the present invention provides a HEMT device, comprising:

[0008] A semiconductor structure comprising a substrate, a channel layer and a barrier layer stacked in sequence;

[0009] A plurality of annular isolation layers are located on the upper surface of the barrier layer, and the area surrounded by the annular isolation layers serves as a main device area;

[0010] a cap layer, located on an upper surface of the barrier layer in the main device region and spaced apart from the annular isolation layer by a preset distance;

[0011] The source and the drain are both electrically connected to the barrier layer on the upper surface of the main device region, and the cap layer is located between the source and the drain and is spaced a preset distance from the source and the drain;

[0012] A gate and an isolation electrode, wherein the gate is located on the upper surface of the cap layer and is electrically connected to the cap layer, and the isolation electrode is located on the upper surface of the annular isolation layer and is electrically connected to the annular isolation layer.

[0013] Optionally, a PN junction is formed between the annular isolation layer and the barrier layer, and a PN junction is formed between the cap layer and the barrier layer.

[0014] Optionally, the material of the annular isolation layer includes P-type GaN or P-type AlGaN, and the material of the cap layer includes P-type GaN or P-type AlGaN.

[0015] Optionally, the width of the annular isolation layer ranges from 0.5 μm to 10 μm.

[0016] Optionally, the thickness of the annular isolation layer is not less than the thickness of the cap layer.

[0017] Optionally, the cap layer surrounds the source.

[0018] Optionally, the doping concentration of the annular isolation layer is not lower than the doping concentration of the cap layer.

[0019] Optionally, the isolation electrode has the same potential as the substrate or the source.

[0020] Optionally, the potential of the isolation electrode is lower than the potential of the substrate.

[0021] The present invention also provides a method for preparing a HEMT device, comprising the following steps:

[0022] Providing a semiconductor structure including a substrate, a channel layer and a barrier layer stacked in sequence, and forming an isolation material layer on the upper surface of the barrier layer;

[0023] Etching the isolation material layer to obtain a plurality of annular isolation layers and cap layers, wherein the annular isolation layer surrounds an area as a main device region, and the cap layer is located on an upper surface of the main device region and is spaced a preset distance from the annular isolation layer;

[0024] A source is formed which is electrically connected to the barrier layer in the main device region, a drain is formed which is electrically connected to the barrier layer in the main device region, a gate is formed which is electrically connected to the cap layer, and an isolation electrode is formed which is electrically connected to the annular isolation layer, wherein the cap layer is located between the source and the drain and is spaced a preset distance from both the source and the drain.

[0025] As described above, the HEMT device and its preparation method of the present invention form the annular isolation layer while forming the cap layer electrically connected to the gate, the surrounding area of ​​the annular isolation layer is used as the main device area, and the isolation electrode electrically connected to the annular isolation layer is formed, and the two-dimensional electron gas density of the channel area below the annular isolation layer is exhausted by the annular isolation layer, and then the channel area in the main device area is isolated from the channel area outside the annular isolation layer, so as to achieve mutual isolation between different devices on the semiconductor structure, save the mask or ion implantation isolation process of separately making the device isolation structure, simplify the process steps of making the device, and reduce the cost and thermal budget. In addition, by applying a voltage lower than the substrate on the isolation electrode, the isolation effect between the channel area of ​​the main device area and the channel area outside the annular isolation layer can be enhanced, the performance of the device can be improved, and it has a high industrial utilization value. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 Shown is a schematic diagram of the cross-sectional structure of a HEMT device.

[0027] Figure 2 Shown is a schematic diagram of the cross-sectional structure of another HEMT device.

[0028] Figure 3 It is a schematic diagram of a top surface structure of the HEMT device of the present invention.

[0029] Figure 4 Another schematic diagram of the top surface structure of the HEMT device of the present invention is shown.

[0030] Figure 5The process flow chart of the HEMT device manufacturing method of the present invention is shown.

[0031] Figure 6 The cross-sectional structure schematic diagram shows the semiconductor structure of the method for preparing the HEMT device of the present invention.

