Solid electrolyte material, preparation method and application thereof, positive plate, solid electrolyte diaphragm and lithium ion battery
By coating the surface of the oxide solid electrolyte with a conductive polymer, the problem that nanoparticle oxide solid electrolytes cannot exert their ionic conductivity is solved, thereby reducing the battery's internal resistance and improving its cycle stability.
Patent Information
- Application Number
- CN202410934389.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-08
AI Technical Summary
The oxide solid electrolyte with nano-sized powder particles cannot exert the expected ionic conductivity in semi-solid batteries, resulting in increased internal resistance when the amount added is high, which affects battery performance.
The oxide solid electrolyte is modified by coating it with a conductive polymer to form a structure in which the core is an oxide solid electrolyte and the shell is a conductive polymer. The conductive polymer is coated on the surface of the oxide solid electrolyte by a preparation method.
It significantly improves the conductivity of electrolyte powder, reduces electrode resistivity, enhances electrochemical reaction kinetics, reduces battery internal resistance, and strengthens battery cycle stability.
Smart Images

Figure BDA0004940845490000061 
Figure BDA0004940845490000071 
Figure BDA0004940845490000072
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of batteries, and specifically relates to a solid electrolyte material and a preparation method, application, a positive electrode sheet, a solid electrolyte diaphragm and a lithium ion battery. Background Art
[0002] Semi-solid batteries have both high safety and high energy density, are compatible with existing traditional battery production lines, and have been used in the power market and energy storage field in small batches in recent years. Oxide solid electrolytes, as key materials in semi-solid batteries, have the advantages of good chemical and thermal stability, high ion migration number, and a wide electrochemical stability window. They are also environmentally friendly and non-toxic, and are low-cost and suitable for large-scale production.
[0003] In semi-solid batteries, oxide solid electrolytes are often used as electrode slurry additives and diaphragm coatings. Their introduction can not only delay the release of oxygen from the positive electrode and the heat generation reaction between the electrode interface and the electrolyte, and improve the thermodynamic stability of the diaphragm, but also produce spontaneous lithium ion exchange between the solid electrolyte and the lean electrolyte to enhance the continuity of the lithium ion transmission route in the semi-solid battery, ensure the lithium ion transmission and transfer kinetics, and enable the semi-solid battery to have a good cycle life. However, the oxide solid electrolytes in the electrode slurry additives and diaphragm coatings are in the form of nano-sized powder particles, which cannot exert their due ionic conductivity, resulting in an increase in the internal resistance of the battery when the addition amount is high, which has a negative impact on the battery performance. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a solid electrolyte material and a preparation method, application, positive electrode sheet, solid electrolyte membrane and lithium ion battery.
[0005] To achieve the above object, the technical solution adopted by the present invention is:
[0006] A solid electrolyte material comprises a core and a shell covering the core, wherein the core is an oxide solid electrolyte and the shell is a conductive polymer.
[0007] The oxide solid electrolyte includes one or a mixture of garnet-type solid electrolyte, NASICON-type solid electrolyte and perovskite-type solid electrolyte.
[0008] The conductive polymer includes one or a mixture of polypyrrole, polyaniline and polythiophene.
[0009] The coating amount of the shell is 0.01%-10%, preferably 2-3.5%.
[0010] The present invention also includes a method for preparing the solid electrolyte material, comprising the following steps: 1) preparing a mixed solution of protonic acid and dopant, adding oxide solid electrolyte and stirring; 2) adding conductive polymer monomer; 3) stirring and polymerizing the solution, and obtaining a conductive polymer-coated oxide solid electrolyte material after treatment, namely the solid electrolyte material.
[0011] The protonic acid includes one of acetic acid, hydrochloric acid, perchloric acid or camphorsulfonic acid or a mixture thereof; the concentration of the protonic acid in the conductive polymer reaction solution is 0.001-1 mol / L, preferably 0.005-0.3 mol / L.
