Negative active material, negative plate and nickel-zinc battery

By using a specific composition of negative electrode active material and protective glue layer in the nickel-zinc battery negative electrode sheet, the powder loss problem of negative electrode sheet is solved, and the storage performance and cycle life of the battery are improved.

CN118919651AInactive Publication Date: 2024-11-08SHENZHEN HIGHPOWER TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411419230.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-12
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The negative electrode sheet of nickel-zinc battery is prone to powder loss after cutting, resulting in a decrease in negative electrode active substances, affecting the storage performance and cycle life of the battery.

Method used

A negative electrode active material is used, containing 58%~68% ZnO, 20%~30% Zn, 0.01%~1% In2O3, 0.08%~2.88% Bi2O3, 3%~5% Al2O3, 1%~2% conductive substance , 3%~5% binder, 0.3%~0.5% thickener and 1%~2% dispersant, where the binder is a mixture of SBR and/or PTFE, and a protective glue is added to the edge of the negative electrode sheet. layer to enhance adhesion and adhesion.

Benefits of technology

Effectively slow down or avoid powder loss of the negative electrode sheet, prevent the negative electrode powder from being transferred to the positive electrode, and extend the storage performance and cycle life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919651A_ABST
    Figure CN118919651A_ABST
Patent Text Reader

Abstract

The invention relates to a negative active material, a negative plate and a nickel-zinc battery. The negative active material comprises the following components in percentage by weight: 58-68% of ZnO; 20 to 30% of Zn; 0.01% to 1% of In2O3; 0.08% to 2.88% of Bi2O3; 3 to 5 percent of Al2O3; 1-2% of a conductive substance; 3-5% of a binder; 0.3%-0.5% of a thickening agent; 1-2% of a dispersant; wherein the binder comprises SBR (Styrene Butadiene Rubber) and / or PTFE (Polytetrafluoroethylene). By improving the components of the negative electrode active material, the adhesive force of the negative electrode active material can be enhanced, the cutting burr and powder falling phenomenon of the negative electrode plate can be slowed down or avoided, and the storage performance and the cycle life of the battery can be ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of new energy technology, and in particular to a negative electrode active material, a negative electrode sheet and a nickel-zinc battery. Background Art

[0002] Nickel-zinc battery (NiZn) is a new type of battery that can replace nickel-metal hydride battery. It has significant advantages such as long life, high voltage, and low internal resistance and is widely used.

[0003] In the production process of negative electrode sheets, the burrs formed after the negative electrode sheets are cut are prone to powder loss. Not only will the fallen powder be transferred to the positive electrode to cause a micro short circuit, but the powder loss will also lead to a reduction in the negative electrode active material, which in turn causes the nickel-zinc battery to show poor storage performance and a shorter cycle life under high-temperature storage. Existing technologies prevent the negative electrode sheets from powdering by increasing the amount of adhesive in the active material layer in the negative electrode sheet. However, increasing the amount of adhesive not only affects the capacity, but also affects the battery life.

[0004] In view of this, it is urgent to propose a technical solution for inhibiting or avoiding the powdering of the negative electrode sheet of nickel-zinc batteries while ensuring the battery storage performance and cycle life. Summary of the invention

[0005] In order to solve or partially solve the problems existing in the related art, the present application provides a negative electrode active material, a negative electrode sheet and a nickel-zinc battery, which can not only slow down or avoid the cutting burrs and powder loss of the negative electrode sheet, but also ensure the battery storage performance and cycle life.

[0006] In a first aspect, the present application provides a negative electrode active material, comprising the following components in weight percentage: 58%~68% ZnO; 20%~30% Zn; 0.01%~1%In2O3; 0.08%~2.88%Bi2O3; 3%~5% Al2O3; 1%~2% conductive material; 3%~5% binder; 0.3%~0.5% thickener; 1%~2% dispersant; Wherein, the binder includes SBR and / or PTFE.

[0007] In one implementation, the binder is a mixture of SBR and PTFE, wherein the ratio of SBR to PTFE is (1:4) to (4:1).

[0008] In one implementation, the thickener is a CMC solution, and the concentration of the CMC solution is 1-2wt%; The binder is PTFE, and the concentration of the PTFE solution is 50wt%-70wt%.

[0009] In one implementation, the fiber material also comprises 1% to 4% by weight.

[0010] In one implementation, the fiber material is a combination of one or more of polyester fiber, polyamide fiber, polyvinyl alcohol fiber, polyacrylonitrile fiber, polypropylene fiber, polyvinyl chloride fiber or aluminum oxide fiber.

[0011] A second aspect of the present application provides a negative electrode sheet, comprising: A negative electrode body, wherein the negative electrode body comprises a negative electrode current collector and a negative electrode active material layer disposed on the surface of the negative electrode current collector, wherein the negative electrode active material layer comprises the negative electrode active material as described in the first aspect above.