[0032] Figure 7 It is a schematic diagram showing the cross-sectional structure after forming an isolation material layer in the method for preparing a HEMT device of the present invention.

[0033] Figure 8 It is a schematic diagram showing the cross-sectional structure after forming the annular isolation layer and the cap layer in the method for preparing the HEMT device of the present invention.

[0034] Fig. 9 It is a schematic diagram showing the cross-sectional structure after forming the isolation electrode in the method for preparing the HEMT device of the present invention.

[0035] Description of Figure Numbers

[0036] 01 Semiconductor structure

[0037] 011 Substrate

[0038] 012 Channel layer

[0039] 013 Barrier layer

[0040] 014 Isolation Channel

[0041] 015 High resistance isolation area

[0042] 02 Cap layer

[0043] 03 Source

[0044] 04 Drain

[0045] 05 Gate

[0046] 1 Semiconductor structure

[0047] 11 Substrate

[0048] 12 Channel layer

[0049] 13 Barrier layer

[0050] 2 Annular isolation layer

[0051] 20 Isolation material layer

[0052] 21 Main device area

[0053] 3 Cap layer

[0054] 4 Source

[0055] 5 Drain

[0056] 6. Gate

[0057] 7 Isolation Electrode DETAILED DESCRIPTION

[0058] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0059] See also Figures 3 to 9 It should be noted that the illustrations provided in this embodiment are only used to illustrate the basic concept of the present invention in a schematic manner, and the drawings only show components related to the present invention rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.

[0060] Embodiment 1

[0061] This embodiment provides a HEMT device, such as Figure 3 and Figure 4 As shown, they are respectively a schematic diagram of a top surface structure of the HEMT device and another schematic diagram of the top surface structure of the HEMT device, comprising a semiconductor structure 1, an annular isolation layer 2, a cap layer 3, a source 4, a drain 5, a gate 6 and an isolation electrode 7, wherein the semiconductor structure 1 comprises a substrate 11, a channel layer 12 and a barrier layer 13 stacked in sequence; a plurality of the annular isolation layers 2 are located on the upper surface of the barrier layer 13, and the area surrounded by the annular isolation layer 2 serves as a main device region 21; the cap layer 3 is located on the upper surface of the barrier layer 13 in the main device region 21 and is spaced apart from the annular isolation layer 2 by a preset distance; the source 4 and the drain 5 are both electrically connected to the barrier layer 13 on the upper surface of the main device region 21, the cap layer 3 is located between the source 4 and the drain 5 and is spaced apart from the source 4 and the drain 5 by a preset distance; the gate 6 is located on the upper surface of the cap layer 3 and is electrically connected to the cap layer 3, and the isolation electrode 7 is located on the upper surface of the annular isolation layer 2 and is electrically connected to the annular isolation layer 2.

[0062] Specifically, the material of the substrate 11 includes sapphire, SiC, Si, GaN, diamond, Al2O3 or other suitable materials.

[0063] Specifically, while ensuring device performance, the shape, size and thickness of the substrate 11 can be selected according to actual conditions and are not limited here.

[0064] Specifically, the material of the channel layer 12 includes GaN, AlGaN, InGaN or other suitable semiconductor materials. In this embodiment, a GaN thin film is used as the channel layer 12 .

[0065] Specifically, a buffer layer (not shown) is further disposed between the channel layers 12 to improve the quality of the film layer forming the channel layer 12 . The material of the buffer layer includes AlN, AlGaN, GaN, InN or other suitable semiconductor materials.

[0066] Specifically, while ensuring the film quality of the channel layer 12, the buffer layer can be a single-layer film structure or a composite film structure. For example, the buffer layer can be a GaN single-layer film or an AlN / AlGaN composite film.

[0067] Specifically, under the condition of ensuring the film quality of the channel layer 12 , the thickness, size and shape of the buffer layer can be selected according to actual conditions, and are not limited here.

