Anion-cation double-doped positive electrode material and preparation thereof, positive electrode plate and battery

By using S and Nb in the positive electrode material for double doping and forming a lithium carbonate shell, the problems of delitting and structural stability of the positive electrode material at high voltage in the prior art are solved, and the high electrochemical dynamics of lithium-ion batteries are realized. Performance and capacity improvements.

CN118919708APending Publication Date: 2024-11-08JINGMEN GEM NEW MATERIAL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410957258.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

When used at high voltages, existing positive electrode materials have problems such as high delitting, structural phase change expansion into the interior, poor electrochemical stability, poor kinetic performance and low capacity.

Method used

S and Nb are used for anion and cation doping, S reduces the migration energy barrier of Li+, and Nb stabilizes the TMO skeleton through strong Nb-O bonds, forming a lithium carbonate shell to inhibit side reactions, and improves electrochemical kinetic performance and cyclic stability.

Benefits of technology

It significantly improves the electrochemical kinetic performance and capacity of lithium-ion batteries, enhances cycling stability, and suppresses cracks caused by material strain during charging and discharging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919708A_ABST
    Figure CN118919708A_ABST
Patent Text Reader

Abstract

The invention provides an anion-cation double-doped positive electrode material and preparation thereof, a positive electrode plate and a battery. The positive electrode material comprises an S and Nb doped core and a lithium carbonate shell coated outside the S and Nb doped core. According to the anion-cation double-doped positive electrode material provided by the invention, S and Nb are adopted for doping, and S can remarkably improve charge transfer kinetics of a battery, remarkably reduce a migration energy barrier of Li < + >, promote rapid migration of Li < + > and improve electrochemical kinetics performance and capacity of the battery; due to Nb element doping, a TMO skeleton can be effectively stabilized by a strong Nb-O bond, voltage attenuation is inhibited, and the cycling stability is enhanced; the positive electrode material contains a lithium carbonate shell, so that side reaction between particles and electrolyte can be inhibited, and cracks generated by material strain in the charging and discharging process are reduced; therefore, the lithium ion battery prepared from the positive electrode material provided by the invention has excellent cycling stability, relatively strong dynamic performance and relatively high capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of batteries, and relates to an anion-cation dual-doped positive electrode material, and in particular to an anion-cation dual-doped positive electrode material and its preparation, a positive electrode plate and a battery. Background Art

[0002] With the increasing development of new energy technologies, lithium-ion batteries, as an efficient and green energy storage device, have always been a research hotspot at home and abroad, among which the development and utilization of positive electrode materials have received extensive attention. At present, positive electrode materials are divided into three types: layered structure, spinel structure and olivine structure, corresponding to ternary materials, lithium cobalt oxide, lithium manganese oxide and lithium iron phosphate respectively. Among them, lithium cobalt oxide (LiCoO2) is the earliest commercialized and most successfully applied lithium-ion battery positive electrode material. Due to its simple preparation method, stable cycle performance, good thermal stability, high material density and compaction density, lithium-ion batteries prepared with lithium cobalt oxide have a high volume energy density, and are widely used in electronic product markets such as laptops, smart phones and mobile phones.

[0003] However, with the development of society, in order to meet the market demand for high energy density materials, researchers have continuously developed higher voltage materials, from the initial low voltage to the current high voltage. However, when the positive electrode material is used under high voltage, the degree of lithium removal on the surface of the material will increase, and the structural phase change will extend from the surface of the material to the inside of the particle, resulting in poor structural and electrochemical stability.

[0004] In addition, during the charge and discharge process of the traditional lithium cobalt oxide cathode material, the electrolyte on the surface of the material will corrode the material, and a large number of side reactions will occur on the surface of the material, causing structural collapse and dissolution of the cathode material. This is manifested as an increase in the internal resistance and a decrease in capacity of the battery after a long cycle.

[0005] CN117577809A discloses a lithium cobalt oxide positive electrode material modified by dual polymers and lithium niobate, and its preparation method and application. The modified LCO particles are, from the outside to the inside, a surface coating layer, a subsurface gradient doping transition layer, a near-surface bulk doping layer, and a lithium cobalt oxide matrix. A preparation method for a lithium cobalt oxide positive electrode material modified by dual polymers and lithium niobate. The lithium cobalt oxide positive electrode material modified by dual polymers and lithium niobate is used as a positive electrode material for lithium-ion batteries. The invention constructs a multi-level modified surface structure, especially the synergistic effect of PAN and PVDF, which enables LCO to have a more uniform lithium niobate coating and a more stable surface, thereby obtaining a high Li + / electronic conductivity, small volume deformation, highly reversible structure, stable spinel-like transition layer, etc., achieving excellent electrochemical performance and long-cycle stability.

[0006] CN103199248A discloses a method for preparing a carbon-coated niobium-doped lithium iron phosphate-lithium cobalt oxide composite positive electrode material, comprising the following steps: (1) preparing carbon-coated niobium-doped lithium iron phosphate by wet and dry mixing; (2) mechanically mixing the carbon-coated niobium-doped lithium iron phosphate and lithium cobalt oxide with a layered structure having a purity of more than 99.5wt%, ball milling for 20-30h at a speed of 300-500r / min, passing through a 100-mesh sieve, and finally obtaining a carbon-coated niobium-doped lithium iron phosphate-lithium cobalt oxide composite positive electrode material. The composite positive electrode material for lithium-ion batteries prepared by the invention is modified by doping lithium iron phosphate with niobium to improve its ion diffusion performance, and then a carbon layer is coated on its surface to improve its conductivity, and finally lithium cobalt oxide whose potential difference is complementary to that of lithium iron phosphate is doped therein.