[0012] Preferably, the dopant comprises ferric perchloride, sodium sulfate, manganese dioxide and ammonium persulfate; preferably, the concentration of the dopant in the conductive polymer reaction solution is 0.001 to 1 mol / L;
[0013] Preferably, the concentration of the conductive polymer monomer in the conductive polymer reaction solution is 0.001-1 mol / L, and the concentration of the conductive polymer monomer can be specifically adjusted according to the coating amount.
[0014] Steps 1)-3) are all carried out under ice bath conditions;
[0015] Preferably, the stirring time in step 1) is 5 to 30 minutes; preferably 10 minutes;
[0016] Preferably, the stirring polymerization time in step 3) is 10 to 300 min; preferably 240 min;
[0017] Preferably, the treatment process of step 3) is: filtering and washing the solution with deionized water, and then vacuum drying; preferably, the drying temperature is 20-50° C.; the time is 1-12 h, preferably 45° C., 8 h.
[0018] The present invention also includes an application of the solid electrolyte material as an electrode additive or a diaphragm coating.
[0019] The present invention also includes a positive electrode sheet, including an active material, the solid electrolyte material, a conductive agent, and a binder;
[0020] Preferably, the mass ratio of the active material, the solid electrolyte material, the conductive agent, and the binder is (90-96): (2-5): (1-3): (1-2);
[0021] Preferably, the active material is LiNi 0.8 Co 0.1 Mn 0.1 O2、LiNi 0.9 Co0.05 Mn 0.05 O2、LiNi 0.6 Co 0.1 Mn 0.3 O2;
[0022] Preferably, the conductive agent is Super P;
[0023] Preferably, the binder is PVDF.
[0024] The present invention also includes a solid electrolyte membrane, including a membrane and a solid electrolyte layer coated on the membrane; the solid electrolyte layer includes the solid electrolyte material and a binder; the binder is PVDF, and the mass ratio of the two is 3.5-5.5:1; preferably 4:1.
[0025] The present invention also includes a lithium ion battery, comprising the positive electrode sheet.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] The present invention uses a conductive polymer to coat and modify the oxide solid electrolyte, which can significantly improve the conductivity of the electrolyte powder, have both ionic conductivity and electronic conductivity, reduce the surface resistivity of the electrode sheet, improve the electrochemical reaction kinetics, and reduce the internal resistance of the battery. The battery assembled using the oxide solid electrolyte material coated with the conductive polymer provided by the present invention can have a smaller internal resistance and long cycle stability, which can improve the electrochemical performance of the battery. DETAILED DESCRIPTION
[0028] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with embodiments.
[0029] Example 1
[0030] 1. A method for preparing a solid electrolyte material, comprising the following steps:
[0031] 1) Prepare 200 ml of 0.3 mol / L HCl solution, add 13.5 g FeCl3·H2O and 3.22 g NASICON solid electrolyte Li 1.3 Al 0.3 Ti 1.7 (PO4)3; 2) stirring in an ice-water bath for 10 minutes, then adding 0.1 ml of pyrrole monomer; 3) then stirring the solution in an ice-water bath for 300 minutes to polymerize, filtering and washing the solution with deionized water until the filtrate is colorless, and vacuum drying at 40°C for 12 hours to obtain a conductive polymer-coated oxide solid electrolyte material Li 1.3 Al0.3 Ti 1.7 (PO4)3@ppy, the coating amount is 3wt.%.
[0032] Application of solid electrolyte materials, using Li 1.3 Al 0.3 Ti 1.7 (PO4)3@ppy as electrode additive.
[0033] 2. A method for preparing a positive electrode sheet, comprising the following steps:
[0034] Press LiNi 0.8 Co 0.1 Mn 0.1 O2: electrode additive: Super P: PVDF = 9.3:0.3:0.2:0.2 in a mass ratio to prepare the positive electrode slurry, apply it on the aluminum foil current collector, vacuum dry at 120°C for 24h, cut to get the positive electrode sheet, use lithium sheet as the negative electrode, Cellgard2400 as the separator, 1 mol / L LiPF6 / EC+DMC (volume ratio 1:1) mixed solution as the electrolyte, and assemble 2032 button batteries.