[0068] Specifically, the material of the barrier layer 13 includes In x Al y Ga 1-x-y N、Al x Ga 1-x N、In x Al 1-x N or other suitable materials. In this embodiment, Al x Ga 1-x N serves as the barrier layer 13 .

[0069] Specifically, under the condition of ensuring device performance, the thickness of the barrier layer 13 can be selected according to actual conditions and is not limited here; the thickness of the channel layer 12 can be selected according to actual conditions and is not limited here.

[0070] Specifically, due to the difference in material properties between the channel layer 12 and the barrier layer 13 , a polarization phenomenon occurs at the interface between the barrier layer 13 and the channel layer 12 , and then a two-dimensional electron gas is generated at the interface between the channel layer 12 and the barrier layer 13 .

[0071] As an example, a PN junction is formed between the annular isolation layer 2 and the barrier layer 13 .

[0072] Specifically, the direction of the built-in electric field of the PN junction between the annular isolation layer 2 and the barrier layer 13 is directed from the barrier layer 13 to the annular isolation layer 2 .

[0073] As an example, the width of the annular isolation layer 2 ranges from 0.5 μm to 10 μm. For example, the width of the annular isolation layer 2 can be 0.5 μm, 1 μm, 4 μm, 8 μm, or 10 μm. In this embodiment, the width of the annular isolation layer 2 is between 0.5 μm and 5 μm to save chip area. The width here refers to the length of the cross section of the annular isolation layer 2 parallel to the barrier layer 13.

[0074] Specifically, the annular isolation layer 2 completely depletes the two-dimensional electron gas density in the channel region below the annular isolation layer 2, thereby achieving isolation of the channel region, and then achieving isolation between the two-dimensional electron gas in the main device region 21 and the two-dimensional electron gas outside the annular isolation layer 2, thereby achieving isolation between devices in different main device regions 21.

[0075] As an example, the material of the annular isolation layer 2 includes P-type GaN, P-type AlGaN or other semiconductor materials that can completely deplete the two-dimensional electron gas density at the interface between the barrier layer 13 and the channel layer 12 below the layer. In this embodiment, a P-type GaN layer is used as the annular isolation layer 2.

[0076] As an example, a PN junction is formed between the cap layer 3 and the barrier layer 13 .

[0077] Specifically, the direction of the built-in electric field of the PN junction between the cap layer 3 and the barrier layer 13 is directed from the barrier layer 13 to the cap layer 3 .

[0078] Specifically, the cap layer 3 completely depletes the density of the two-dimensional electron gas in the channel region below the cap layer 3 to achieve isolation of the channel region, and then isolates the two-dimensional electron gas electrically connected to the source 4 from the two-dimensional electron gas electrically connected to the drain 5, thereby isolating the channel region between the source 4 and the drain 5.

[0079] Specifically, under the condition that the device performance is guaranteed and the cap layer 3 can deplete the two-dimensional electron gas density in the channel region below the cap layer 3 , the size and shape of the cap layer 3 can be selected according to actual conditions.

[0080] As an example, the cap layer 3 is made of P-type GaN, P-type AlGaN or other semiconductor materials that can completely deplete the two-dimensional electron gas channel at the interface between the barrier layer 13 and the channel layer 12 below the layer. In this embodiment, a P-type GaN layer is used as the cap layer 3.

[0081] As an example, the thickness of the annular isolation layer 2 is not less than the thickness of the cap layer 3. In this embodiment, the thickness of the cap layer 3 is the same as the thickness of the annular isolation layer 2.

[0082] Specifically, while ensuring device performance, the size and shape of the main device area 21 can be set according to actual conditions and are no longer limited here; the distance between the annular isolation layer 2 and the cap layer 3 can be set according to actual conditions and are no longer limited here.

[0083] As an example, the cap layer 3 surrounds the source 4 to isolate the two-dimensional electron gas under the source 4 from the two-dimensional electron gas under the drain 5, that is, through the setting of the cap layer 3, the two-dimensional electron gas density under the cap layer 3 is depleted, so that the channel region outside the cap layer 3 in the main device area 21 is isolated from the channel region under the source 4, and then the isolation of the channel region between the source 4 and the drain 5 is achieved.