[0012] In one implementation, the negative electrode sheet further includes a protective adhesive layer covering the edge of the negative electrode body; The protective adhesive layer is a tape layer adhered to the edge of the negative electrode body, or the protective adhesive layer is a colloid layer coated on the edge of the negative electrode body.

[0013] In one implementation, the adhesive tape layer has insulating properties; The colloid layer is made of an organic material that is easy to volatilize and form a film and has elasticity.

[0014] In one implementation, the width of the adhesive tape layer or the colloid layer is 2 mm to 5 mm.

[0015] In one implementation, the surface area of ​​the negative electrode body covered by the protective rubber layer accounts for 5% to 18% of the surface area of ​​the negative electrode body.

[0016] A third aspect of the present application provides a nickel-zinc battery, comprising the negative electrode sheet as described in the second aspect above.

[0017] The technical solution provided by this application may have the following beneficial effects: The negative electrode active material provided in the present application includes the following components in weight percentage: 58~68% ZnO; 20~30% Zn; 0.01~1% In2O3; 0.08~2.88% Bi2O3; 3~5% Al2O3; 1~2% conductive material; 3~5% binder; 0.3~0.5% thickener; 1~2% dispersant; wherein the binder includes SBR and / or PTFE. The scheme of the present application, by improving the components of the negative electrode active material, for example, adding a specific weight percentage of binder to the negative electrode active material, the binder includes SBR and / or PTFE, can enhance the adhesion of the negative electrode active material, thereby slowing down or avoiding the powder falling off of the cutting edges of the negative electrode sheet, not only avoiding the transfer of negative electrode powder to the positive electrode to cause micro short circuit, but also avoiding the capacity reduction caused by the shedding of negative electrode active material, slowing down the phenomenon of battery self-discharge, and ensuring the storage performance and cycle life of the battery.

[0018] Furthermore, the negative electrode sheet of the present application includes a protective adhesive layer covering the edge of the negative electrode body; the protective adhesive layer is a tape layer attached to the edge of the negative electrode body, or the protective adhesive layer is a colloid layer coated on the edge of the negative electrode body. By applying the tape layer or colloid layer on the edge of the negative electrode body, the adhesion of the negative electrode active material on the negative electrode sheet is improved, and the powder falling phenomenon at the edge of the negative electrode sheet is further avoided by physical means.

[0019] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] The above and other objects, features and advantages of the present application will become more apparent by describing in more detail exemplary embodiments of the present application in conjunction with the accompanying drawings, wherein the same reference numerals generally represent the same components in the exemplary embodiments of the present application.

[0021] Figure 1 is a schematic structural diagram of a negative electrode sheet shown in an embodiment of the present application; Figure 2 It is a schematic diagram of the width of the protective glue layer of the negative electrode sheet shown in the embodiment of the present application. DETAILED DESCRIPTION

[0022] The embodiments of the present application will be described in more detail below with reference to the accompanying drawings. Although the embodiments of the present application are shown in the accompanying drawings, it should be understood that the present application can be implemented in various forms and should not be limited by the embodiments described herein. On the contrary, these embodiments are provided to make the present application more thorough and complete, and to fully convey the scope of the present application to those skilled in the art.

[0023] The terms used in this application are for the purpose of describing specific embodiments only and are not intended to limit this application. The singular forms of "a", "said" and "the" used in this application and the appended claims are also intended to include plural forms unless the context clearly indicates other meanings. It should also be understood that the term "and / or" used herein refers to and includes any or all possible combinations of one or more associated listed items.

[0024] It should be understood that although the terms "first", "second", "third", etc. may be used in this application to describe various information, this information should not be limited to these terms. These terms are only used to distinguish the same type of information from each other. For example, without departing from the scope of this application, the first information may also be referred to as the second information, and similarly, the second information may also be referred to as the first information. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of this application, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined.

[0025] During the production process of negative electrode sheets, the burrs formed after the negative electrode sheets are cut are prone to powder loss. Not only will the fallen powder be transferred to the positive electrode to cause a micro short circuit, but the powder loss will also lead to a reduction in the negative electrode active material, which in turn causes the nickel-zinc battery to exhibit poor storage performance and a shorter cycle life under high-temperature storage. Existing technologies avoid powder loss of negative electrode sheets by increasing the amount of adhesive in the active material layer of the negative electrode sheet. However, increasing the amount of adhesive not only affects the capacity, but also affects the battery life.

[0026] In view of the above problems, the embodiments of the present application provide a negative electrode active material, a negative electrode sheet and a nickel-zinc battery, which can not only slow down or avoid the phenomenon of powder falling off the cutting edges of the negative electrode sheet, but also ensure the storage performance and cycle life of the battery.

[0027] The technical solution of the embodiments of the present application is described in detail below with reference to the accompanying drawings.