[0035] The constant current charge and discharge mode was used to perform charge and discharge tests at a current density of 200 mA / g and a voltage range of 2.5-4.25 V.
[0036] Example 2
[0037] 1. A method for preparing a solid electrolyte material, comprising the following steps:
[0038] 1) Prepare 50 ml of 0.3 mol / L HCl solution, add 0.082 g MnO2 and 2.5 g garnet solid electrolyte Li 6.4 Ln3Z 1.4 Ta 0.6 O 12 ; 2) After stirring in an ice-water bath for 20 minutes, 0.088 g of aniline was added; 3) The solution was then stirred in an ice-water bath for 360 minutes for polymerization, the solution was filtered and washed with deionized water, and vacuum dried at 50°C for 8 hours to obtain a conductive polymer-coated oxide solid electrolyte material Li 6.4 Ln3Z 1.4 Ta 0.6 O 12 @PANI, the coating amount is 3.5wt.%.
[0039] Application of solid electrolyte materials using Li 6.4 Ln3Z 1.4 Ta 0.6 O 12@PANI as electrode additive;
[0040] 2. A method for preparing a positive electrode sheet, comprising the following steps:
[0041] Press LiNi 0.8 Co 0.1 Mn 0.1 O2: electrode additive: Super P: PVDF = 9.3: 0.3: 0.2: 0.2 mass ratio mixed to make positive electrode slurry, coated on aluminum foil current collector, 120 ℃ vacuum drying for 24h, cut to get positive electrode sheet, lithium sheet as negative electrode, Cellgard2400 as separator, 1 mol / L LiPF6 / EC+DMC (volume ratio 1:1) mixed solution as electrolyte, assembled 2032 button cells. Use constant current charge and discharge mode, charge and discharge test at a current density of 200mA / g, voltage range of 2.5-4.25V.
[0042] Example 3
[0043] 1. A method for preparing a solid electrolyte material, comprising the following steps:
[0044] 1) Weigh 100 ml of deionized water, add 0.12 g of camphorsulfonic acid, 0.6 g of ammonium persulfate and 5 g of perovskite solid electrolyte Li 0.33 La 0.56 TiO3; 2) After stirring in an ice-water bath for 10 minutes, 0.12 mL of 3,4-ethylenedioxythiophene was added dropwise; 3) The solution was then stirred in an ice-water bath for 240 minutes for polymerization, and the solution was filtered and washed with deionized water, and vacuum dried at 45°C for 8 hours to obtain a conductive polymer-coated oxide solid electrolyte material Li 0.33 La 0.56 TiO3@PTh, coating amount is 2.4wt.%.
[0045] Application of solid electrolyte materials, using Li 0.33 La 0.56 TiO3@PTh as electrode additive;
[0046] 2. A method for preparing a positive electrode sheet, comprising the following steps:
[0047] Press LiNi 0.8 Co 0.1 Mn 0.1O2: electrode additive: Super P: PVDF = 9.3: 0.3: 0.2: 0.2 mass ratio mixed to make positive electrode slurry, coated on aluminum foil current collector, 120 ℃ vacuum drying for 24h, cut to get positive electrode sheet, lithium sheet as negative electrode, Cellgard2400 as separator, 1 mol / L LiPF6 / EC+DMC (volume ratio 1:1) mixed solution as electrolyte, assembled 2032 button cells. Use constant current charge and discharge mode, charge and discharge test at a current density of 200mA / g, voltage range of 2.5-4.25V.
