Doped polyanion material as well as preparation method and application thereof
By using monovalent positive ion doping technology in iron-based polyanionic materials, Na4+xMxFe3-x(PO4)2P2O7 is formed, the shortcomings in rate performance and cycle stability of iron-based polyanionic materials are solved, and high capacity is achieved Combined with excellent cycle stability and rate performance.
Patent Information
- Application Number
- CN202311351867.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-18
- Publication Date
- 2024-11-08
AI Technical Summary
It is difficult for iron-based polyanionic cathode materials to have high rate performance and high cycle stability, and existing methods are difficult to effectively suppress lattice distortion during charging and discharging, resulting in poor rate performance and cycle performance of sodium ion batteries.
The monovalent positive ion M part replaces the divalent Fe element to form the doped polyanionic material Na4+xMxFe3-x(PO4)2P2O7, which improves electron conductivity and sodium ion diffusion, inhibits lattice distortion, and passes through multiple ions or ions. The synergistic effect of the group optimizes capacity, cycle stability and rate performance.
The specific capacity, rate performance and cyclic stability of polyanionic materials are significantly improved, and the optimal balance of capacity, cycle stability and rate performance is achieved.
Smart Images

Figure CN118919716A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of methods or devices for directly converting electrical energy into chemical energy, and more specifically, to a doped polyanion material and a preparation method and application thereof. Background Art
[0002] At present, lithium-ion batteries represented by lithium iron phosphate dominate energy storage batteries, but lithium resources are limited and it is difficult to meet the rapid development of automotive electrification. Compared with lithium-ion batteries, sodium-ion batteries have advantages such as abundant resources and are more suitable for large-scale energy storage. The positive electrode material of sodium-ion batteries is the key factor restricting its performance. Currently, the materials suitable for positive electrode materials of sodium-ion batteries mainly include layered oxides, Prussian blue materials and polyanion materials. Among them, polyanion materials have the characteristics of stable structure, high cycle life, high thermal stability and high operating voltage, and are more suitable as positive electrode materials for sodium-ion batteries.
[0003] Polyanion cathode materials are mainly divided into vanadium-based polyanion materials and iron-based polyanion materials. Vanadium-based polyanion materials are rich in vanadium valence states (V 2+ 、V 3+ 、V 4+ or V 5+ ), high redox potential, fast sodium ion diffusion, stable structure and other advantages have attracted widespread attention, but due to the high price and toxicity of vanadium, the cost of sodium ion batteries is high, making it difficult to achieve large-scale application. Compared with vanadium-based polyanion materials, iron-based polyanion materials not only have higher theoretical capacity and moderate working voltage, but also have three-dimensional sodium ion diffusion channels and unique phosphate and pyrophosphate mixed ion stable structure, which gives them excellent cycle performance, but their low conductivity and lattice distortion during charging and discharging lead to poor rate performance and cycle performance of sodium ion batteries.
[0004] At present, the above problems are mainly solved by methods such as cation doping, carbon layer coating and particle refinement. For example, the prior art discloses a positive electrode material and a preparation method thereof, in which the ternary metal (Ni x Co y Mn z ) is doped into lithium iron phosphate in the form of cations to replace the Fe element to improve ion conductivity and the migration rate of ions in the material. At the same time, an organic carbon source is deposited on the surface of the material and then carbonized at high temperature to form an amorphous carbon coating to improve the electronic conductivity of the material, thereby improving the rate performance of the sodium ion battery. However, this method is difficult to effectively suppress the lattice distortion during the charge and discharge process, resulting in the cycle stability of the sodium ion battery. Summary of the invention
[0005] The purpose of the present invention is to overcome the defects and shortcomings of existing iron-based polyanion positive electrode materials that are difficult to have both high rate performance and high cycle stability, and to provide a doped polyanion material.
[0006] Another object of the present invention is to provide a method for preparing a doped polyanion material.
[0007] Another object of the present invention is to provide an application of a doped polyanion material in a positive electrode sheet or a sodium ion battery.
[0008] Another object of the present invention is to provide a positive electrode plate comprising the above-mentioned doped polyanion material.
[0009] Another object of the present invention is to provide a sodium ion battery comprising the above-mentioned doped polyanion material.