[0028] The first aspect of the present application provides a negative electrode active material, comprising the following components in weight percentage: 58%~68% ZnO; 20%~30% Zn; 0.01%~1% In2O3; 0.08%~2.88% Bi2O3; 3%~5% Al2O3; 1%~2% conductive material; 3%~5% binder; 0.3%~0.5% thickener; 1%~2% dispersant; wherein the binder is SBR and / or PTFE.

[0029] The solution provided in the embodiment of the present application improves the components of the negative electrode active material, for example, by adding 3% to 5% by weight of a binder to the negative electrode active material, wherein the binder is SBR and / or PTFE, thereby enhancing the adhesion of the negative electrode active material, thereby slowing down or avoiding the cutting burrs and powder falling of the negative electrode sheet, which not only avoids the transfer of negative electrode powder to the positive electrode to cause a micro short circuit, but also avoids the capacity reduction caused by the shedding of the negative electrode active material, slows down the self-discharge of the battery, and ensures the storage performance and cycle life of the battery.

[0030] In the solution provided in the embodiment of the present application, the binder includes SBR (Styrene~Butadiene Rubber) and / or PTFE (Polytetrafluoroethylene), that is, the binder can be one of SBR and PTFE, or it can be a mixture of SBR and PTFE. The SBR binder is a high molecular polymer emulsion formed by free radical emulsion polymerization of two monomers, 1,3-butadiene and styrene. In this embodiment, the groups on the surface of SBR can undergo condensation reaction with the groups on the surface of the current collector to form chemical bonds, thereby providing strong bonding force. This bonding force helps to tightly bind the particles of the negative electrode active material together and firmly adhere to the negative electrode current collector to prevent the negative electrode active material from falling off the current collector. PTFE has good high temperature resistance, and can not only maintain the viscosity of the negative electrode active material at 300°C~450°C, but in this embodiment, PTFE is matched with the thickener CMC, and PTFE can inhibit the decomposition of the thickener CMC, thereby inhibiting the decrease in the adhesiveness of the negative electrode active material and improving the adhesion of the negative electrode active material on the negative electrode current collector. Therefore, the binder of the present application uses SBR and / or PTFE, which can enhance the adhesion of the negative electrode active material and thus slow down the powder falling phenomenon. Since the negative electrode active material will not fall off, the battery capacity using the negative electrode active material of this embodiment will not be reduced, and will not cause micro short circuits, while also ensuring the storage performance and cycle life of the battery.

[0031] The related art generally avoids the powdering of the negative electrode sheet by increasing the amount of adhesive in the active material layer in the negative electrode sheet. For example, the weight percentage of the adhesive in the negative electrode active material often reaches 10-20%. Such a high amount of adhesive will reduce the effective contact area between the active material particles, thereby increasing the transmission resistance of electrons and ions in the electrode material, thereby reducing the discharge capacity, cycle stability and cycle life of the battery. In the solution provided by this application, the weight percentage of the binder in the negative electrode active material is 3-5%, which is much lower than the amount of adhesive in the related art, so it can avoid the above-mentioned defects of the related art.

[0032] In some embodiments, the thickener may be a CMC (Carboxymethyl Cellulose) solution with a concentration of 1-2 wt %, and CMC can significantly increase the viscosity of the negative electrode active material and improve its fluidity and stability. The binder may be a PTFE solution with a concentration of 50-70 wt %.

[0033] In some specific embodiments, the concentration of the thickener CMC can be 1 wt%, and the concentration of PTFE can be 50 wt%; or, the concentration of the thickener CMC can be 1.5 wt%, and the concentration of PTFE can be 60 wt%; or, the concentration of the thickener CMC can be 2 wt%, and the concentration of PTFE can be 70 wt%. By setting the thickener CMC and PTFE to specific concentrations, the effect of PTFE in inhibiting the decomposition of the thickener CMC is enhanced, and the adhesion of the negative electrode active material to the negative electrode current collector is further improved.

[0034] In some embodiments, the thickener may be 1.5 wt% CMC and the binder may be SBR. Alternatively, the thickener may be 1.5 wt% CMC and the binder may be a mixture of SBR and PTFE, specifically, the thickener may be 1.5 wt% CMC, wherein the ratio of SBR to PTFE is 1:4.

[0035] In some embodiments, the thickener is 1.5 wt % CMC, and the binder is a mixture of SBR and PTFE, wherein the ratio of SBR to PTFE is 2:3.

[0036] In some embodiments, the thickener is 1.5 wt % CMC, and the binder is a mixture of SBR and PTFE, wherein the ratio of SBR to PTFE is 3:2.

[0037] In some embodiments, the thickener is 1.5 wt % CMC, and the binder is a mixture of SBR and PTFE, wherein the ratio of SBR to PTFE is 4:1.

[0038] In this embodiment, different ratios of the SBR and PTFE mixture have different effects on suppressing the powder falling of the negative electrode. When the ratio of SBR to PTFE is 4:1, the negative electrode active material particles are more tightly bound to each other and have stronger adhesion to the negative electrode current collector. Therefore, the powder falling is suppressed optimally. At the same time, the life and storage performance of the battery cell using the negative electrode active material are optimal.