[0048] Example 4
[0049] 1. A method for preparing a solid electrolyte material, comprising the following steps:
[0050] 1) Prepare 200 ml of 0.3 mol / L HCl solution, add 13.5 g FeCl3·H2O and 4.2 g garnet solid electrolyte Li 6.4 Ln3Z 1.4 Ta 0.6 O 12 ; 2) After stirring in an ice-water bath for 10 minutes, 0.1 ml of pyrrole monomer was added dropwise; 3) The solution was then stirred in an ice-water bath for 300 minutes for polymerization, and the solution was filtered and washed with deionized water until the filtrate was colorless, and vacuum dried at 40°C for 12 hours to obtain a conductive polymer-coated oxide solid electrolyte material Li 6.4 Ln3Z 1.4 Ta 0.6 O 12 @ppy, the coating amount is 2.4wt.%.
[0051] Application of solid electrolyte materials, using Li 6.4 Ln3Z 1.4 Ta 0.6 O 12 @ppy as an electrode additive.
[0052] 2. A method for preparing a positive electrode sheet, comprising the following steps:
[0053] Press LiNi 0.8 Co 0.1 Mn 0.1O2: electrode additive: Super P: PVDF = 9.3: 0.3: 0.2: 0.2 mass ratio mixed to make positive electrode slurry, coated on aluminum foil current collector, 120 ℃ vacuum drying for 24h, cut to get positive electrode sheet, lithium sheet as negative electrode, Cellgard2400 as separator, 1 mol / L LiPF6 / EC+DMC (volume ratio 1:1) mixed solution as electrolyte, assembled 2032 button cells. Use constant current charge and discharge mode, charge and discharge test at a current density of 200mA / g, voltage range of 2.5-4.25V.
[0054] Example 5
[0055] 1. A method for preparing a solid electrolyte material, comprising the following steps:
[0056] 1) Prepare 50 ml of 0.3 mol / L HCl solution, add 0.082 g MnO2 and 3 g perovskite solid electrolyte Li 0.33 La 0.56 TiO3; 2) stirring in an ice-water bath for 20 minutes, then adding 0.088 g of aniline; 3) then stirring the solution in an ice-water bath for 360 minutes to polymerize, filtering and washing the solution with deionized water, and vacuum drying at 50°C for 8 hours to obtain a conductive polymer-coated oxide solid electrolyte material Li 0.33 La 0.56 TiO3@PANI, coating amount is 3wt.%.
[0057] Application of solid electrolyte materials, using Li 0.33 La 0.56 TiO3@PANI as electrode additive.
[0058] 2. A method for preparing a positive electrode sheet, comprising the following steps:
[0059] Press LiNi 0.8 Co 0.1 Mn 0.1 O2: electrode additive: Super P: PVDF = 9.3: 0.3: 0.2: 0.2 mass ratio mixed to make positive electrode slurry, coated on aluminum foil current collector, 120 ℃ vacuum drying for 24h, cut to get positive electrode sheet, lithium sheet as negative electrode, Cellgard2400 as separator, 1 mol / L LiPF6 / EC+DMC (volume ratio 1:1) mixed solution as electrolyte, assembled 2032 button cells. Use constant current charge and discharge mode, charge and discharge test at a current density of 200mA / g, voltage range of 2.5-4.25V.
[0060] Example 6
[0061] 1. A method for preparing a solid electrolyte material, comprising the following steps:
[0062] 1) Weigh 100 ml of deionized water, add 0.12 g of camphorsulfonic acid, 0.6 g of ammonium persulfate and 6 g of NASICON solid electrolyte Li 1.3 Al 0.3 Ti 1.7 (PO4)3; 2) After stirring in an ice-water bath for 10 minutes, 0.12 mL of 3,4-ethylenedioxythiophene was added dropwise; 3) The solution was then stirred in an ice-water bath for 240 minutes for polymerization, and the solution was filtered and washed with deionized water, and vacuum dried at 45°C for 8 hours to obtain a conductive polymer-coated oxide solid electrolyte material Li 1.3 Al 0.3 Ti 1.7 (PO4)3@PTh, coating amount is 2wt.%.
