Nitrogen and sulfur co-doped core-shell porous carbon electrocatalyst as well as preparation method and application thereof

By co-doping the core-shell porous carbon electrocatalyst, the oxygen reduction reaction activity of zinc air batteries is improved, and the problem of insufficient cathodic catalytic activity in zinc air batteries is solved, and a high energy density and stable operation of zinc air batteries is achieved. Simple process and low cost.

CN118919743AInactive Publication Date: 2024-11-08GUANGDONG UNIV OF TECH

Patent Information

Application Number
CN202411089998.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The complex cathode and slow kinetic oxygen reduction reaction and oxygen evolution reaction in zinc air batteries hinder their application. The existing precious metal catalysts have poor stability, scarcity and high cost problems, and it is necessary to develop structural engineering to improve catalytic activity and atomic utilization efficiency. Strategy.

Method used

The electrocatalyst using nitrogen and sulfur co-doped core-shell porous carbon is used to increase the specific surface area and surface functional groups of the catalyst through the synergistic effect of ZIF-8@ZIF-67 nanocrystals and trithiocyanuric acid, and utilize the synergistic effect of iron and cobalt , forming a Co@Fe-HNSC catalyst to enhance the oxygen reduction reaction activity.

Benefits of technology

The high energy density and stable operation of zinc air batteries were achieved. The catalyst showed a high half-wave potential and limit current density under 0.1M KOH conditions. The assembled zinc air batteries operated stably for more than 500 hours at 5mA/cm2, which was better than Based on Pt/C performance, simple process and low cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004986261170000011
    Figure HDA0004986261170000011
  • Figure HDA0004986261170000021
    Figure HDA0004986261170000021
  • Figure HDA0004986261170000031
    Figure HDA0004986261170000031
Patent Text Reader

Abstract

The invention belongs to the technical field of electrochemistry, and discloses a nitrogen and sulfur co-doped core-shell porous carbon electrocatalyst and a preparation method and application thereof. The preparation method comprises the following steps: based on a zeolite imidazate framework (ZIF-8) structure, putting the zeolite imidazate framework (ZIF-8) structure in a methanol solution of cobalt salt and 2-methylimidazole to coat ZIF-8 in situ so as to form a ZIF-8-ZIF-67 precursor with a core-shell structure; zIF-8-ZIF-67 is subjected to surface functionalization treatment by dipping ferric salt and trithiocyanuric acid, and then the ZIF-8-ZIF-67 is subjected to variable-speed heating pyrolysis carbonization in an inert gas atmosphere, so that the Fe and Co loaded dodecahedron oxygen reduction electrocatalyst with the hollow structure is prepared and has good dispersity, high atom utilization rate and large specific surface area; the excellent electrocatalytic activity is shown on the oxygen reduction reaction. And the assembled ZAB also shows excellent stability, and can stably operate for more than 500 hours under the condition of 5mA / cm < 2 >.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electrochemistry, and particularly relates to a nitrogen-sulfur co-doped core-shell porous carbon electrocatalyst and a preparation method and application thereof. Background Art

[0002] In order to meet the world's energy needs, and traditional energy is gradually being valued due to environmental pollution, renewable energy and electric vehicles are increasingly seen as solutions to the current environmental and energy crisis. In this context, the development of advanced energy storage equipment has become an indispensable compensation for intermittent renewable energy.

[0003] Zinc-air batteries (ZABs) have attracted widespread attention in recent years due to their high energy density, safety, availability, and low cost. Zinc-air batteries generate electricity through redox reactions between zinc and oxygen in the air. Due to the abundant oxygen supply in the atmosphere, they have a high theoretical energy density. Zinc-air batteries combine the advantages of lithium-ion batteries and fuel cells, especially in portable and flexible devices, providing an effective solution for future sustainable development and clean energy storage.

[0004] However, the complex and kinetically slow oxygen reduction reaction (ORR) and oxygen evolution reaction (OER) at the cathode in zinc-air batteries hinder their application. Usually, certain catalysts are required to improve the activity of ORR and OER. At present, Pt and RuO2 are regarded as the most classic cathode catalysts, but precious metal catalysts still have disadvantages such as poor stability, scarcity, and high price. Single-atom catalysts in cathode non-precious metal catalysts have great research potential and have attracted much attention. In addition to the coordinated environment of the single-atom center, the utilization efficiency of the active site has a profound impact on the overall performance. However, most M-N4 sites are buried in a dense carbon framework, which limits their contribution to the catalytic reaction. It is urgent to develop a simple and practical structural engineering strategy to improve the atom utilization efficiency and mass transfer to achieve the improvement of the catalytic activity of zinc-air batteries.