[0084] Specifically, under the condition that the density of the two-dimensional electron gas below the cap layer 3 is ensured to be depleted, the doping concentration of the cap layer 3 can be selected according to actual conditions, and is not limited here.

[0085] Specifically, the doping concentration of the annular isolation layer 2 is not lower than the doping concentration of the cap layer 3, so that the isolation effect of the annular isolation layer 2 is stronger than the isolation effect of the cap layer 3. In this embodiment, the doping concentration of the cap layer 3 is the same as the doping concentration of the annular isolation layer 2.

[0086] Specifically, under the condition that the devices in different main device regions 21 can be isolated from each other, two adjacent annular isolation layers 2 can be adjacent to each other or separated by a preset distance.

[0087] Specifically, an ohmic contact is formed between the source electrode 4 and the barrier layer 13 to reduce the contact resistance of the device, thereby reducing the on-resistance of the device; an ohmic contact is formed between the drain electrode 5 and the barrier layer 13 to reduce the contact resistance of the device, thereby reducing the on-resistance of the device.

[0088] Specifically, the material of the source electrode 4 includes one of titanium, titanium nitride, silver, gold, copper, aluminum, nickel and tungsten, or other suitable conductive materials; the material of the drain electrode includes one of titanium, titanium nitride, silver, gold, copper, aluminum, nickel and tungsten, or other suitable conductive materials.

[0089] Specifically, an ohmic contact is formed between the gate 6 and the cap layer 3, so that the gate 6 can control the density of the two-dimensional electron gas below the cap layer 3; an ohmic contact is formed between the isolation electrode 7 and the annular isolation layer 2, so that the isolation electrode 7 can control the density of the two-dimensional electron gas below the annular isolation layer 2.

[0090] Specifically, the material of the gate 6 includes one of titanium, titanium nitride, silver, gold, copper, aluminum, nickel and tungsten, or other suitable conductive materials; the material of the isolation electrode 7 includes one of titanium, titanium nitride, silver, gold, copper, aluminum, nickel and tungsten, or other suitable conductive materials.

[0091] As an example, the isolation electrode 7 has the same potential as the substrate 11 or the source 4, so that the annular isolation layer 2 is at a low potential, preventing the shutdown of the channel region below the annular isolation layer 2 from being disturbed by the induced voltage and affecting the performance of the device.

[0092] As an example, the potential of the isolation electrode 7 is lower than the potential of the substrate 11, so that the annular isolation layer 2 is at a lower potential, so that the density of the two-dimensional electron gas under the annular isolation layer 2 is depleted more thoroughly, thereby enhancing the isolation effect between the two-dimensional electron gas outside the annular isolation layer 2 and the two-dimensional electron gas in each of the main device areas 21, thereby enhancing the device performance.

[0093] Specifically, when the potential of the isolation electrode 7 is lower than the potential of the substrate 11 , a circuit for controlling the isolation electrode 7 is further provided in the device to control the potential of the isolation electrode 7 .

[0094] Specifically, the annular isolation layer 2 is provided on the upper surface of the barrier layer 13, and holes are injected into the two-dimensional electron gas below the annular isolation layer 2 by utilizing the annular isolation layer 2, so that the density of the two-dimensional electron gas below the annular isolation layer 2 is depleted, thereby achieving isolation between the two-dimensional electron gas in each of the main device regions 21 and the two-dimensional electron gas outside the annular isolation layer 2.

[0095] Specifically, by setting the potential of the isolation electrode 7 and making the potential of the isolation electrode 7 not higher than the potential of the substrate 11, the density of the two-dimensional electron gas under the annular isolation layer 2 is depleted more thoroughly, thereby enhancing the isolation effect between the two-dimensional electron gas in the main device area 21 and the two-dimensional electron gas outside the annular isolation layer 2.