[0010] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0011] The present invention protects a doped polyanion material, the chemical formula of which is Na 4+ x M x Fe 3-x (PO4)2P2O7; wherein M is a monovalent positive ion and its doping position is Fe, 0.03≤x≤0.3.
[0012] The inventors have found through research that the partial replacement of the divalent Fe element with a monovalent positive ion M (either a metal ion or a non-metal ion) is not only beneficial for reducing the band gap to improve the electronic conductivity of the polyanion material, but also for improving the electrochemical activity of the polyanion material, thereby improving its specific capacity and rate performance; it can also effectively increase the interstitial Na content in the polyanion material, so that Na 4+x M x Fe 3-x The Na content in (PO4)2P2O7 is greater than 4, which can significantly promote the diffusion of sodium ions and thus significantly improve the rate performance of polyanion materials; it can also inhibit the lattice distortion of polyanion materials during sodium removal and improve their cycle stability.
[0013] Optionally, Na 4+x M x Fe 3-x The value range of x in (PO4)2P2O7 is 0.03 to 0.15; specifically, it can be 0.03, 0.05, 0.07, 0.09, 0.1, 0.13 or 0.15.
[0014] Optionally, the M is Li + , K + , Rb + , Cs +, Cu + 、Ag + or NH4 + Preferably, M is Li + , K + , Rb + , Cs + , Cu + 、Ag + or NH4 + At least two of the .
[0015] At the same time, the study found that when the doping element M contains Li, due to Li I -O bond length and Fe II -O bond length is the same, which can promote Li to enter Na 4+x M x Fe 3-x (PO4)2P2O7 lattice is evenly distributed, and during the charge and discharge process, Li + The valence is unchanged, and the Fe(Li)O6 octahedral structure can be stabilized, thereby stabilizing the lattice and improving the cycle stability of the polyanion material. Therefore, the M is preferably Li + , K + , Rb + , Cs + , Cu + 、Ag + or NH4 + At least two of which one is Li + .
[0016] Specifically, the doped polyanion material has an orthorhombic crystal structure, wherein the M element is evenly distributed in the crystal lattice, and the M element and the O element are in octahedral coordination.
[0017] The present invention also protects a method for preparing the above-mentioned doped polyanion material, comprising the following steps:
[0018] The pre-sintered product is first sintered at 250-400° C. in an inert atmosphere for 2-8 hours, and then calcined at 450-600° C. in an inert atmosphere for 5-15 hours to obtain a doped polyanion material;
[0019] The pre-sintered product is prepared from a phosphorus source, a sodium source, an iron source, a carbon source and an M source by a sol-gel method, a spray drying method or a direct solid phase reaction method.
[0020] Specifically, the above-mentioned phosphorus source can be one or more of sodium dihydrogen phosphate, ammonium dihydrogen phosphate, sodium pyrophosphate, disodium hydrogen phosphate or phosphoric acid; the sodium source can be one or more of sodium oxide, sodium hydroxide, sodium carbonate, sodium nitrate or sodium citrate; the iron source can be one or more of ferric nitrate, ferric oxide, ferric oxalate, ferric oxide or ferric acetate; the carbon source can be one or more of citric acid, oxalic acid, glucose, fructose or starch; the M source can be a salt and / or oxide of element M.
[0021] Optionally, the inert atmosphere may be an argon atmosphere or a nitrogen atmosphere. After the calcination treatment, the doped polyanion material may be crushed and sieved to obtain a suitable particle size according to actual needs, and may also be subjected to a demagnetization treatment.
[0022] Optionally, the pre-sintered product can be prepared by a sol-gel method, which specifically includes the following steps: dissolving ammonium dihydrogen phosphate, sodium nitrate, ferric nitrate, citric acid (also serving as a chelating agent, carbon source, and reducing agent), and nitrate of element M (such as LiNO3) in deionized water, stirring to form a sol, and then stirring under certain temperature conditions (60-90°C) to form a gel, and then drying the gel to remove water to obtain a pre-sintered product.