[0039] In some embodiments, the negative electrode active material further includes 1-4% by weight of fiber material, specifically, the weight percentage of the fiber material can be 1%, 2%, 3% or 4%. After the fiber material of the above weight percentage is added to the negative electrode active material, the negative electrode active material particles are dispersed in the gaps formed by the overlap of the fiber material, so that the negative electrode active material particles and the powder generated by shedding are in contact with each other, thereby forming a network state of overlapping fiber material inside the negative electrode sheet, and the powder generated by shedding is kept in the network structure, so as to avoid the separation of the negative electrode active material particles at the burrs after the negative electrode sheet is cut, thereby avoiding the transfer of powder to the positive electrode to cause micro short circuit.

[0040] In this embodiment, when the concentration of the fiber material is greater than 4%, it will affect the capacity of the battery cell. When the concentration is less than 1%, it is difficult to form gaps where the fibers overlap in the negative active material, and a network structure cannot be formed in the negative electrode sheet. Therefore, powder loss will occur at the cutting edges. When the concentration of the fiber material is 3%, the density of the fiber material in the negative active material makes the network of overlapping fibers inside the negative electrode sheet more uniform and dense, and powder loss will not occur at the cutting edges, thereby achieving the best effect in suppressing powder loss.

[0041] In some embodiments, the fiber material may be a combination of one or more of polyester fiber, polyamide fiber, polyvinyl alcohol fiber, polyacrylonitrile fiber, polypropylene fiber, polyvinyl chloride fiber or aluminum oxide fiber.

[0042] When the fiber material is a combination of one or more of polyamide fiber, polyvinyl alcohol fiber, polyester fiber, the fiber material can improve the binding force between particles of thickener, binder, conductive material, etc., and can also improve the adhesion of negative electrode active materials on the surface of negative electrode current collector, thereby inhibiting powder loss; when the fiber material is alumina fiber, alumina fiber has good thermal conductivity and can quickly transfer heat inside the battery to the external environment to ensure the normal operation of the battery. This feature helps to maintain the stability of the internal temperature of the battery, improve the safety and reliability of the battery, effectively prevent the negative electrode sheet from deformation or failure at high temperature, and improve the safety and stability of the battery.

[0043] Figure 1 It is a schematic diagram of the structure of the negative electrode sheet shown in the embodiment of the present application.

[0044] See also Figure 1 In a second aspect, the present application provides a negative electrode sheet, comprising a negative electrode body 100, wherein the negative electrode body 100 comprises a negative electrode current collector and a negative electrode active material layer disposed on the surface of the negative electrode current collector, wherein the active material layer has the characteristics of the negative electrode active material as described in any embodiment of the first aspect.

[0045] The negative electrode sheet of the present application improves the components of the negative electrode active material layer, for example, a binder and a thickener are added to the negative electrode active material, thereby improving the adhesion of the active material on the negative electrode body, thereby reducing the powder falling phenomenon. In addition, it can avoid the capacity reduction caused by the negative electrode active material falling off the negative electrode body, slow down the self-discharge phenomenon of the nickel-zinc battery, and ensure the storage performance and cycle life of the battery using the negative electrode sheet.

[0046] In some embodiments, the negative electrode sheet further includes a protective adhesive layer 101 covering the edge of the negative electrode body; the protective adhesive layer 101 is a tape layer adhered to the edge of the negative electrode body, or the protective adhesive layer is a colloid layer coated on the edge of the negative electrode body.

[0047] In this embodiment, the edge of the negative electrode body 100 may be a side formed by cutting the negative electrode sheet. By applying a protective adhesive layer 101 on the edge of the negative electrode body, powder loss at the edge can be further avoided in a physical manner.

[0048] In the negative electrode sheet of the present embodiment, the negative electrode current collector can be a metal mesh, such as an obliquely drawn tin-plated copper mesh. In the related art, the obliquely drawn tin-plated copper mesh is prone to form burrs after cutting, and the negative electrode active material is prone to fall off at the burrs, that is, powder falling. After adopting the solution of the present application, the powder falling phenomenon at the cutting burrs can be effectively suppressed.

[0049] In the process of making the negative electrode sheet of the present application, the negative electrode active material of the first aspect is mixed in proportion, stirred evenly, and then coated on an obliquely drawn tin-plated copper mesh, and then rolled, softened, cut, and other processes to form the negative electrode sheet. Since the negative electrode active material of the present application has better viscosity, even on the obliquely drawn tin-plated copper mesh, the negative electrode active material has a strong bonding force with the surface of the obliquely drawn tin-plated copper mesh, so the negative electrode active material will not fall off at the cutting burrs.