[0096] Specifically, by setting the annular isolation layer 2, the density of the two-dimensional electron gas below the annular isolation layer 2 is exhausted, so that the two-dimensional electron gas in the main device area 21 is isolated from the two-dimensional electron gas outside the annular isolation layer 2, and at the same time, isolation between different main device areas 21 is achieved, and then isolation between devices is achieved.

[0097] The HEMT device of this embodiment is provided with the annular isolation layer 2 on the upper surface of the barrier layer 13, and the isolation electrode 7 electrically connected to the annular isolation layer 2 is provided. The annular isolation layer 2 is used to inject holes into the two-dimensional electron gas below the annular isolation layer 2, so that the density of the two-dimensional electron gas below the annular isolation layer 2 is depleted, and then the two-dimensional electron gas in the main device area 21 is isolated from the two-dimensional electron gas outside the annular isolation layer 2, so as to achieve isolation between devices; by applying a voltage lower than that of the substrate 11 to the isolation electrode 7, the isolation effect between the two-dimensional electron gas in the main device area 21 and the two-dimensional electron gas outside the annular isolation layer 2 is enhanced, thereby improving the performance of the device.

[0098] Embodiment 2

[0099] This embodiment provides a method for preparing a HEMT device, such as Figure 5 FIG. 1 is a process flow chart of the method for preparing the HEMT device, comprising the following steps:

[0100] S1: providing a semiconductor structure including a substrate, a channel layer and a barrier layer stacked in sequence, and forming an isolation material layer on an upper surface of the barrier layer;

[0101] S2: etching the isolation material layer to obtain a plurality of annular isolation layers and cap layers, wherein the area surrounded by the annular isolation layer serves as a main device region, and the cap layer is located on an upper surface of the main device region and is spaced a preset distance from the annular isolation layer;

[0102] S3: forming a source electrode electrically connected to the barrier layer in the main device region, forming a drain electrode electrically connected to the barrier layer in the main device region, forming a gate electrode electrically connected to the cap layer, and forming an isolation electrode electrically connected to the annular isolation layer, wherein the cap layer is located between the source electrode and the drain electrode and is spaced apart from the source electrode and the drain electrode by a preset distance.

[0103] See also Figure 6 to Figure 7 , performing the step S1: providing a semiconductor structure 1 including a substrate 11 , a channel layer 12 and a barrier layer 13 stacked in sequence, and forming an isolation material layer 20 on the upper surface of the barrier layer 13 .

[0104] Specifically, Figure 6 , which is a schematic diagram of the cross-sectional structure of the semiconductor structure 1 . The semiconductor structure 1 is further provided with a buffer layer, and the buffer layer is located between the channel layer 12 and the substrate 11 .

[0105] Specifically, the method of forming the isolation material layer 20 includes chemical vapor deposition, physical vapor deposition or other suitable methods.

[0106] Specifically, the material of the isolation material layer 20 includes P-type GaN, P-type AlGaN or other suitable semiconductor materials. In this embodiment, a P-type GaN layer is used as the isolation material layer 20 .

[0107] Please see again Figure 8 , perform the step S2: etch the isolation material layer 20 to obtain a plurality of annular isolation layers 2 and cap layers 3, wherein the surrounding area of ​​the annular isolation layer 2 serves as the main device area 21 (see Figure 8 The cap layer 3 is located on the upper surface of the main device region 21 and is spaced apart from the annular isolation layer 2 by a preset distance.

[0108] Specifically, before etching the isolation material layer 20 , a step of forming a patterned photoresist layer on the upper surface of the isolation material layer 20 is also included.

[0109] Specifically, the method of forming the photoresist layer includes coating or other suitable methods.

[0110] Specifically, patterning the photoresist layer includes the following steps: providing a mask with a preset pattern, and aligning the mask with the semiconductor structure 1 after the photoresist layer is formed; exposing the photoresist layer for a preset time based on the mask, and performing a developing process on the exposed photoresist layer to obtain the patterned photoresist layer.

[0111] Specifically, the alignment of the photomask and the development of the photoresist layer are conventional processes, which will not be described in detail here.