[0023] Optionally, the pre-sintered product can also be prepared by spray drying, which specifically includes the following steps: mixing sodium dihydrogen phosphate, ferric nitrate, nitrate of element M (such as lithium nitrate), ammonium dihydrogen phosphate and water-soluble organic matter (such as oxalic acid, citric acid or glucose, etc., which also serve as a carbon source and a reducing agent) by sand milling, the sand milling speed is generally set to 1000-2000rpm, the sand milling time is generally 1-10h, and then the sand milling slurry is spray dried to obtain a pre-sintered product.
[0024] Optionally, the pre-sintered product can also be prepared by a direct solid phase reaction method, which specifically includes the following steps: sodium carbonate, ferrous oxalate, oxalate of element M (such as lithium oxalate), diammonium phosphate and water-soluble organic matter (such as oxalic acid, citric acid or glucose, etc., which also serve as a carbon source and a reducing agent) are mixed evenly by ball milling (the ball milling can be dry ball milling or wet ball milling, and the role of ball milling is to improve the uniformity of the mixture; wet ball milling is preferred, with anhydrous ethanol, acetone, etc. as the ball milling medium, the ball milling speed is generally set to 300-500rpm, and the ball milling time is generally 5-15h), and the pre-sintered product is obtained by drying.
[0025] The use of the above-mentioned doped polyanion material in a positive electrode sheet or a sodium ion battery is also within the protection scope of the present invention.
[0026] The present invention also protects a positive electrode plate, comprising a current collector and a positive electrode active material layer disposed on at least one side of the current collector, wherein the positive electrode active material layer comprises the above-mentioned doped polyanion material.
[0027] The present invention also protects a sodium ion battery, comprising a positive electrode plate, a negative electrode plate, and an electrolyte (which may be a solid electrolyte or a liquid electrolyte + a separator) located between the positive electrode plate and the negative electrode plate, wherein the positive electrode plate comprises the above-mentioned doped polyanion material.
[0028] Compared with the prior art, the present invention has the following beneficial technical effects:
[0029] The doped polyanion material of the present invention adopts monovalent positive ions M to partially replace divalent Fe elements, which is not only beneficial to reducing the band gap to improve the electronic conductivity of the polyanion material, improve the electrochemical activity of the polyanion material, and thus improve its specific capacity and rate performance; it can also effectively increase the interstitial Na content in the polyanion material, significantly promote the diffusion of sodium ions, and thus significantly improve the rate performance of the polyanion material; it can also inhibit the lattice distortion of the polyanion material during sodium removal, improve its cycle stability, and achieve an optimized balance of capacity, cycle stability and rate performance through the synergistic effect of multiple ions or ion groups. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is the X-ray diffraction pattern (XRD) of the doped polyanion material in Example 1.
[0031] Figure 2 This is a charge and discharge curve diagram of the doped polyanion material in Example 1. DETAILED DESCRIPTION
[0032] The present invention is further described below in conjunction with specific embodiments, but the embodiments do not limit the present invention in any form. Unless otherwise specified, the raw materials and reagents used in the embodiments of the present invention are conventionally purchased raw materials and reagents.
[0033] Example 1
[0034] A doped polyanion material, the chemical formula of which is Na 4.05 Li 0.05 Fe 2.95 (PO4)2P2O7.
[0035] The above-mentioned doped polyanion material can be prepared by the following preparation method:
[0036] S1. According to the doped polyanion material (Na 4.05 Li 0.05 Fe 2.95(PO4)2P2O7) stoichiometric ratio, and the pre-sintered product was prepared by spray drying;
[0037] S2. The pre-sintered product in S1 is first sintered at 300° C. in a nitrogen atmosphere for 4 hours, and then the temperature is increased to 500° C. and the sintering treatment is continued for 10 hours to obtain a doped polyanion material.
[0038] Among them, the specific steps of preparing the pre-sintered product by the above-mentioned spray drying method are as follows: NaH2PO4, NaNO3, LiNO3, Fe(NO3)3 and citric acid are mixed evenly by sand grinding (the sand grinding speed is 1000-2000rpm, and the sand grinding time is 1-10h), and then the sand grinding slurry is spray dried to obtain the pre-sintered product.
[0039] Example 2
[0040] A doped polyanion material, the chemical formula of which is Na 4.1 Li 0.1 Fe 2.9 (PO4)2P2O7.