[0007] The positive electrode materials disclosed at present have certain defects. When the positive electrode material is used under high voltage, the degree of lithium removal on the surface of the positive electrode material is high, and the structural phase change extends from the surface of the positive electrode material to the inside, resulting in poor electrochemical stability. There is a problem that the electrolyte on the surface of the positive electrode material corrodes the positive electrode material, resulting in poor electrochemical stability. There are also problems that the battery prepared with the positive electrode material has poor kinetic performance and low capacity. Therefore, it is very important to develop and design a positive electrode material and preparation of an anion and cation dual doped positive electrode sheet and battery. Summary of the invention

[0008] In view of the shortcomings of the prior art, the present invention aims to provide a positive electrode material and preparation thereof, a positive electrode plate and a battery. The positive electrode material provided by the present invention is doped with S and Nb. S can significantly improve the charge transfer kinetics of the battery and significantly reduce Li + The migration barrier of Li + The rapid migration of the positive electrode material improves the electrochemical kinetic performance and capacity of the battery; the Nb element is doped, and the strong Nb-O bond can effectively stabilize the TMO skeleton, inhibit voltage decay and enhance the cycle stability; the positive electrode material contains a lithium carbonate shell, which can inhibit the side reaction of the particles and the electrolyte and reduce the cracks caused by material strain during the charge and discharge process; therefore, the lithium ion battery prepared with the positive electrode material provided in the present invention has excellent cycle stability, strong kinetic performance and high capacity.

[0009] To achieve this object, the present invention adopts the following technical solutions:

[0010] In a first aspect, the present invention provides a positive electrode material doped with both anions and cations, the positive electrode material comprising a S and Nb doped core, and a lithium carbonate shell coating the S and Nb doped core.

[0011] In the cathode material with dual doping of anions and cations provided by the present invention, S and Nb are used for doping. S can significantly improve the charge transfer kinetics of the battery, significantly reduce the migration energy barrier of Li + , promote the rapid migration of Li + , and improve the electrochemical kinetics performance and capacity of the battery; the doping of Nb element, the strong Nb-O bond can effectively stabilize the TMO framework, inhibit voltage decay and enhance the cycle stability; the cathode material contains a lithium carbonate shell, which can inhibit the side reaction between the particles and the electrolyte and reduce the cracks generated by the material strain during charge and discharge; therefore, the lithium ion battery prepared with the cathode material provided by the present invention has excellent cycle stability, strong kinetics performance and high capacity.

[0012] Preferably, the S and Nb doping core includes any one of S and Nb doped LiCoO2 core, S and Nb doped LiMn2O4 core, S and Nb doped LiNi 0.5 Mn 1.5 O4 core, S and Nb doped LiNi x Co y Mn 1-x-y O2 core, and preferably S and Nb doped LiCoO2 core.

[0013] In the present invention, by doping S and Nb elements into the crystal structure of the LiCoO2 core, occupying the space position of cobalt ions, the effects of stabilizing the lithium deintercalation crystal, expanding the lattice spacing and supporting the layered structure are achieved, thereby inhibiting the dissolution of cobalt ions in the LiCoO2 core, and thus improving the electrochemical stability.

[0014] Preferably, 0 < x < 1 and 0 < y < 1 in the LiNi x Co y Mn 1-x-y O2.

[0015] In the LiNi x Co y Mn 1-x-y O2 of the present invention, 0 < x < 1, and the value of x can be, for example, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8 or 0.9, but is not limited to the listed values, and other unlisted values within this numerical range are equally applicable.

[0016] In the LiNi x Co y Mn 1-x-yIn O2, 0 < y < 1. The value of y can be, for example, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, or 0.9, but is not limited to the listed values. Other unlisted values within this numerical range are equally applicable.

[0017] In a second aspect, the present invention provides a method for preparing the cathode material described in the first aspect. The preparation method includes:

[0018] (1) Mixing a bottom solution, a precipitant solution, and a mixed solution containing a Co source, an Nb source, and an S source, and performing a coprecipitation reaction to obtain a precipitate;

[0019] (2) Subjecting the precipitate obtained in step (1) to a first calcination to obtain an oxide precursor, then mixing the obtained oxide precursor with a lithium source, and then performing a second calcination to obtain a lithium cobaltate precursor;

[0020] (3) Sintering the lithium cobaltate precursor obtained in step (2), and introducing carbon dioxide during the sintering process to obtain the cathode material.

[0021] In the method for preparing the cathode material with dual doping of anions and cations provided by the present invention, when S and Nb are dual-doped, they are mixed with the cobalt raw material and incorporated during coprecipitation, ensuring the doping uniformity. Additionally, in the preparation method, during the calcination process, carbon dioxide is introduced to form a lithium carbonate shell layer on the surface of the sample. The operation is simple and the cost is relatively low.

[0022] Preferably, the bottom solution in step (1) includes an ammonium bicarbonate solution and / or ammonia water.