[0050] In some embodiments, the protective adhesive layer 101 is a tape layer pasted on the edge portion, and the tape layer has insulation properties, for example, it can be an insulating tape or a masking tape, so that the fallen powder can be kept on the side of the tape layer away from the positive electrode, avoiding the contact of the fallen negative electrode powder with the positive electrode and causing a short circuit. In this embodiment, after adding 1-4wt% fiber material to the negative electrode active material, the overlapping network structure of the fiber material inside the negative electrode sheet and the mesh of the mesh body of the negative electrode collector are interwoven, so that the combination of the negative electrode active material layer and the negative electrode collector is more firmly, and after the negative electrode sheet is cut, the negative electrode active material attached to the cut edge is not easy to fall off, thereby more effectively inhibiting or avoiding the powder falling phenomenon.

[0051] In some embodiments, the protective adhesive layer 101 is a colloidal layer coated on the edge portion, and the colloidal layer is formed by curing an organic material that evaporates into a film and has elasticity. The organic material is, for example, organic glue. This can increase the speed of laying the protective adhesive layer on the negative electrode sheet, thereby improving production efficiency and making it easier to achieve mass and automated production. See also Figure 2 In some embodiments, the protective adhesive layer 101 is a colloid layer coated on the edge portion, and the width W of the colloid layer may be 2-5 mm. Specifically, the width of the adhesive paper layer may be 2 mm, 3 mm, 4 mm or 5 mm.

[0052] In some embodiments, when the protective adhesive layer 101 is a tape layer pasted on the edge, the width W of the tape layer can be 2 to 5 mm. Specifically, the width of the tape layer can be 2 mm, 3 mm, 4 mm or 5 mm. If the width of the tape layer or the colloid layer on the negative electrode body is less than 2 mm, the tape or the glue will fall off, and the covered negative electrode powder will fall off, and the anti-powder falling effect cannot be achieved; if the width of the tape layer or the colloid layer on the negative electrode body is greater than 5 mm, the area covered on the negative electrode body is large, resulting in a reduction in the active area on the negative electrode sheet, and the capacity of the battery cell is not fully utilized.

[0053] In some embodiments, the surface area of ​​the negative electrode body covered by the protective glue layer accounts for 5% to 18% of the surface area of ​​the negative electrode body; that is, when the surface area of ​​the negative electrode body covered by the protective glue layer is S1 and the surface area of ​​the negative electrode body is S2, (S1 / S2)*100%=5% to 18%; the surface area of ​​the negative electrode body covered by the protective glue layer accounts for 5%, 8%, 12%, 15% or 18% of the surface area of ​​the negative electrode body. If the surface area of ​​the negative electrode body covered by the protective glue layer accounts for less than 5% of the surface area of ​​the negative electrode body, the adhesive tape or the glue coating will fall off, and the covered negative electrode powder will fall off, and the anti-powder falling effect cannot be achieved; if the surface area of ​​the negative electrode body covered by the protective glue layer accounts for more than 18% of the surface area of ​​the negative electrode body, the active area on the negative electrode sheet will be reduced due to the large area covered on the negative electrode body, and the capacity of the battery cell will not be fully utilized. Therefore, when the surface area of ​​the negative electrode body covered by the protective rubber layer accounts for 5~18% of the surface area of ​​the negative electrode body, the powder loss prevention effect can be achieved and the battery cell capacity can also be stably exerted.

[0054] In this embodiment, the negative electrode body is in the shape of a rectangular sheet, and the edge portions are formed on the four sides of the negative electrode body. The four sides can be formed by cutting the negative electrode sheet, and a glue layer or a colloid layer is applied on the four sides of the negative electrode body. The glue layer or the colloid layer can improve the bonding strength of the negative electrode active material at the cut edges of the negative electrode body, and can confine the powder falling off the negative electrode body to the inside of the glue layer or the colloid layer, so as to prevent the powder from falling out and transferring to the positive electrode to form a micro short circuit, and can improve the safety of the battery using the negative electrode sheet.

[0055] It can be seen from the above embodiments that the negative electrode sheet provided in the present application not only improves the components of the negative electrode active material, for example, by adding 3-5% of a binder to the negative electrode active material, the binder is a mixture of SBR and PTFE, thereby improving the adhesion of the active material on the negative electrode body and reducing the powder falling phenomenon. In addition, a protective adhesive layer is physically coated on the edge of the negative electrode structure, so that the powder falling off the negative electrode body can be retained inside the negative electrode body to avoid being transferred to the positive electrode and causing a micro short circuit. The combination of chemical and physical methods, and the joint action of the internal and external can not only avoid the reduction of the negative electrode active material and effectively avoid the powder falling phenomenon of the negative electrode sheet, but also can improve the storage performance and cycle life of the battery cell.