[0041] The above-mentioned doped polyanion material can be prepared by the following preparation method:
[0042] S1. According to the doped polyanion material (Na 4.1 Li 0.1 Fe 2.9 (PO4)2P2O7) stoichiometric ratio, and a pre-sintered product was prepared by spray drying (the specific preparation method of the pre-sintered product is the same as that in Example 1);
[0043] S2. The pre-sintered product in S1 is first sintered at 300° C. in a nitrogen atmosphere for 4 hours, and then the temperature is increased to 500° C. and the sintering treatment is continued for 10 hours to obtain a doped polyanion material.
[0044] Example 3
[0045] A doped polyanion material, the chemical formula of which is Na 4.03 Li 0.03 Fe 2.97 (PO4)2P2O7.
[0046] The above-mentioned doped polyanion material can be prepared by the following preparation method:
[0047] S1. According to the doped polyanion material (Na 4.03 Li 0.03 Fe 2.97 (PO4)2P2O7) stoichiometric ratio, and a pre-sintered product was prepared by spray drying (the specific preparation method of the pre-sintered product is the same as that in Example 1);
[0048] S2. The pre-sintered product in S1 is first sintered at 300° C. in a nitrogen atmosphere for 4 hours, and then the temperature is increased to 500° C. and the sintering treatment is continued for 10 hours to obtain a doped polyanion material.
[0049] Example 4
[0050] A doped polyanion material, the chemical formula of which is Na 4.05 K 0.05 Fe 2.95 (PO4)2P2O7.
[0051] The above-mentioned doped polyanion material can be prepared by the following preparation method:
[0052] S1. According to the doped polyanion material (Na 4.05 K 0.05 Fe 2.95 (PO4)2P2O7) stoichiometric ratio, and a pre-sintered product was prepared by spray drying (the specific preparation method of the pre-sintered product is the same as that in Example 1);
[0053] S2. The pre-sintered product in S1 is first sintered at 350° C. in a nitrogen atmosphere for 3 h, then the temperature is raised to 510° C. and the calcination is continued for 11 h to obtain a doped polyanion material.
[0054] Example 5
[0055] A doped polyanion material, the chemical formula of which is Na 4.1 K 0.1 Fe 2.9 (PO4)2P2O7.
[0056] The above-mentioned doped polyanion material can be prepared by the following preparation method:
[0057] S1. According to the doped polyanion material (Na 4.1 K 0.1 Fe 2.9 (PO4)2P2O7) stoichiometric ratio, and a pre-sintered product was prepared by spray drying (the specific preparation method of the pre-sintered product is the same as that in Example 1);
[0058] S2. The pre-sintered product in S1 is first sintered at 350° C. in a nitrogen atmosphere for 3 h, then the temperature is raised to 510° C. and the calcination is continued for 11 h to obtain a doped polyanion material.
[0059] Example 6
[0060] A doped polyanion material, the chemical formula of which is Na 4.1K 0.05 Li 0.05 Fe 2.9 (PO4)2P2O7.
[0061] The above-mentioned doped polyanion material can be prepared by the following preparation method:
[0062] S1. According to the doped polyanion material (Na 4.1 K 0.05 Li 0.05 Fe 2.9 (PO4)2P2O7) stoichiometric ratio, and a pre-sintered product was prepared by spray drying (the specific preparation method of the pre-sintered product is the same as that in Example 1);
[0063] S2. The pre-sintered product in S1 is first sintered at 300° C. in a nitrogen atmosphere for 4 hours, and then the temperature is increased to 500° C. and the sintering treatment is continued for 10 hours to obtain a doped polyanion material.
[0064] Example 7
[0065] A doped polyanion material, the chemical formula of which is Na 4.05 Li 0.05 Fe 2.95 (PO4)2P2O7.
[0066] The above-mentioned doped polyanion material can be prepared by the following preparation method:
[0067] S1. According to the doped polyanion material (Na 4.05 Li 0.05 Fe 2.95 (PO4)2P2O7) stoichiometric ratio, the pre-sintered product was prepared by sol-gel method;
[0068] S2. The pre-sintered product in S1 is first sintered at 300° C. in a nitrogen atmosphere for 4 hours, and then the temperature is increased to 500° C. and the sintering treatment is continued for 10 hours to obtain a doped polyanion material.