[0023] Preferably, the concentration of the bottom solution in step (1) is 20 - 40 g / L. For example, it can be 20 g / L, 22 g / L, 24 g / L, 26 g / L, 28 g / L, 30 g / L, 32 g / L, 34 g / L, 36 g / L, 38 g / L, or 40 g / L, but is not limited to the listed values. Other unlisted values within this numerical range are equally applicable.

[0024] Preferably, the precipitant solution in step (1) includes any one or a combination of at least two of an ammonium bicarbonate solution, a sodium carbonate solution, or a sodium bicarbonate solution. Typical but non-limiting combinations include a combination of an ammonium bicarbonate solution and a sodium carbonate solution, a combination of a sodium carbonate solution and a sodium bicarbonate solution, or a combination of an ammonium bicarbonate solution, a sodium carbonate solution, and a sodium bicarbonate solution.

[0025] Preferably, the concentration of the precipitant solution in step (1) is 50-200 g / L, for example, 50 g / L, 60 g / L, 70 g / L, 80 g / L, 90 g / L, 100 g / L, 110 g / L, 120 g / L, 130 g / L, 140 g / L, 150 g / L, 160 g / L, 170 g / L, 180 g / L, 190 g / L or 200 g / L, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0026] Preferably, the Co source in step (1) comprises any one of cobalt chloride, cobalt sulfate or cobalt nitrate, or a combination of at least two of them. Typical but non-limiting combinations include a combination of cobalt chloride and cobalt sulfate, a combination of cobalt sulfate and cobalt nitrate, or a combination of cobalt chloride, cobalt sulfate and cobalt nitrate.

[0027] Preferably, the concentration of the Co source in the mixed solution of step (1) is 1.5 to 2 mol / L, for example, 1.5 mol / L, 1.55 mol / L, 1.6 mol / L, 1.65 mol / L, 1.7 mol / L, 1.75 mol / L, 1.8 mol / L, 1.85 mol / L, 1.9 mol / L, 1.95 mol / L or 2 mol / L, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0028] Preferably, the Nb source in step (1) comprises any one of niobium oxalate, niobium acetate or niobium chloride, or a combination of at least two of them. Typical but non-limiting combinations include a combination of niobium oxalate and niobium acetate, a combination of niobium acetate and niobium chloride, and a combination of niobium oxalate, niobium acetate and niobium chloride.

[0029] Preferably, the concentration of the Nb source in the mixed solution of step (1) is 0.08-0.12 g / L, for example, 0.08 g / L, 0.085 g / L, 0.09 g / L, 0.095 g / L, 0.1 g / L, 0.105 g / L, 0.11 g / L, 0.115 g / L or 0.12 g / L, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0030] Preferably, the S source in step (1) comprises sodium dodecyl sulfonate and / or sodium p-alkylbenzene sulfonate.

[0031] Preferably, the concentration of the S source in the mixed solution of step (1) is 2 to 5 g / L, for example, 2 g / L, 2.5 g / L, 3 g / L, 3.5 g / L, 4 g / L, 4.5 g / L or 5 g / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0032] Preferably, the mixing in step (1) comprises: simultaneously adding a precipitant solution and a mixed solution containing a Co source, a Nb source and a S source into the base solution.

[0033] Preferably, the flow ratio of the precipitant solution to the mixed solution during the simultaneous addition is (1-3):1, for example, it can be 1:1, 1.2:1, 1.4:1, 1.6:1, 1.8:1, 2:1, 2.2:1, 2.4:1, 2.6:1, 2.8:1 or 3:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0034] Preferably, the synchronous addition process is accompanied by stirring at a speed of 60 to 200 rpm, for example, 60 rpm, 80 rpm, 100 rpm, 120 rpm, 140 rpm, 160 rpm, 180 rpm or 200 rpm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0035] Preferably, during the simultaneous adding process, the pH is adjusted to 7.0-8.5 and the temperature is adjusted to 40-60°C.

[0036] During the simultaneous addition process of the present invention, the pH is adjusted to 7.0-8.5, for example, 7.0, 7.1, 7.2, 7.3, 7.4, 7.5, 7.6, 7.7, 7.8, 7.9, 8.0, 8.1, 8.2, 8.3, 8.4 or 8.5, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0037] The temperature is adjusted to 40-60°C during the simultaneous adding process described in the present invention, for example, it can be 40°C, 42°C, 44°C, 46°C, 48°C, 50°C, 52°C, 54°C, 56°C, 58°C or 60°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0038] Preferably, the growth rate of the precipitate during the coprecipitation reaction in step (1) is 0.02 to 0.2 μm / h, for example, 0.02 μm / h, 0.04 μm / h, 0.06 μm / h, 0.08 μm / h, 0.1 μm / h, 0.12 μm / h, 0.14 μm / h, 0.16 μm / h, 0.18 μm / h or 0.2 μm / h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0039] Preferably, the coprecipitation reaction in step (1) further comprises solid-liquid separation, slurry washing and drying.

[0040] Preferably, the drying temperature is 60-100°C, for example, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C or 100°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0041] Preferably, the first calcination in step (2) includes a first heating and a first heat preservation performed sequentially.

[0042] Preferably, the first heating rate is 2-10° C. / min, the end temperature is 500-700° C., and the first insulation time is 1-3 h.