[0063] Application of solid electrolyte materials, using Li 1.3 Al 0.3 Ti 1.7 (PO4)3@PTh as an electrode additive;
[0064] 2. A method for preparing a positive electrode sheet, comprising the following steps:
[0065] Press LiNi 0.8 Co 0.1 Mn 0.1 O2: electrode additive: Super P: PVDF = 9.3: 0.3: 0.2: 0.2 mass ratio mixed to make positive electrode slurry, coated on aluminum foil current collector, 120 ℃ vacuum drying for 24h, cut to get positive electrode sheet, lithium sheet as negative electrode, Cellgard2400 as separator, 1 mol / L LiPF6 / EC+DMC (volume ratio 1:1) mixed solution as electrolyte, assembled 2032 button cells. Use constant current charge and discharge mode, charge and discharge test at a current density of 200mA / g, voltage range of 2.5-4.25V.
[0066] Comparative Example 1
[0067] A method for preparing a positive electrode sheet comprises the following steps:
[0068] Using Li 1.3 Al 0.3 Ti 1.7 (PO4)3 as an electrode additive, according to LiNi 0.8 Co 0.1 Mn 0.1O2: electrode additive: Super P: PVDF = 9.3: 0.3: 0.2: 0.2 mass ratio mixed to make positive electrode slurry, coated on aluminum foil current collector, 120 ℃ vacuum drying for 24h, cut to get positive electrode sheet, lithium sheet as negative electrode, Cellgard2400 as separator, 1 mol / L LiPF6 / EC+DMC (volume ratio 1:1) mixed solution as electrolyte, assembled 2032 button cells. Use constant current charge and discharge mode, charge and discharge test at a current density of 200mA / g, voltage range of 2.5-4.25V.
[0069] Comparative Example 2
[0070] A method for preparing a positive electrode sheet comprises the following steps:
[0071] Using Li 6.4 Ln3Z 1.4 Ta 0.6 O 12 As an electrode additive, LiNi 0.8 Co 0.1 Mn 0.1 O2: electrode additive: Super P: PVDF = 9.3: 0.3: 0.2: 0.2 mass ratio mixed to make positive electrode slurry, coated on aluminum foil current collector, 120 ℃ vacuum drying for 24h, cut to get positive electrode sheet, lithium sheet as negative electrode, Cellgard2400 as separator, 1 mol / L LiPF6 / EC+DMC (volume ratio 1:1) mixed solution as electrolyte, assembled 2032 button cells. Use constant current charge and discharge mode, charge and discharge test at a current density of 200mA / g, voltage range of 2.5-4.25V.
[0072] Comparative Example 3
[0073] A method for preparing a positive electrode sheet comprises the following steps:
[0074] Using Li 0.33 La 0.56 TiO3 as an electrode additive, according to LiNi 0.8 Co 0.1 Mn 0.1O2: electrode additive: SuperP: PVDF = 9.3: 0.3: 0.2: 0.2 mass ratio mixed to make positive electrode slurry, coated on aluminum foil current collector, 120 ℃ vacuum drying for 24h, cut to get positive electrode sheet, lithium sheet as negative electrode, Cellgard2400 as separator, 1 mol / L LiPF6 / EC+DMC (volume ratio 1:1) mixed solution as electrolyte, assembled 2032 button cells. Use constant current charge and discharge mode, charge and discharge test at a current density of 200mA / g, voltage range of 2.5-4.25V.
[0075] Table 1 shows the surface resistivity of the electrodes of Comparative Examples 1 to 3 and Examples 1 to 6. The surface resistivity of the Examples is lower than that of the Comparative Examples, indicating that the conductive polymer coating modification can improve the conductivity of the solid electrolyte material.
[0076]
[0077]
[0078] Table 2 shows the impedance values of comparative examples 1 to 3 and embodiments 1 to 6. The impedance values of the embodiments are all lower than those of the comparative examples, indicating that the conductive polymer coating can reduce the internal resistance of the battery and promote interfacial charge transfer.