[0069] Among them, the specific steps of preparing the pre-sintered product by the above-mentioned sol-gel method are as follows: dissolve NH4H2PO4, NaNO3, LiNO3, Fe(NO3)3 and citric acid in deionized water, stir to form a sol, then stir at 80°C to form a gel, and then dry the gel to obtain a pre-sintered product.
[0070] Example 8
[0071] A doped polyanion material, the chemical formula of which is Na 4.05 Cu 0.05 Fe 2.95(PO4)2P2O7.
[0072] The above-mentioned doped polyanion material can be prepared by the following preparation method:
[0073] S1. According to the doped polyanion material (Na 4.05 Cu 0.05 Fe 2.95 (PO4)2P2O7) stoichiometric ratio, and the pre-sintered product was prepared by spray drying;
[0074] S2. The pre-sintered product in S1 is first sintered at 320° C. in a nitrogen atmosphere for 4 hours, and then the temperature is increased to 510° C. and the sintering treatment is continued for 10 hours to obtain a doped polyanion material.
[0075] Among them, the specific steps of preparing the pre-sintered product by the above-mentioned spray drying method are as follows: NaH2PO4, NaNO3, Cu2O, Fe(NO3)3 and citric acid are mixed evenly by sand grinding (the sand grinding speed is 1000-2000rpm, and the sand grinding time is 1-10h), and then the sand grinding slurry is spray dried to obtain the pre-sintered product.
[0076] Example 9
[0077] A doped polyanion material, the chemical formula of which is Na 4.05 Ag 0.05 Fe 2.95 (PO4)2P2O7.
[0078] The above-mentioned doped polyanion material can be prepared by the following preparation method:
[0079] S1. According to the doped polyanion material (Na 4.05 Ag 0.05 Fe 2.95 (PO4)2P2O7) stoichiometric ratio, and the pre-sintered product was prepared by spray drying;
[0080] S2. The pre-sintered product in S1 is first sintered at 320° C. in a nitrogen atmosphere for 4 hours, and then the temperature is increased to 510° C. and the sintering treatment is continued for 10 hours to obtain a doped polyanion material.
[0081] Among them, the specific steps of preparing the pre-sintered product by the above-mentioned spray drying method are as follows: NaH2PO4, NaNO3, AgNO3, Fe(NO3)3 and citric acid are mixed evenly by sand grinding (the sand grinding speed is 1000-2000rpm, and the sand grinding time is 1-10h), and then the sand grinding slurry is spray dried to obtain the pre-sintered product.
[0082] Example 10
[0083] A doped polyanion material, the chemical formula of which is Na 4.05 Ag 0.02 Li 0.03 Fe 2.96 (PO4)2P2O7.
[0084] The above-mentioned doped polyanion material can be prepared by the following preparation method:
[0085] S1. According to the doped polyanion material (Na 4.05 Ag 0.02 Li 0.03 Fe 2.96 (PO4)2P2O7) stoichiometric ratio, and the pre-sintered product was prepared by spray drying;
[0086] S2. The pre-sintered product in S1 is first sintered at 300° C. in a nitrogen atmosphere for 4 hours, and then the temperature is increased to 500° C. and the sintering treatment is continued for 10 hours to obtain a doped polyanion material.
[0087] Among them, the specific steps of preparing the pre-sintered product by the above-mentioned spray drying method are as follows: NaH2PO4, NaNO3, AgNO3, LiNO3, Fe(NO3)3 and citric acid are mixed evenly by sand grinding (the sand grinding speed is 1000-2000rpm, and the sand grinding time is 1-10h), and then the sand grinding slurry is spray dried to obtain the pre-sintered product.
[0088] Comparative Example 1
[0089] A doped polyanion material, the chemical formula of which is Na4Fe3(PO4)2P2O7.