[0043] The first heating rate in the present invention is 2 to 10°C / min, for example, it can be 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min or 10°C / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0044] The terminal temperature of the first heating in the present invention is 500-700°C, for example, it can be 500°C, 520°C, 540°C, 560°C, 580°C, 600°C, 620°C, 640°C, 660°C, 680°C or 700°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0045] The first insulation time in the present invention is 1 to 3 hours, for example, it can be 1h, 1.2h, 1.4h, 1.6h, 1.8h, 2h, 2.2h, 2.4h, 2.6h, 2.8h or 3h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0046] Preferably, the mass ratio of the oxide precursor to the lithium source in step (2) is 1:(1-1.3), for example, it can be 1:1, 1:1.2, 1:1.5, 1:1.7, 1:2, 1:2.2, 1:2.5, 1:2.7 or 1:3, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0047] Preferably, the lithium source in step (2) comprises lithium hydroxide and / or lithium carbonate.

[0048] Preferably, the second calcination in step (2) includes a second heating and a second heat preservation performed sequentially.

[0049] Preferably, the second heating rate is 2-10° C. / min, the end temperature is 700-900° C., and the second insulation time is 8-14 h.

[0050] The purpose of the second calcination in the preparation method of the positive electrode material described in the present invention is to prepare a lithium carbonate shell layer. The end temperature of the second heating when preparing the lithium carbonate shell layer, that is, the temperature of the second insulation, will affect the performance of the lithium ion battery prepared by the positive electrode material doped with both anions and cations; when the temperature is low, the capacity retention rate of the lithium ion battery will be reduced, because the shell layer prepared at low temperature is loose and difficult to protect the positive electrode material; when the temperature is high, the formed lithium carbonate will decompose immediately and cannot form a protective layer.

[0051] The second heating rate in the present invention is 2 to 10°C / min, for example, it can be 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min or 10°C / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0052] The terminal temperature of the second heating in the present invention is 700-900°C, for example, it can be 700°C, 720°C, 740°C, 760°C, 780°C, 800°C, 820°C, 840°C, 860°C, 880°C or 900°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0053] The second insulation time in the present invention is 8 to 14 hours, for example, it can be 8 hours, 8.5 hours, 9 hours, 9.5 hours, 10 hours, 11.5 hours, 12 hours, 12.5 hours, 13 hours, 13.5 hours or 14 hours, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0054] Preferably, the sintering temperature in step (3) is 450-550° C. and the sintering time is 3-7 minutes.

[0055] The sintering temperature in step (3) of the present invention is 450-550°C, for example, it can be 450°C, 460°C, 470°C, 480°C, 490°C, 500°C, 510°C, 520°C, 530°C, 540°C or 550°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0056] Preferably, step (3) also includes cooling by natural cooling before sintering.

[0057] As a preferred technical solution of the preparation method of the present invention, the preparation method comprises:

[0058] (1) adding a precipitant solution with a concentration of 50 to 200 g / L and a mixed solution containing a Co source with a concentration of 1.5 to 2 mol / L, a Nb source with a concentration of 0.08 to 0.12 g / L and a S source with a concentration of 2 to 5 g / L to a base solution with a concentration of 20 to 40 g / L, wherein the flow ratio of the precipitant solution to the mixed solution is (1 to 3):1 during the simultaneous addition, adjusting the pH to 7.0 to 8.5, adjusting the temperature to 40 to 60° C., and stirring at a speed of 60 to 200 rpm to perform a coprecipitation reaction, wherein the growth rate of the precipitate during the coprecipitation reaction is 0.02 to 0.2 μm / h, and obtaining a precipitate;

[0059] (2) heating the precipitate obtained in step (1) to 500-700° C. at a rate of 2-10° C. / min and then keeping the temperature for 1-3 hours to obtain an oxide precursor, and then mixing the obtained oxide precursor with a lithium source at a mass ratio of 1:(1-1.3), and then heating it to 700-900° C. at a rate of 2-10° C. / min and keeping the temperature for 8-14 hours to obtain a lithium cobalt oxide precursor;

[0060] (3) The lithium cobalt oxide precursor obtained in step (2) is naturally cooled to 450-550° C. and then sintered for 3-7 minutes, during which carbon dioxide is introduced to obtain the positive electrode material.

[0061] In a third aspect, the present invention provides a positive electrode plate, wherein the positive electrode plate comprises the positive electrode material described in the first aspect.

[0062] In a fourth aspect, the present invention provides a lithium-ion battery, wherein the lithium-ion battery comprises the positive electrode sheet described in the third aspect.

[0063] Compared with the prior art, the present invention has the following beneficial effects:

[0064] (1) The anion-cation dual-doped positive electrode material provided by the present invention is doped with S and Nb. S can significantly improve the charge transfer kinetics of the battery and significantly reduce Li + The migration barrier of Li + The rapid migration of Nb improves the electrochemical kinetic performance and capacity of the battery; Nb element doping and strong Nb-O bond can effectively stabilize the TMO skeleton, inhibit voltage decay and enhance cycle stability; the positive electrode material contains a lithium carbonate shell, which can inhibit the side reaction of particles and electrolyte and reduce cracks caused by material strain during charging and discharging; therefore, the lithium ion battery prepared by the positive electrode material provided in the present invention has excellent cycle stability, strong kinetic performance and high capacity;

[0065] (2) In the preparation method of the anion-cation dual-doped positive electrode material provided by the present invention, when S and Nb are dual-element doped, they are mixed with the cobalt raw material and added during coprecipitation, thereby ensuring the uniformity of doping; in addition, in the preparation method, carbon dioxide is introduced during the calcination process to form a lithium carbonate shell layer on the surface of the sample, which is simple to operate and has low cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0066] Figure 1 This is a SEM image of the surface of the positive electrode material provided in Example 1.