[0005] Surface heteroatom doping has been shown to be an effective strategy to increase the surface area for oxygen reduction reaction. In a typical synthesis process, the introduction of S species prevents Fe and Co atoms from agglomerating with themselves during high-temperature calcination, and a large amount of catalysts with FeCoN4 configuration can be synthesized on the surface of the electrocatalyst. In addition, compared with the S-free precursor catalyst, the addition of S atoms greatly increases the surface area exposure, resulting in higher catalytic activity. The rechargeable Zn-air battery integrated with this electrocatalyst shows relatively high performance in both discharge and charge processes, indicating enhanced activity for ORR and OER reactions. Summary of the invention

[0006] In order to overcome the above-mentioned shortcomings and deficiencies in the prior art, the primary purpose of the present invention is to provide a method for preparing a nitrogen-sulfur co-doped core-shell porous carbon electrocatalyst; this method directly increases the specific surface area and the number of surface functional groups of the catalyst, utilizes the synergistic effect of iron and cobalt, improves the atomic utilization of the catalyst, and thus improves the activity of the oxygen reduction reaction.

[0007] Another object of the present invention is to provide a nitrogen-sulfur co-doped core-shell porous carbon electrocatalyst prepared by the above preparation method.

[0008] Another object of the present invention is to provide an application of the above-mentioned nitrogen-sulfur co-doped core-shell porous carbon electrocatalyst, which can be assembled to obtain a zinc-air battery with higher energy density.

[0009] The purpose of the present invention can be achieved by the following technical solutions:

[0010] A method for preparing a nitrogen-sulfur co-doped core-shell porous carbon electrocatalyst, according to the following steps:

[0011] S1. Preparation of ZIF-8 nanocrystals:

[0012] Dissolve zinc nitrate and 2-methylimidazole (2-MeIM) in a methanol solution to form a zinc nitrate methanol solution and a 2-methylimidazole (2-MeIM) methanol solution; then, dropwise add the 2-methylimidazole (2-MeIM) methanol solution into the zinc nitrate methanol solution; after ultrasonic treatment for 10 minutes, stir for 1 hour, and then let the resulting mixed solution stand at room temperature overnight; centrifuge to separate the precipitate, wash the precipitate with a methanol solution several times, and then dry it in a vacuum oven at 60°C to obtain ZIF-8 nanocrystals;

[0013] S2. Preparation of ZIF-8@ZIF-67 nanocrystals:

[0014] Weigh 150 mg of the ZIF-8 nanocrystals obtained in step S1 and disperse them in 40 ml of a methanol solution, and perform ultrasonic treatment for 20 min to obtain a methanol solution of ZIF-8 nanoparticles; dropwise add methanol solutions containing cobalt salt and 2-methylimidazole (2-MeIM) to the methanol solution of ZIF-8 nanoparticles; stir at room temperature, centrifuge to separate the precipitate, wash the precipitate with a methanol solution, and then dry it in a vacuum oven at 60° C. to obtain ZIF-8@ZIF-67 nanocrystals;

[0015] Preparation of S3 and Co@Fe-HNSC catalysts

[0016] Weigh 150 mg of the ZIF-8@ZIF-67 nanocrystals obtained in step S2 and disperse them in 40 ml of methanol solution. Ultrasonicate for 20 min, add an iron source, immerse, add trithiocyanuric acid, stir, centrifuge, dry, place in a tubular furnace porcelain boat, heat from 20-30 ° C to 800-950 ° C under an inert gas atmosphere, anneal and carbonize to obtain a Co@Fe-HNSC catalyst, which is a nitrogen-sulfur co-doped core-shell porous carbon electrocatalyst.

[0017] The molar ratio of zinc nitrate to 2-methylimidazole in step S1 is 1:4-1:12.

[0018] The particle size of the ZIF-8 nanocrystals in step S1 is 150-200 nm.

[0019] In step S2, the cobalt salt is one or more of cobalt nitrate, cobalt chloride, cobalt sulfate, and cobalt acetate; and the stirring time is 10 min-60 min.

[0020] In step S3, the iron source is ferric nitrate nonahydrate; and the inert gas is one or both of nitrogen and argon.

[0021] In step S3, the immersion time is 10 min-20 min; the stirring time is 10 min-60 min; and the heating is carried out at a heating rate of 2-10°C.

[0022] A nitrogen-sulfur co-doped core-shell porous carbon electrocatalyst prepared by the above preparation method. The electrocatalyst has a carbon content of 0.191 mg / cm 2 The load capacity, half-wave potential is 0.88, and the limiting current density is 6.02 mA / cm 2 .

[0023] The above-mentioned nitrogen-sulfur co-doped core-shell porous carbon electrocatalyst can be applied to zinc-air batteries. The zinc-air battery assembled with the electrocatalyst is subjected to a high current density of 5 mA / cm 2 Stable operation for more than 500h.