[0090] The above-mentioned doped polyanion material can be prepared by the following preparation method:
[0091] S1. A pre-sintered product was prepared by spray drying according to the stoichiometric ratio of the doped polyanion material (Na4Fe3(PO4)2P2O7);
[0092] S2. The pre-sintered product in S1 is first sintered at 300° C. in a nitrogen atmosphere for 4 hours, and then the temperature is increased to 500° C. and the sintering treatment is continued for 10 hours to obtain a doped polyanion material.
[0093] Among them, the specific steps of preparing the pre-sintered product by the above-mentioned spray drying method are as follows: NaH2PO4, NaNO3, Fe(NO3)3 and citric acid are mixed evenly by sand grinding (the sand grinding speed is 1000-2000rpm, and the sand grinding time is 1-10h), and then the sand grinding slurry is spray dried to obtain the pre-sintered product.
[0094] Comparative Example 2
[0095] A doped polyanion material, the chemical formula of which is Na 4.02 Li 0.02 Fe 2.98 (PO4)2P2O7.
[0096] The above-mentioned doped polyanion material can be prepared by the following preparation method:
[0097] S1. According to the doped polyanion material (Na 4.02 Li 0.02 Fe 2.98 (PO4)2P2O7) stoichiometric ratio, and the pre-sintered product was prepared by spray drying;
[0098] S2. The pre-sintered product in S1 is first sintered at 300° C. in a nitrogen atmosphere for 4 hours, and then the temperature is increased to 500° C. and the sintering treatment is continued for 10 hours to obtain a doped polyanion material.
[0099] Among them, the specific steps of preparing the pre-sintered product by the above-mentioned spray drying method are as follows: NaH2PO4, NaNO3, LiNO3, Fe(NO3)3 and citric acid are mixed evenly by sand grinding (the sand grinding speed is 1000-2000rpm, and the sand grinding time is 1-10h), and then the sand grinding slurry is spray dried to obtain the pre-sintered product.
[0100] Comparative Example 3
[0101] A doped polyanion material, the chemical formula of which is Na 4.4 Li 0.4 Fe 2.6 (PO4)2P2O7.
[0102] The above-mentioned doped polyanion material can be prepared by the following preparation method:
[0103] S1. According to the doped polyanion material (Na 4.4 Li 0.4 Fe 2.6 (PO4)2P2O7) stoichiometric ratio, and the pre-sintered product was prepared by spray drying;
[0104] S2. The pre-sintered product in S1 is first sintered at 300° C. in a nitrogen atmosphere for 4 hours, and then the temperature is increased to 500° C. and the sintering treatment is continued for 10 hours to obtain a doped polyanion material.
[0105] Among them, the specific steps of preparing the pre-sintered product by the above-mentioned spray drying method are as follows: NaH2PO4, NaNO3, LiNO3, Fe(NO3)3 and citric acid are mixed evenly by sand grinding (the sand grinding speed is 1000-2000rpm, and the sand grinding time is 1-10h), and then the sand grinding slurry is spray dried to obtain the pre-sintered product.
[0106] Comparative Example 4
[0107] A doped polyanion material, the chemical formula of which is Na4Cu 0.05 Fe 2.95 (PO4)2P2O7.
[0108] The above-mentioned doped polyanion material can be prepared by the following preparation method:
[0109] S1. According to the doped polyanion material (Na4Cu 0.05 Fe 2.95 (PO4)2P2O7) stoichiometric ratio, and the pre-sintered product was prepared by spray drying;
[0110] S2. The pre-sintered product in S1 is first sintered at 320° C. in a nitrogen atmosphere for 4 hours, and then the temperature is increased to 520° C. and the sintering process is continued for 10 hours to obtain a doped polyanion material.
[0111] Among them, the specific steps of preparing the pre-sintered product by the above-mentioned spray drying method are as follows: NaH2PO4, NaNO3, Cu(NO3)2, Fe(NO3)3 and citric acid are mixed evenly by sand grinding (the sand grinding speed is 1000-2000rpm, and the sand grinding time is 1-10h), and then the sand grinding slurry is spray dried to obtain the pre-sintered product.
[0112] Comparative Example 5
[0113] A doped polyanion material, the chemical formula of which is Na 3.95 Al 0.05 Fe 2.95 (PO4)2P2O7.