[0067] Figure 2 This is a SEM image of the cross section of the positive electrode material provided in Example 1.

[0068] Figure 3 This is a distribution diagram of the S element in the cross section of the positive electrode material provided in Example 1.

[0069] Figure 4 This is a distribution diagram of the Nb element in the cross section of the positive electrode material provided in Example 1. DETAILED DESCRIPTION

[0070] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0071] Example 1

[0072] The present embodiment provides a positive electrode material doped with both anions and cations, the positive electrode material comprising a LiCoO2 core doped with S and Nb, and a lithium carbonate shell coating the LiCoO2 core doped with S and Nb.

[0073] The preparation method of the positive electrode material comprises:

[0074] (1) adding an ammonium bicarbonate solution with a concentration of 100 g / L and a mixed solution containing cobalt chloride with a concentration of 1.5 mol / L, niobium oxalate with a concentration of 0.1 g / L and sodium dodecyl sulfate with a concentration of 2 g / L to a base solution of ammonium bicarbonate with a concentration of 30 g / L, wherein the flow ratio of the ammonium bicarbonate solution to the mixed solution is 1:1, the pH is adjusted to 7.0, the temperature is adjusted to 40° C., and a coprecipitation reaction is performed accompanied by stirring at a rotation speed of 100 rpm, wherein the growth rate of the precipitate during the coprecipitation reaction is 0.1 μm / h, and a precipitate is obtained;

[0075] (2) heating the precipitate obtained in step (1) to 500° C. at a rate of 2° C. / min and then keeping the temperature for 3 h to obtain an oxide precursor, and then mixing the obtained oxide precursor with lithium hydroxide at a mass ratio of 1:1.1, and then heating it to 700° C. at a rate of 2° C. / min and keeping the temperature for 12 h to obtain a lithium cobalt oxide precursor;

[0076] (3) The lithium cobalt oxide precursor obtained in step (2) is naturally cooled to 500° C. and then sintered for 5 minutes, during which carbon dioxide is introduced to obtain the positive electrode material.

[0077] The surface of the obtained positive electrode material was scanned by a scanning electron microscope to obtain a SEM image of the surface of the positive electrode material. Figure 1 As shown;

[0078] The cross section of the obtained positive electrode material was scanned using a scanning electron microscope to obtain a SEM image of the cross section of the positive electrode material. Figure 2 As shown;

[0079] The cross section of the obtained positive electrode material was scanned by EDS energy spectrum to obtain the distribution diagram of S element in the cross section of the positive electrode material as shown in Figure 3 As shown;

[0080] The cross section of the obtained positive electrode material was scanned by EDS energy spectrum to obtain the distribution diagram of Nb element in the cross section of the positive electrode material. Figure 4 shown.

[0081] Example 2

[0082] The present embodiment provides a positive electrode material doped with both anions and cations, the positive electrode material comprising a LiCoO2 core doped with S and Nb, and a lithium carbonate shell coating the LiCoO2 core doped with S and Nb.

[0083] The preparation method of the positive electrode material comprises:

[0084] (1) adding a sodium bicarbonate solution with a concentration of 200 g / L and a mixed solution containing cobalt sulfate with a concentration of 1.8 mol / L, niobium chloride with a concentration of 0.08 g / L and sodium p-alkylbenzene sulfonate with a concentration of 3 g / L to an ammonia base solution with a concentration of 20 g / L, wherein the flow ratio of the sodium bicarbonate solution to the mixed solution is 2:1 during the simultaneous addition, adjusting the pH to 8, adjusting the temperature to 50° C., and stirring at a rotation speed of 60 rpm to perform a coprecipitation reaction, wherein the growth rate of the precipitate during the coprecipitation reaction is 0.02 μm / h, and obtaining a precipitate;

[0085] (2) heating the precipitate obtained in step (1) to 600° C. at a rate of 5° C. / min and then keeping the temperature for 2 h to obtain an oxide precursor, and then mixing the obtained oxide precursor with lithium carbonate at a mass ratio of 1:1, and then heating it to 800° C. at a rate of 5° C. / min and keeping the temperature for 14 h to obtain a lithium cobalt oxide precursor;

[0086] (3) The lithium cobalt oxide precursor obtained in step (2) is naturally cooled to 450° C. and then sintered for 7 minutes, during which carbon dioxide is introduced to obtain the positive electrode material.

[0087] Example 3

[0088] The present embodiment provides a positive electrode material doped with both anions and cations, the positive electrode material comprising a LiCoO2 core doped with S and Nb, and a lithium carbonate shell coating the LiCoO2 core doped with S and Nb.