[0112] Specifically, the method of etching the isolation material layer 20 includes dry etching, wet etching or other suitable methods.

[0113] Specifically, after forming the annular isolation layer 2 and the cap layer 3, the method further includes a step of removing the photoresist layer.

[0114] Specifically, the method for removing the photoresist layer is a conventional photoresist removal method, which will not be described in detail here.

[0115] Specifically, by forming the annular isolation layer 2 and the cap layer 3 simultaneously, the process steps are simplified and the manufacturing cost of the device is saved.

[0116] Specifically, the doping concentration of the formed annular isolation layer 2 is not lower than the doping concentration of the cap layer 3. When the doping concentration of the cap layer 3 is higher than the doping concentration of the annular isolation layer 2, the annular isolation layer 3 needs to be doped to increase the doping concentration of the annular isolation layer 2 so that the doping concentration of the annular isolation layer 2 is equal to or higher than the doping concentration of the cap layer 3.

[0117] Specifically, the thickness of the annular isolation layer 2 is not less than the thickness of the cap layer 3 .

[0118] See also Fig. 9 , perform step S3: form a source 4 electrically connected to the barrier layer 13 in the main device area 21, form a drain 5 electrically connected to the barrier layer 13 in the main device area 21, form a gate 6 electrically connected to the cap layer 3, and form an isolation electrode 7 electrically connected to the annular isolation layer 2, wherein the cap layer 3 is located between the source 4 and the drain 5 and is spaced a preset distance from the source 4 and the drain 5.

[0119] Specifically, the method for forming the source 4 includes sputtering, physical vapor deposition, chemical vapor deposition, metal compound vapor deposition, molecular beam epitaxy, atomic vapor deposition, atomic layer deposition or other suitable methods; the method for forming the drain 5 includes sputtering, physical vapor deposition, chemical vapor deposition, metal compound vapor deposition, molecular beam epitaxy, atomic vapor deposition, atomic layer deposition or other suitable methods.

[0120] Specifically, while ensuring device performance, the distance between the source 4 and the cap layer 3 can be selected according to actual conditions and is not limited here; the distance between the drain 5 and the cap layer 3 can be selected according to actual conditions and is not limited here.

[0121] Specifically, the method for forming the gate 6 includes sputtering, physical vapor deposition, chemical vapor deposition, metal compound vapor deposition, molecular beam epitaxy, atomic vapor deposition, atomic layer deposition or other suitable methods; the method for forming the isolation electrode 7 includes sputtering, physical vapor deposition, chemical vapor deposition, metal compound vapor deposition, molecular beam epitaxy, atomic vapor deposition, atomic layer deposition or other suitable methods. In this embodiment, the source 4, the drain 5, the gate 6 and the isolation electrode 7 are formed simultaneously.

[0122] Specifically, the annular isolation layer 2 is formed on the upper surface of the barrier layer 13, and holes are injected into the two-dimensional electron gas below the annular isolation layer 2 by using the annular isolation layer 2 to deplete the two-dimensional electron gas density below the annular isolation layer 2, thereby achieving isolation between devices. At the same time, there is no need to cut off the two-dimensional electron gas around the main device area 21, or to perform ion implantation on the barrier layer 13 around the main device area 21 to produce a high-resistance area surrounding the main device area 21, thereby eliminating the process of separately producing a device isolation structure, reducing costs and thermal budgets, and improving the market competitiveness of products.

[0123] Specifically, by simultaneously forming the cap layer 3 and the annular isolation layer 2, the etching mask or ion implantation mask for separately manufacturing the isolation structure of the device can be saved, and then a photolithography process (including photolithography, exposure, development, feature size measurement, alignment measurement, etc.), an etching process or an ion implantation process, a degumming and cleaning process can be omitted, thereby saving the time and cost of manufacturing the device and improving production efficiency.