[0114] The above-mentioned doped polyanion material can be prepared by the following preparation method:
[0115] S1. According to the doped polyanion material (Na 3.95 Al 0.05 Fe 2.95 (PO4)2P2O7) stoichiometric ratio, and the pre-sintered product was prepared by spray drying;
[0116] S2. The pre-sintered product in S1 is first sintered at 320° C. in a nitrogen atmosphere for 4 hours, and then the temperature is increased to 510° C. and the sintering treatment is continued for 10 hours to obtain a doped polyanion material.
[0117] Among them, the specific steps of preparing the pre-sintered product by the above-mentioned spray drying method are as follows: NaH2PO4, NaNO3, Al(NO3)3, Fe(NO3)3 and citric acid are mixed evenly by sand grinding (the sand grinding speed is 1000-2000rpm, and the sand grinding time is 1-10h), and then the sand grinding slurry is spray dried to obtain the pre-sintered product.
[0118] Comparative Example 6
[0119] A doped polyanion material, the chemical formula of which is Na4Mg 0.05 Fe 2.95 (PO4)2P2O7.
[0120] The above-mentioned doped polyanion material can be prepared by the following preparation method:
[0121] S1. According to the doped polyanion material (Na4Mg 0.05 Fe 2.95 (PO4)2P2O7) stoichiometric ratio, and the pre-sintered product was prepared by spray drying;
[0122] S2. The pre-sintered product in S1 is first sintered at 320° C. in a nitrogen atmosphere for 4 hours, and then the temperature is increased to 510° C. and the sintering treatment is continued for 10 hours to obtain a doped polyanion material.
[0123] Among them, the specific steps of preparing the pre-sintered product by the above-mentioned spray drying method are as follows: NaH2PO4, NaNO3, Mg(NO3)2, Fe(NO3)3 and citric acid are mixed evenly by sand grinding (the sand grinding speed is 1000-2000rpm, and the sand grinding time is 1-10h), and then the sand grinding slurry is spray dried to obtain the pre-sintered product.
[0124] Performance Testing
[0125] (1) XRD test
[0126] The doped polyanion materials in Examples 1 to 10 and Comparative Examples 1 to 6 were subjected to XRD detection, wherein the XRD spectrum of the doped polyanion material in Example 1 is as follows: Figure 1 As shown, it can be seen that the doped polyanion material has an orthorhombic crystal structure, and the XRD spectrum analysis determines that Li +Doping at the Fe position. The XRD patterns of the doped polyanion materials in Examples 2 to 9 are similar to those in Example 1, and analysis thereof can confirm that the monovalent positive ion M is doped at the Fe position.
[0127] (2) Electrochemical performance test
[0128] The doped polyanion materials in Examples 1 to 10 and Comparative Examples 1 to 6 were used as positive electrode materials to prepare positive electrode plates, respectively. At the same time, metallic sodium was used as a negative electrode plate, glass fiber was used as a separator, 1M NaPF6 propylene carbonate (PC) / ethyl methyl carbonate (EMC) solution was used as an electrolyte, and 4% by weight of fluorinated ethylene carbonate (FEC) was added to the electrolyte. Button cells were assembled and charge and discharge tests were carried out at room temperature. The cycle test conditions were: first, charge and discharge cycles were performed 3 times at a current density of 13 mA / g (0.1C) and a voltage range of 1.7 to 4.3 V, and the capacity was evaluated at 0.1C. Then, charge and discharge cycles were performed 500 times under 1C conditions, and the cycle stability of the doped polyanion material was evaluated by the capacity retention rate after 500 charge and discharge cycles. The rate test conditions are: first cycle 3 times at 0.1C and 1.7-4.3V, cycle 5 times at 1C, and then cycle 5 times at 10C. The rate performance of the doped polyanion material is evaluated by the discharge capacity retention rate under 10C and 1C conditions. The test results are shown in Table 1 and Figure 2 shown.
[0129] Capacity retention rate after 500 charge and discharge cycles at 1C (%) = 500th discharge capacity / 1st discharge capacity × 100%;
[0130] 10C / 1C discharge capacity retention rate (%) = discharge capacity at 10C / discharge capacity at 1C×100%.