[0089] The preparation method of the positive electrode material comprises:

[0090] (1) adding a 50 g / L ammonium bicarbonate solution and a mixed solution containing 2 mol / L cobalt chloride, 0.12 g / L niobium acetate and 5 g / L sodium dodecyl sulfate to a 40 g / L ammonium bicarbonate solution base solution, wherein the flow ratio of the ammonium bicarbonate solution to the mixed solution is 3:1, the pH is adjusted to 8.5, the temperature is adjusted to 60° C., and a coprecipitation reaction is performed with stirring at a rotation speed of 200 rpm, wherein the growth rate of the precipitate during the coprecipitation reaction is 0.2 μm / h, and a precipitate is obtained;

[0091] (2) heating the precipitate obtained in step (1) to 700° C. at a rate of 10° C. / min and then keeping the temperature for 1 h to obtain an oxide precursor, and then mixing the obtained oxide precursor with lithium hydroxide at a mass ratio of 1:1.3, and then heating it to 900° C. at a rate of 10° C. / min and keeping the temperature for 8 h to obtain a lithium cobalt oxide precursor;

[0092] (3) The lithium cobalt oxide precursor obtained in step (2) is naturally cooled to 550° C. and then sintered for 3 minutes, during which carbon dioxide is introduced to obtain the positive electrode material.

[0093] Example 4

[0094] This embodiment provides a positive electrode material doped with both anions and cations. Except that the concentration of niobium oxalate in step (1) of the method for preparing the positive electrode material is 0.05 g / L, the rest is the same as that of embodiment 1.

[0095] Example 5

[0096] This embodiment provides a positive electrode material doped with both anions and cations. Except that the concentration of niobium oxalate in step (1) of the method for preparing the positive electrode material is 0.15 g / L, the rest is the same as that of embodiment 1.

[0097] Example 6

[0098] This embodiment provides a positive electrode material doped with both anions and cations. Except that the concentration of sodium dodecyl sulfate in step (1) of the method for preparing the positive electrode material is 1 g / L, the rest is the same as that of embodiment 1.

[0099] Example 7

[0100] This embodiment provides a positive electrode material doped with both anions and cations. Except that the concentration of sodium dodecyl sulfate in step (1) of the method for preparing the positive electrode material is 8 g / L, the rest is the same as that of embodiment 1.

[0101] Example 8

[0102] This embodiment provides a positive electrode material doped with both anions and cations. Except for step (2) of the method for preparing the positive electrode material, the precipitate obtained in step (1) is heated to 400° C. and then kept warm to obtain an oxide precursor. The rest is the same as in embodiment 1.

[0103] Example 9

[0104] This embodiment provides a positive electrode material doped with both anions and cations. Except for step (2) of the method for preparing the positive electrode material, the precipitate obtained in step (1) is heated to 800° C. and then kept warm to obtain an oxide precursor. The rest is the same as that of embodiment 1.

[0105] Example 10

[0106] This embodiment provides a positive electrode material doped with both anions and cations. The preparation method of the positive electrode material is the same as that of Embodiment 1 except that the oxide precursor is mixed with lithium and calcined, and then the temperature is reduced to 300° C. and then kept warm.

[0107] Embodiment 11

[0108] This embodiment provides a positive electrode material doped with both anions and cations. The preparation method of the positive electrode material is the same as that of Embodiment 1 except that the oxide precursor is mixed with lithium and calcined, and then the temperature is reduced to 700° C. and then kept warm.

[0109] Comparative Example 1

[0110] This comparative example provides a positive electrode material, which is the same as Example 1 except that the S- and Nb-doped LiCoO2 core is replaced by the LiCoO2 core, that is, the niobium oxalate and sodium dodecyl sulfate contained in the mixed solution in step (1) of the preparation method of the positive electrode material are omitted.

[0111] Comparative Example 2

[0112] This comparative example provides a positive electrode material doped with both anions and cations, which is the same as Example 1 except that the lithium carbonate shell coating the outside of the S and Nb-doped LiCoO2 core is replaced by a carbon shell, i.e., the introduction of carbon dioxide during the sintering process in step (3) of the preparation method of the positive electrode material is omitted.

[0113] Comparative Example 3

[0114] This comparative example provides a positive electrode material doped with both anions and cations, which is the same as Example 1 except that the lithium carbonate shell covering the outside of the S- and Nb-doped LiCoO2 core is omitted, that is, step (3) of the preparation method of the positive electrode material is omitted.

[0115] A positive electrode sheet is prepared using the positive electrode materials provided in Examples 1 to 11 and Comparative Examples 1 to 3, and the preparation method of the positive electrode sheet is as follows: 80 wt% of the positive electrode active material, 10 wt% of Super-P and 10 wt% of polyvinylidene fluoride (PVDF) are dispersed in an N-methylpyrrolidone (NMP) solution to prepare an electrode slurry, which is coated on an aluminum foil and dried to obtain a positive electrode sheet; a lithium-ion battery is prepared using the obtained positive electrode sheet, and the preparation method of the lithium-ion battery is as follows: 1 mol / L LiPF6 is used as an electrolyte, a graphite electrode is used as a negative electrode, the above-mentioned positive electrode sheet is used as a positive electrode, and a CR2032 button battery is assembled.