[0124] The method for preparing the HEMT device of this embodiment forms the annular isolation layer 3 simultaneously with the formation of the cap layer 3, and utilizes the annular isolation layer 2 to deplete the two-dimensional electron gas density below the annular isolation layer 2, thereby realizing the isolation between the two-dimensional electron gas in the main device area 21 and the two-dimensional electron gas outside the annular isolation layer 2, thereby realizing the isolation of the device, simplifying the process steps of manufacturing the device, and reducing the manufacturing cost and thermal budget.

[0125] In summary, the HEMT device and its preparation method of the present invention form an annular isolation layer defining the main device area while forming a cap layer electrically connected to the gate, and form an isolation electrode electrically connected to the annular isolation layer, so that the annular isolation layer depletes the two-dimensional electron gas density below the annular isolation layer, and then the two-dimensional electron gas in the main device area is isolated from the two-dimensional electron gas outside the annular isolation layer, thereby realizing mutual isolation between devices, eliminating the need for a mask or ion implantation isolation process for separately making a device isolation structure, simplifying the process steps for making the device, and reducing costs and thermal budgets. In addition, applying a voltage lower than the substrate to the isolation electrode can enhance the isolation effect between the two-dimensional electron gas in the main device area and the two-dimensional electron gas outside the annular isolation layer, thereby improving the performance of the device. Therefore, the present invention effectively overcomes the various shortcomings of the prior art and has a high industrial utilization value.

[0126] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A HEMT device, characterized in that: include: A semiconductor structure comprising a substrate, a channel layer and a barrier layer stacked in sequence; A plurality of annular isolation layers are located on the upper surface of the barrier layer, and the area surrounded by the annular isolation layers serves as a main device area; a cap layer, located on an upper surface of the barrier layer in the main device region and spaced apart from the annular isolation layer by a preset distance; The source and the drain are both electrically connected to the barrier layer on the upper surface of the main device region, and the cap layer is located between the source and the drain and is spaced a preset distance from the source and the drain; A gate and an isolation electrode, wherein the gate is located on the upper surface of the cap layer and is electrically connected to the cap layer, and the isolation electrode is located on the upper surface of the annular isolation layer and is electrically connected to the annular isolation layer.

2. The HEMT device according to claim 1, characterized in that: A PN junction is formed between the annular isolation layer and the barrier layer, and a PN junction is formed between the cap layer and the barrier layer.

3. The HEMT device according to claim 1, characterized in that: The material of the annular isolation layer includes P-type GaN and P-type AlGaN, and the material of the cap layer includes P-type GaN and P-type AlGaN.

4. The HEMT device according to claim 1, characterized in that: The width of the annular isolation layer ranges from 0.5 μm to 10 μm.

5. The HEMT device according to claim 1, characterized in that: The thickness of the annular isolation layer is not less than the thickness of the cap layer.

6. The HEMT device according to claim 1, characterized in that: The cap layer surrounds the source electrode.

7. The HEMT device according to claim 1, characterized in that: The doping concentration of the annular isolation layer is not lower than the doping concentration of the cap layer.

8. The HEMT device according to claim 1, characterized in that: The isolation electrode has the same potential as the substrate or the source.

9. The HEMT device according to claim 1, characterized in that: The potential of the isolation electrode is lower than the potential of the substrate.

10. A method for preparing a HEMT device, characterized in that: The following steps are involved: Providing a semiconductor structure including a substrate, a channel layer and a barrier layer stacked in sequence, and forming an isolation material layer on the upper surface of the barrier layer; Etching the isolation material layer to obtain a plurality of annular isolation layers and cap layers, wherein the annular isolation layer surrounds an area as a main device region, and the cap layer is located on an upper surface of the main device region and is spaced a preset distance from the annular isolation layer; A source is formed which is electrically connected to the barrier layer in the main device region, a drain is formed which is electrically connected to the barrier layer in the main device region, a gate is formed which is electrically connected to the cap layer, and an isolation electrode is formed which is electrically connected to the annular isolation layer, wherein the cap layer is located between the source and the drain and is spaced a preset distance from both the source and the drain.