[0131] Table 1 Performance of doped polyanion materials in various embodiments and comparative examples
[0132]
[0133] It can be seen from the test results in Table 1 that the sodium ion battery assembled by using the doped polyanion material in Examples 1 to 10 as the positive electrode material to prepare the positive electrode sheet has a capacity of more than 110 mAh / g under the conditions of voltage of 1.7 to 4.3 V and 0.1C; and the capacity retention rate after 500 charge and discharge cycles under 1C conditions is ≥90%, and the 10C / 1C discharge capacity retention rate is ≥80%, indicating that the doped polyanion material of the present invention has high capacity, excellent cycle stability and good rate performance.
[0134] It can be found from Comparative Example 1 that, compared with the undoped modified polyanion material, doping with monovalent positive ions at the Fe position can significantly increase the capacity of the polyanion material while improving its cycle stability and rate performance. Moreover, according to Comparative Examples 4 to 5, it can be found that only by doping with monovalent positive ions at the Fe position can high capacity, excellent cycle stability and good rate performance be achieved, and doping with divalent positive ions or trivalent positive ions at the Fe position cannot achieve the above effects. The reason is that: compared with undoped, divalent or trivalent positive ion doping, monovalent positive ion doping can increase the concentration of interstitial sodium ions, thereby improving the capacity, rate performance and cycle stability of the polyanion material. At the same time, through Comparative Examples 2 and 3, it can also be found that although monovalent positive ion doping is beneficial to the improvement of rate performance and cycle stability, it will also lead to a decrease in capacity. When the doping amount of monovalent positive ions is too much or too little, it is not conducive to obtaining a polyanion material with high capacity, excellent cycle stability and good rate performance. In addition, by Figure 2 It can be seen from the charge and discharge curves that the discharge specific capacity of the doped polyanion material in Example 1 reaches 117.4 mAh / g under the conditions of a voltage range of 1.7 to 4.3 V and a current density of 13 mA / g (0.1C), and the charge and discharge curve is smooth, indicating that it not only has a high capacity but also has excellent cycle stability.
[0135] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A doped polyanion material, characterized in that: The chemical formula of the doped polyanion material is Na 4+x M x Fe 3-x (PO4)2P2O7; wherein M is a monovalent positive ion and its doping position is Fe, 0.03≤x≤0.
3.
2. The doped polyanion material according to claim 1, characterized in that: The M is Li + , K + , Rb + , Cs + , Cu + 、Ag + or NH4 + One or more of the .
3. The doped polyanion material according to claim 2, characterized in that: The M is Li + , K + , Rb + , Cs + , Cu + 、Ag + or NH4 + At least two of the .
4. The doped polyanion material according to claim 3, characterized in that: The M is Li + , K + , Rb + , Cs + , Cu + 、Ag + or NH4 + At least two of which one is Li + .
5. The doped polyanion material according to claim 1, characterized in that: The doped polyanion material has an orthorhombic crystal structure.
6. The doped polyanion material according to claim 5, characterized in that: The M element and the O element in the doped polyanion material are in octahedral coordination.
7. A method for preparing the doped polyanion material according to any one of claims 1 to 6, characterized in that: The following steps are involved: The pre-sintered product is first sintered at 250-400° C. in an inert atmosphere for 2-8 hours; and then calcined at 450-600° C. in an inert atmosphere for 5-15 hours to obtain a doped polyanion material; The pre-sintered product is prepared from a phosphorus source, a sodium source, an iron source, a carbon source and an M source by a sol-gel method, a spray drying method or a direct solid phase reaction method.
8. Use of the doped polyanion material according to any one of claims 1 to 6 in a positive electrode sheet or a sodium ion battery.
9. A positive electrode sheet, comprising a current collector and a positive electrode active material layer disposed on at least one side of the current collector, characterized in that: The positive electrode active material layer comprises the doped polyanion material according to any one of claims 1 to 6.
10. A sodium ion battery, comprising a positive electrode sheet, a negative electrode sheet, and an electrolyte located between the positive electrode sheet and the negative electrode sheet, characterized in that: The positive electrode plate comprises the doped polyanion material according to any one of claims 1 to 6.
Citation Information
Cited By
Low-band-gap ferric sodium pyrophosphate positive electrode material as well as preparation method and application thereof
CN121376950A