[0116] The obtained lithium-ion battery was tested for capacity and cycle stability. The test method is as follows: using a battery test system, the lithium-ion battery was tested at 25°C in a 0.5C (1C = 250 mAh / g) charge and discharge regime within a voltage range of 2V to 4.65V. The first cycle capacity at 0.5C and the capacity retention rate after 100 cycles are shown in Table 1.

[0117] The obtained lithium-ion battery was subjected to a kinetic performance test, and the battery Warburg impedance was used to characterize the diffusion kinetics of lithium ions in the material. The smaller the impedance, the easier the lithium ions migrate. The battery electrochemical impedance spectrum and equivalent circuit were tested using an electrochemical workstation to obtain the battery Warburg impedance. -2 -10 5 In the HZ range, the test results are shown in Table 1.

[0118] Table 1

[0119] First cycle capacity (mA·h / g) Capacity retention rate (%) Warburg impedance(Ω) Example 1 203.1 93.1 41.52 Example 2 205.2 93.9 38.27 Example 3 202.9 92.5 32.27 Example 4 199.5 87.3 53.15 Example 5 191.3 91.8 51.18 Example 6 196.5 88.1 95.38 Example 7 197.6 84.2 43.44 Example 8 187.5 89.4 75.69 Example 9 189 82.5 83.77 Example 10 194.5 88.5 65.29 Embodiment 11 189.6 87.5 73.52 Comparative Example 1 187.3 81.3 117.22 Comparative Example 2 185.7 85.3 94.86 Comparative Example 3 184.5 83.1 101.02

[0120] From Table 1, we can get:

[0121] (1) The lithium-ion battery prepared with the anion-cation dual-doped positive electrode material provided in Examples 1 to 3 exhibits a high capacity retention rate in the cycle stability test and has excellent kinetic performance;

[0122] (2) By comparing Example 1 with Examples 4 and 5, it can be seen that the concentration of niobium oxalate in step (1) of the method for preparing the positive electrode material of the present invention will affect the doping amount of Nb in the positive electrode material and thus affect the performance of the lithium-ion battery; when the concentration of the Nb source is low, the capacity retention rate of the lithium-ion battery will be low and the kinetic performance will be poor. This is because the low doping amount of Nb has limited enhancement on the stability of the material structure, and the material structure collapses during the charge and discharge cycle, and the electrochemical performance deteriorates; when the concentration of the Nb source is high, the capacity of the lithium-ion battery will be slightly reduced. This is because Nb itself does not provide lithium ion storage capacity, and excessive Nb reduces the material capacity density;

[0123] (3) By comparing Example 1 with Examples 6 and 7, it can be seen that the concentration of the S source in step (1) of the method for preparing the positive electrode material of the present invention affects the performance of the lithium-ion battery; when the concentration of the S source is low, the improvement of the positive electrode material is not obvious; when the concentration of the S source is high, the capacity retention rate decreases. This is because too high a sulfur content will make the electrolyte in the battery unstable, thereby accelerating the aging of the battery;

[0124] (4) By comparing Example 1 with Examples 8 and 9, it can be seen that the end temperature of the first heating in the preparation method of the positive electrode material of the present invention will affect the performance of the lithium-ion battery; when the end temperature of the first heating is low, the calcination is incomplete, the doping elements are unstable, and the material tap density is low, resulting in a very low capacity density of the subsequent lithium-ion battery; when the end temperature of the first heating is high, it will be over-burned, and the cobalt oxide spherical particles will have a large number of cracks or even break, resulting in deterioration of the electrochemical performance of the material;

[0125] (5) By comparing Example 1 with Examples 10 and 11, it can be seen that the temperature of sintering after calcining mixed lithium and cooling in the preparation method of the positive electrode material of the present invention will affect the performance of the lithium-ion battery; when the sintering temperature is low, the capacity retention rate of the lithium-ion battery will be reduced and the kinetic performance will be poor. This is because it is difficult to form a tight lithium carbonate protective shell on the surface of the material when the calcination temperature is too low; when the sintering temperature is high, the capacity of the lithium-ion battery will be reduced. This is because the high temperature causes the material structure to be destroyed after calcination, making it difficult for lithium ions to escape, and on the other hand, it also causes energy waste;

[0126] (6) By comparing Example 1 with Comparative Examples 1 to 3, it can be seen that the anion-cation dual-doped positive electrode material provided by the present invention is doped with S and Nb. S can significantly improve the charge transfer kinetics of the battery and significantly reduce Li + The migration barrier of Li + The rapid migration of Nb improves the electrochemical kinetic performance and capacity of the battery; Nb element doping and strong Nb-O bonds can effectively stabilize the TMO skeleton, inhibit voltage decay and enhance cycle stability; the positive electrode material contains a lithium carbonate shell, which can inhibit the side reaction of particles and electrolyte and reduce cracks caused by material strain during charging and discharging; therefore, the lithium ion battery prepared with the positive electrode material provided in the present invention has excellent cycle stability, strong kinetic performance and high capacity.

[0127] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A positive electrode material doped with both anions and cations, It is characterized in that The positive electrode material includes a S and Nb doped core and a lithium carbonate shell coated outside the S and Nb doped core.