[0056] The third aspect of the present application provides a nickel-zinc battery, which includes a positive electrode sheet, an electrolyte, and a negative electrode sheet as described in any embodiment of the second aspect above. The nickel-zinc battery of the present application can be applied to electrical equipment, which can be a smart lock, an electric tool, a lamp, or a toy. Since the nickel-zinc battery of the electrical equipment has a longer life and storage performance, the performance of the electrical equipment can be improved.

[0057] In some embodiments, the electrolyte of the battery of this embodiment includes the following concentration components: 5~5.5 mol / L KOH, 0.1~0.5 mol / L ZnO, 1~2wt% disodium hydrogen phosphate, and 2wt% boric acid.

[0058] The positive electrode sheet of the nickel-zinc battery of the present application includes a positive electrode current collector and a positive electrode active material, and the positive electrode current collector has a surface density of 300-400 g / m 2 The positive active materials of nickel foam are Ni(OH)2, ZnO, CoO, Ni powder, Ca(OH)2, Y2O3, Yb2O3, graphite, CMC, PTFE, and the weight ratios of the above materials are 85:1:3:2:1:2.5:2:2:0.5:3. In the production process, the above positive active materials are mixed according to the proportion, stirred evenly, coated on the positive current collector, and rolled, softened, cut, etc. to make the positive electrode sheet of nickel-zinc battery.

[0059] The nickel-zinc battery provided by the present application can avoid the defects of poor storage performance and cycle life under high-temperature storage due to micro-short circuits and reduction of negative electrode active materials in the battery of the related art, because the cutting edge of the negative electrode sheet will not cause powder falling. In addition, by improving the components of the negative electrode active materials of the battery, the capacity reduction caused by the shedding of the negative electrode active materials can be avoided, the self-discharge of the nickel-zinc battery can be slowed down, and the storage performance and cycle life of the nickel-zinc battery can be guaranteed.

[0060] To make the present invention easier to understand, the present application is further described in detail below. The % mentioned in the following examples all represent percentages by weight. This example is used to illustrate the nickel-zinc battery negative electrode sheet and nickel-zinc battery disclosed in the present invention. It should be noted that the following examples do not exhaust all possible situations, and the materials used in the following examples can be obtained from commercial channels unless otherwise specified.

[0061] Example 1 The negative electrode active material in the nickel-zinc battery of this embodiment includes the following components in weight percentage: 62% ZnO; 25% Zn; 0.05% In2O3; 1.55% Bi2O3; 4% Al2O3; 1.5% conductive material; 4% binder; 0.4% thickener; 1.5% dispersant; wherein the binder is a mixture of SBR and PTFE, wherein the ratio of SBR to PTFE is 4:1.

[0062] The negative electrode current collector of this embodiment is an obliquely drawn tin-plated copper mesh.

[0063] The above negative electrode active materials are mixed according to proportion, stirred evenly, coated on the negative electrode current collector, and then rolled, softened, and cut to obtain the negative electrode sheet of the nickel-zinc battery.

[0064] The positive electrode sheet of this embodiment includes a positive electrode current collector and a positive electrode active material, wherein the components of the positive electrode active material include ~Ni(OH)2, ZnO, CoO, Ni powder, Ca(OH)2, Y2O3, Yb2O3, graphite, CMC, PTFE, wherein the weight ratio of the above substances is 85:1:3:2:1:2.5:2:2:0.5:3. The above positive electrode active materials are mixed according to the proportion, stirred evenly, coated on the positive electrode current collector, and rolled, softened, cut, etc. to obtain a positive electrode sheet for a nickel-zinc battery.

[0065] The nickel-zinc battery of this embodiment includes a positive electrode, a negative electrode, and an electrolyte. The negative electrode is the negative electrode sheet of the nickel-zinc battery, and the electrolyte is the electrolyte of the nickel-zinc battery.

[0066] Examples 2 to 5 and Comparative Examples 1 to 2 are prepared in the same manner as Example 1, except that the components and addition amounts of the negative electrode active materials are different. For details, see Table 1.

[0067] Table 1

[0068] The applicant conducted life and storage performance tests on the nickel-zinc batteries prepared in Examples 1 to 5 and Comparative Examples 1 to 2 under the following conditions, and the test results obtained are entered into Table 2.

[0069] (1) Life test Test method: The condition is 1C charging to 1.9V, 1C discharging to 1.3V, and the test is stopped until the capacity / initial capacity is less than 60%; (2) Storage performance test Test method: Storage performance test environment: 60℃, 28 days; Storage performance capacity test conditions, 0.2C discharge to 1.3V, 0.2C charge to 1.9V, stand for 10 min, cycle the above steps three times.

[0070] The test results are shown in Table 2: Table 2

[0071] In Table 2, SOC (State of Charge) % refers to the ratio of the remaining capacity of the battery pack after it has been used for a period of time or has been left unused for a long time to its rated capacity when fully charged, and SOH (State of Health) % indicates the remaining capacity and service life of the battery.