[0079]
[0080] Table 3 shows the capacity retention rates of comparative examples 1 to 3 and embodiments 1 to 6 after 300 cycles. The capacity retention rates of the embodiments are all higher than those of the comparative examples, indicating that the conductive polymer coating can enhance the conductivity of the oxide solid electrolyte, improve the electrochemical reaction kinetics, and help improve the battery cycle stability.
[0081]
[0082] The results show that 3,4-ethylenedioxythiophene as a conductive polymer, NASICON-type solid electrolyte Li 1.3 Al 0.3 Ti 1.7 (PO4)3 is the best oxide solid electrolyte, and the coating amount is 2-3.5%, which is the best. The coating amount is 2% (Example 6) for illustration.
[0083] Comparative Example 4
[0084] Diaphragm: 1g PVDF, 20g NMP solvent and 4g Li 1.3 Al 0.3 Ti 1.7The (PO4)3 powders were mixed evenly to prepare a mixed slurry, and then the slurry was evenly coated on the Cellgard2400 diaphragm and dried at 100°C for 12 hours to remove the solvent to obtain Li 1.3 Al 0.3 Ti 1.7 (PO4)3 coated modified Cellgard2400 membrane, coating thickness 2μm.
[0085] Battery: LiNi 0.8 Co 0.1 Mn 0.1 O2: Super P: PVDF = 9.6: 0.2: 0.2 mass ratio was mixed to make positive electrode slurry, coated on aluminum foil current collector, vacuum dried at 120℃ for 24h, cut to get positive electrode sheet, and use lithium sheet as negative electrode, Li 1.3 Al 0.3 Ti 1.7 (PO4)3 coated modified Cellgard2400 was used as the separator, 1 mol / L LiPF6 / EC+DMC (volume ratio 1:1) mixed solution was used as the electrolyte, and 2032 button cells were assembled. The constant current charge and discharge mode was used to perform charge and discharge tests at a current density of 200mA / g, with a voltage range of 2.5-4.25V.
[0086] Example 7
[0087] Diaphragm: 1g PVDF, 20g NMP solvent and 4g Li 1.3 Al 0.3 Ti 1.7 The (PO4)3@ppy (prepared in Example 1) powders were mixed evenly to prepare a mixed slurry, and then the slurry was evenly coated on the Cellgard2400 diaphragm and dried at 100°C for 12 hours to remove the solvent to obtain Li 1.3 Al 0.3 Ti 1.7 (PO4)3@ppy coated modified Cellgard2400 membrane with a coating thickness of 2μm.
[0088] Battery: LiNi 0.8 Co 0.1 Mn 0.1 O2: Super P: PVDF = 9.6: 0.2: 0.2 mass ratio was mixed to make positive electrode slurry, coated on aluminum foil current collector, vacuum dried at 120℃ for 24h, cut to get positive electrode sheet, and use lithium sheet as negative electrode, Li 1.3 Al 0.3 Ti 1.7(PO4)3@ppy coated modified Cellgard2400 was used as the separator, 1 mol / L LiPF6 / EC+DMC (volume ratio 1:1) mixed solution was used as the electrolyte, and 2032 button cells were assembled. The constant current charge and discharge mode was used to perform charge and discharge tests at a current density of 200 mA / g, with a voltage range of 2.5-4.25 V.
[0089] Table 4 shows the internal resistance values of the batteries of the comparative example and the embodiment. The internal resistance of the embodiment is lower than that of the comparative example, indicating that the conductivity of the conductive polymer-coated modified solid electrolyte coated diaphragm is higher.
[0090]
[0091] Similarly, other solid electrolyte materials, such as the solid electrolytes coated with conductive polymers provided in Examples 2-6, can change the conductivity of the diaphragm to varying degrees, among which Example 7 is used as an example to illustrate.