2. The positive electrode material according to claim 1, It is characterized in that The S and Nb doped core comprises S and Nb doped LiCoO 2 Core, S and Nb doped LiMn 2 O 4 Core, S and Nb doped LiNi 0.5 Mn 1.5 O 4 Core, S and Nb doped LiNi x Co y Mn 1-x-y O 2 Any one of the cores, preferably S and Nb doped LiCoO 2 nuclear; Preferably, the LiNi x Co y Mn 1-x-y O 2 0 <x<1,0<y<1。 3. A method for preparing the positive electrode material according to claim 1 or 2, It is characterized in that The preparation method comprises: (1) mixing a base solution, a precipitant solution, and a mixed solution containing a Co source, a Nb source, and a S source to perform a coprecipitation reaction to obtain a precipitate; (2) calcining the precipitate obtained in step (1) to obtain an oxide precursor, mixing the obtained oxide precursor with a lithium source, and then calcining it for a second time to obtain a lithium cobalt oxide precursor; (3) Sintering the lithium cobalt oxide precursor obtained in step (2), introducing carbon dioxide during the sintering process, to obtain the positive electrode material.

4. The preparation method according to claim 3, It is characterized in that The base liquid in step (1) comprises ammonium bicarbonate solution and / or ammonia water; Preferably, the concentration of the base solution in step (1) is 20 to 40 g / L; Preferably, the precipitant solution in step (1) comprises any one of ammonium bicarbonate solution, sodium carbonate solution or sodium bicarbonate solution or a combination of at least two thereof; Preferably, the concentration of the precipitant solution in step (1) is 50 to 200 g / L; Preferably, the Co source in step (1) comprises any one of cobalt chloride, cobalt sulfate or cobalt nitrate, or a combination of at least two thereof; Preferably, the concentration of the Co source in the mixed solution in step (1) is 1.5 to 2 mol / L; Preferably, the Nb source in step (1) comprises any one of niobium oxalate, niobium acetate or niobium chloride, or a combination of at least two thereof; Preferably, the concentration of the Nb source in the mixed solution in step (1) is 0.08 to 0.12 g / L; Preferably, the S source in step (1) comprises sodium dodecyl sulfonate and / or sodium p-alkylbenzene sulfonate; Preferably, the concentration of the S source in the mixed solution in step (1) is 2 to 5 g / L.

5. The preparation method according to claim 3 or 4, It is characterized in that The mixing in step (1) comprises: adding a precipitant solution and a mixed solution containing a Co source, a Nb source and a S source to the base solution simultaneously; Preferably, the flow ratio of the precipitant solution to the mixed solution during the simultaneous addition is (1-3):1; Preferably, the synchronous addition process is accompanied by stirring at a speed of 60 to 200 rpm; Preferably, during the simultaneous addition, the pH is adjusted to 7.0-8.5 and the temperature is adjusted to 40-60°C; Preferably, the growth rate of the precipitate during the coprecipitation reaction in step (1) is 0.02 to 0.2 μm / h.

6. The preparation method according to any one of claims 3 to 5, It is characterized in that Step (2) the first calcination comprises a first heating and a first heat preservation performed sequentially; Preferably, the first heating rate is 2-10°C / min, the end temperature is 500-700°C, and the first insulation time is 1-3h; Preferably, the mass ratio of the oxide precursor to the lithium source in step (2) is 1:(1-1.3); Preferably, the second calcination in step (2) comprises a second heating and a second heat preservation performed sequentially; Preferably, the second heating rate is 2-10° C. / min, the end temperature is 700-900° C., and the second insulation time is 8-14 h.

7. The preparation method according to any one of claims 3 to 6, It is characterized in that The sintering temperature in step (3) is 450-550° C. and the sintering time is 3-7 min. Preferably, step (3) also includes cooling by natural cooling before sintering.

8. The preparation method according to any one of claims 3 to 7, It is characterized in that The preparation method comprises: (1) adding a precipitant solution with a concentration of 50 to 200 g / L and a mixed solution containing a Co source with a concentration of 1.5 to 2 mol / L, a Nb source with a concentration of 0.08 to 0.12 g / L and a S source with a concentration of 2 to 5 g / L to a base solution with a concentration of 20 to 40 g / L, wherein the flow ratio of the precipitant solution to the mixed solution is (1 to 3):1 during the simultaneous addition, adjusting the pH to 7.0 to 8.5, adjusting the temperature to 40 to 60° C., and stirring at a speed of 60 to 200 rpm to perform a coprecipitation reaction, wherein the growth rate of the precipitate during the coprecipitation reaction is 0.02 to 0.2 μm / h, and obtaining a precipitate; (2) heating the precipitate obtained in step (1) to 500-700° C. at a rate of 2-10° C. / min and then keeping the temperature for 1-3 hours to obtain an oxide precursor, and then mixing the obtained oxide precursor with a lithium source at a mass ratio of 1:(1-1.3), and then heating it to 700-900° C. at a rate of 2-10° C. / min and keeping the temperature for 8-14 hours to obtain a lithium cobalt oxide precursor; (3) The lithium cobalt oxide precursor obtained in step (2) is naturally cooled to 450-550° C. and then sintered for 3-7 minutes, during which carbon dioxide is introduced to obtain the positive electrode material.

9. A positive electrode sheet, It is characterized in that The positive electrode sheet comprises the positive electrode material according to claim 1 or 2.

10. A lithium ion battery, It is characterized in that The lithium-ion battery comprises the positive electrode sheet according to claim 9.