[0072] The data of Comparative Examples 1-2 and Examples 1-5 show that the negative electrode active material of Comparative Example 1 does not introduce 3-5% binder by mass, and powder is easily lost, so the SOC% and SOH% values ​​are low. This is because powder loss will lead to a reduction in negative electrode active material, thereby affecting the storage performance and life of the nickel-zinc battery. Although a thickener is introduced into the negative electrode active material of Comparative Example 2, the adhesion of the negative electrode active material is still poor, and powder is easily lost, resulting in low SOC% and SOH% values, and poor life and storage performance of the nickel-zinc battery.

[0073] Example 6 The only difference between this embodiment and embodiment 1 is that the binder is PTFE.

[0074] Example 7 The only difference between this embodiment and embodiment 1 is that the binder is SBR. Example 8 The only difference between this embodiment and embodiment 1 is that the binder is a mixture of SBR and PTFE, wherein the ratio of SBR to PTFE is 1:4.

[0075] Example 9 The only difference between this embodiment and Embodiment 1 is that the binder is a mixture of SBR and PTFE, wherein the ratio of SBR to PTFE is 3:2.

[0076] Example 10 The only difference between this embodiment and Embodiment 1 is that the binder is a mixture of SBR and PTFE, wherein the ratio of SBR to PTFE is 2:3.

[0077] Embodiment 11 The only difference between this embodiment and embodiment 1 is that the thickener is a CMC solution, and the concentration of the CMC solution is 1 wt %; the binder is a PTFE solution, and the concentration of the PTFE solution is 50 wt %.

[0078] Example 12 The only difference between this embodiment and embodiment 1 is that the thickener is a CMC solution, and the concentration of the CMC solution is 1.5 wt %; the binder is a PTFE solution, and the concentration of the PTFE solution is 60 wt %.

[0079] Example 13 The only difference between this embodiment and embodiment 1 is that the thickener is a CMC solution, and the concentration of the CMC solution is 2 wt %; the binder is a PTFE solution, and the concentration of the PTFE solution is 70 wt %.

[0080] Embodiment 14 The only difference between this embodiment and embodiment 1 is that it also includes 1% by weight of fiber material.

[0081] Embodiment 15 The only difference between this embodiment and embodiment 1 is that it also includes 2.5% by weight of fiber material.

[0082] Example 16 The only difference between this embodiment and embodiment 1 is that it also includes 4% by weight of fiber material.

[0083] Embodiment 17 The only difference between this embodiment and embodiment 1 is that the fiber material is polyester fiber with a weight percentage of 2.5%.

[0084] Embodiment 18 The only difference between this embodiment and embodiment 1 is that the fiber material is a combination of polyester fiber and polyamide fiber, with a weight percentage of 2.5%.

[0085] Embodiment 19 The only difference between this embodiment and Embodiment 1 is that the fiber material is aluminum oxide fiber with a weight percentage of 2.5%.

[0086] Comparative Example 3 The only difference between this comparative example and Example 1 is that the negative electrode active material in the nickel-zinc battery of Comparative Example 1 does not include a binder.

[0087] Comparative Example 4 The only difference between this comparative example and Example 1 is that the negative electrode active material in the nickel-zinc battery of this comparative example includes a mixture of SBR and PTFE, but the ratio of SBR to PTFE is 0.5:4.

[0088] Comparative Example 5 The only difference between this comparative example and Example 1 is that the negative electrode active material in the nickel-zinc battery of this comparative example includes a mixture of SBR and PTFE, but the ratio of SBR to PTFE is 5:1.

[0089] Comparative Example 6 The only difference between this comparative example and Example 1 is that the concentration of the CMC solution of the negative electrode active material in the nickel-zinc battery of this comparative example is 5 wt %.

[0090] The applicant conducted life and storage performance tests on the nickel-zinc batteries prepared in Examples 6 to 19 and Comparative Examples 3 to 6 under the following conditions, and the test results obtained are entered into Table 3.

[0091] (1) Life test Test method: The condition is 1C charging to 1.9V, 1C discharging to 1.3V, and the test is stopped until the capacity / initial capacity is less than 60%; (2) Storage performance test Test method: Storage performance test environment: 60℃, 28 days; Storage performance capacity test conditions, 0.2C discharge to 1.3V, 0.2C charge to 1.9V, stand for 10 min, cycle the above steps three times. The test results are shown in Table 3: Table 3:

[0092] In Table 3, the data of Comparative Examples 3 to 6 and Examples 6 to 19 show that no binder is introduced into the negative electrode active material of Comparative Example 3, and powder is easily lost, so the SOC% and SOH% values ​​are relatively low. This is because powder loss will lead to a reduction in the negative electrode active material, thereby affecting the storage performance and life of the nickel-zinc battery. Although binders SBR and PTFE are introduced into the negative electrode active materials of Comparative Examples 4 to 5, the ratio of the two cannot make the adhesion of the negative electrode active material reach the best, and powder is also easily lost, resulting in low SOC% and SOH% values. The concentration of CMC in the negative electrode active material of Comparative Example 6 is too high, resulting in reduced adhesion of the negative electrode active material on the negative electrode current collector, and powder is easily lost, resulting in poor life and storage performance of the nickel-zinc battery.