[0092] In summary, the present invention uses a conductive polymer to coat and modify the oxide solid electrolyte, which can significantly improve the conductivity of the electrolyte powder, have both ionic conductivity and electronic conductivity, reduce the surface resistivity of the electrode sheet, improve the electrochemical reaction kinetics, and reduce the internal resistance of the battery. The battery assembled using the oxide solid electrolyte material coated with the conductive polymer provided by the present invention can have a smaller internal resistance and long cycle stability, which can improve the electrochemical performance of the battery.
[0093] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A solid electrolyte material, characterized in that: It comprises a core and a shell covering the core, wherein the core is an oxide solid electrolyte and the shell is a conductive polymer.
2. The solid electrolyte material according to claim 1, characterized in that The oxide solid electrolyte includes one or a mixture of garnet-type solid electrolyte, NASICON-type solid electrolyte and perovskite-type solid electrolyte.
3. The solid electrolyte material according to claim 1, characterized in that The conductive polymer includes one or a mixture of polypyrrole, polyaniline and polythiophene.
4. The solid electrolyte material according to claim 1, characterized in that The coating amount of the shell is 0.01%-10%, preferably 2%-3.5%.
5. A method for preparing a solid electrolyte material according to any one of claims 1 to 4, characterized in that: The method comprises the following steps: 1) preparing a mixed solution of protonic acid and dopant, adding oxide solid electrolyte and stirring; 2) adding conductive polymer monomer; 3) stirring and polymerizing the solution, and obtaining a conductive polymer-coated oxide solid electrolyte material, which is a solid electrolyte material.
6. The preparation method according to claim 5, characterized in that: The proton acid includes one of acetic acid, hydrochloric acid, perchloric acid or camphorsulfonic acid or a mixture thereof; the concentration of the proton acid in the conductive polymer reaction solution is 0.001 to 1 mol / L; preferably camphorsulfonic acid, 1.2 g / L; Preferably, the dopant includes ferric perchloride, sodium sulfate, manganese dioxide and ammonium persulfate; preferably, the concentration of the dopant in the conductive polymer reaction solution is 0.001 to 1 mol / L; preferably, ammonium persulfate, 6 g / L; Preferably, the concentration of the conductive polymer monomer in the conductive polymer reaction solution is 0.001-1 mol / L, preferably 3,4-ethylenedioxythiophene, with a concentration of 1.2 ml / L. Preferably, steps 1) to 3) are all performed under ice bath conditions; Preferably, the stirring time in step 1) is 5 to 30 minutes; Preferably, the stirring polymerization time in step 3) is 10 to 300 min; Preferably, the treatment process of step 3) is: filtering and washing the solution with deionized water, and then vacuum drying; preferably, the drying temperature is 20 to 50° C. and the drying time is 1 to 12 hours.
7. Use of the solid electrolyte material according to any one of claims 1 to 8, characterized in that: Used as electrode additive or separator coating.
8. A solid electrolyte membrane, comprising a membrane and a solid electrolyte layer coated on the membrane; the solid electrolyte layer comprises the solid electrolyte material and a binder; the binder is PVDF, and the mass ratio of the two is 3.5-5.5:1; preferably 4:
1.
9. A positive electrode sheet, characterized in that: Comprising an active substance, the solid electrolyte material according to any one of claims 1 to 4, a conductive agent, and a binder; Preferably, the mass ratio of the active material, the solid electrolyte material, the conductive agent, and the binder is (90-96): (2-5): (1-3): (1-2); Preferably, the active material is LiNi 0.8 Co 0.1 Mn 0.1 O2、LiNi 0.9 Co 0.05 Mn 0.05 O2、LiNi 0.6 Co 0.1 Mn 0.3 O2; Preferably, the conductive agent is Super P; Preferably, the binder is PVDF.
10. A lithium ion battery, characterized in that: Including the positive electrode sheet as described in claim 9.
Citation Information
Cited By
Preparation method and application of solid electrolyte coated diaphragm
CN120237377A
Preparation method and application of solid electrolyte coated diaphragm
CN120237377B