[0093] In Examples 6 to 10, a binder is introduced into the negative electrode active material, and the cycle number of the nickel-zinc battery is greater than 210 cycles, and both SOC% and SOH% are increased, wherein SOC% is greater than 33%, and SOH% is greater than 83%. Compared with Comparative Example 3, adding a binder to the negative electrode active material, and the binder is SBR and / or PTFE, can significantly improve the storage performance and life of the nickel-zinc battery.

[0094] The data of Examples 11 to 13 show that when the thickener of the negative electrode active material is a CMC solution and the binder is a PTFE solution, the SOC% and SOH% of the nickel-zinc battery both increase. This is because PTFE is combined with the thickener CMC, and PTFE can inhibit the decomposition of the thickener CMC, thereby inhibiting the decrease in the adhesion of the negative electrode active material, improving the adhesion of the negative electrode active material to the negative electrode current collector, thereby avoiding the reduction of the negative electrode active material due to shedding, and improving the storage performance and life of the nickel-zinc battery.

[0095] The data of Examples 14 to 19 show that when the fiber material is added to the negative electrode active material, the SOC% and SOH% of the nickel-zinc battery further increase. This is because the overlapping network structure of the fiber material inside the negative electrode sheet is interwoven with the mesh of the negative electrode current collector, making the negative electrode active material layer and the negative electrode current collector more firmly bonded. After the negative electrode sheet is cut, the negative electrode active material attached to the cutting edge is not easy to fall off, thereby more effectively suppressing or avoiding the powder falling phenomenon. Therefore, the nickel-zinc battery of the present application can not only avoid the problem of negative electrode powder falling, but also ensure its service life and storage performance.

[0096] The embodiments of the present application have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or improvements to the technology in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.

Claims

1. A negative electrode active material, characterized in that: The composition comprises the following weight percentages: 58%~68% ZnO; 20%~30% Zn; 0.01%~1%In2O3; 0.08%~2.88%Bi2O3; 3%~5% Al2O3; 1%~2% conductive material; 3%~5% binder; 0.3%~0.5% thickener; 1%~2% dispersant; Wherein, the binder includes SBR and / or PTFE.

2. The negative electrode active material according to claim 1, characterized in that: The binder is a mixture of SBR and PTFE, wherein the ratio of SBR to PTFE is (1:4) to (4:1).

3. The negative electrode active material according to claim 1, characterized in that: The thickener is a CMC solution, and the concentration of the CMC solution is 1 wt% to 2wt%; The binder is a PTFE solution, and the concentration of the PTFE solution is 50 wt% to 70 wt%.

4. The negative electrode active material according to claim 1, characterized in that: It also includes 1% to 4% fiber material by weight.

5. The negative electrode active material according to claim 4, characterized in that: The fiber material is a combination of one or more of polyester fiber, polyamide fiber, polyvinyl alcohol fiber, polyacrylonitrile fiber, polypropylene fiber, polyvinyl chloride fiber or aluminum oxide fiber.

6. A negative electrode sheet, characterized in that: include: A negative electrode body, the negative electrode body comprising a negative electrode current collector and a negative electrode active material layer arranged on the surface of the negative electrode current collector, the negative electrode active material layer comprising the negative electrode active material according to any one of claims 1 to 5.

7. The negative electrode sheet according to claim 6, characterized in that: The negative electrode sheet also includes a protective glue layer covering the edge of the negative electrode body; The protective adhesive layer is a layer of adhesive tape pasted on the edge of the negative electrode body, or, The protective glue layer is a colloid layer coated on the edge of the negative electrode body.

8. The negative electrode sheet according to claim 7, characterized in that: The adhesive tape layer has insulation properties; The colloid layer is made of an organic material that is easy to volatilize and form a film and has elasticity.

9. The negative electrode sheet according to claim 7, characterized in that: The width of the adhesive paper layer or the colloid layer is 2 mm to 5 mm.

10. The negative electrode sheet according to claim 7, characterized in that: The surface area of ​​the negative electrode body covered by the protective rubber layer accounts for 5% to 18% of the surface area of ​​the negative electrode body.

11. A nickel-zinc battery, characterized in that: Comprising the negative electrode sheet as described in any one of claims 6 to 10.

Citation Information

Patent Citations

  • Negative plate of nickel-zinc battery and nickel-zinc battery

    CN118448595A

  • Negative electrode material, negative electrode slurry, preparation method of negative electrode slurry, negative electrode plate and nickel-zinc battery

    CN118507731A

  • Lithium ion battery pole group capable of reducing battery self-discharge and improving battery safety

    CN211578881U