[0024] ORR half-cell test:

[0025] The rotating disk electrode was used as the working electrode with a loading of 0.191 mg / cm 2 The ORR performance of the catalyst was tested. The entire test was conducted under 0.1M KOH electrolyte conditions. Before the test, high-purity O2 was continuously introduced into the electrolyte to obtain a gas-saturated electrolyte, and the aeration state was maintained during the test to maintain gas saturation in the electrolyte.

[0026] Preparation and testing of rechargeable zinc-air battery catalyst layers:

[0027] The 60-mesh stainless steel mesh and the waterproof breathable membrane were rolled and meshed, and cut into 2x8cm specifications for later use. The catalyst ink prepared above was applied to the surface of the stainless steel mesh in small amounts and multiple times using a pipette gun, and then dried under an infrared lamp to obtain a catalyst loading of 1 mg / cm 2 As a control, 20% Pt / C catalyst was used to prepare catalyst ink and air cathode catalyst layer in the same way. Polished zinc foil was used as anode, and a mixed solution of 0.2M zinc acetate and 6M KOH was used as electrolyte to assemble a rechargeable zinc-air battery. The battery polarization curve and constant current curve were recorded using CHI 760E and battery test system (LAND CT3001A1U), respectively.

[0028] Beneficial effects of the present invention:

[0029] (1) The electrocatalyst prepared by the present invention is doped with N and S by trithiocyanuric acid. The lower electronegativity of the heteroatom is expected to improve the d band delocalization, regulate the delocalization of the catalyst, and regulate the electronic structure of Fe and Co atoms. After carbonization, a certain hollow structure is formed. Compared with the original ZIF-8@ZIF-67, Co@Fe-7-HNSC-900 has the largest specific surface area (797.316m2g-1), and the pore structure is concentrated at about 4nm, which can expose more redox reaction active sites.

[0030] (2) The electrocatalyst prepared by the present invention shows through the corresponding energy dispersion spectrum (EDS) that Co, Fe and other elements in the catalyst are uniformly distributed on the catalyst surface. The metal nanoparticles generated during carbonization catalytically derive a large number of carbon nanotubes, which contain two different carbon forms: porous carbon and carbon nanotubes, which enhance mass transfer / charge transfer. The carbon nanotubes and hollow structures provide more anchoring points for FeCo-HNSC, and the M-Nx active sites are exposed on the surface of the carbon-based material, thereby improving the utilization efficiency of the M-Nx active sites.

[0031] (3) The electrocatalyst prepared by the present invention has good electrochemical performance. Its O2 reduction performance in 0.1M KOH is: 2 The load capacity, half-wave potential is about 0.88V, and the limiting current density is 6.02mA / cm 2 .

[0032] (4) After the electrocatalyst prepared by the present invention is assembled into a zinc-air battery, the ZAB peak power density of the Co@Fe-7-HNSC-900 electrocatalyst reaches 169 mW / cm 2 , which is superior to the peak power density of 70 mW / cm based on Pt / C ZAB. 2The ZAB of Co@Fe-7-HNSC-900 electrocatalyst exhibits excellent stability and can 2 Stable operation for more than 500h.

[0033] (4) The equipment required by the present invention is simple, easy to operate, safe, and low in cost, which is conducive to large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is a scanning electron microscope image of a Co@Fe-7-HNSC-900 electrocatalyst prepared in Example 1.

[0035] Figure 2 This is the EDS element distribution diagram of a Co@Fe-7-HNSC-900 electrocatalyst prepared in Example 1.

[0036] Figure 3 is a scanning electron microscope image of a Co-HNC electrocatalyst prepared in Example 4.

[0037] Figure 4 This is a transmission electron micrograph of a Co@Fe-7-HNSC-900 electrocatalyst prepared in Example 1.

[0038] Figure 5 This is a transmission electron micrograph of a Co-HNC electrocatalyst prepared in Example 4.

[0039] Figure 6 It is the X-ray diffraction pattern of the electrocatalyst prepared in Examples 1 and 4 of the present invention.

[0040] Figure 7 It is the nitrogen adsorption-desorption isotherm diagram of the electrocatalyst prepared in Examples 1 and 4 of the present invention.

[0041] Figure 8 It is the pore size distribution diagram of the electrocatalyst prepared in Examples 1 and 4 of the present invention.

[0042] Fig. 9 Graph showing the oxygen reduction performance of the electrocatalysts prepared in Examples 1-4 of the present invention.

[0043] Fig.10 It is the power density of the zinc-air battery assembled with the Co@Fe-7-HNSC-900 electrocatalyst prepared in Example 1.

[0044] Fig.11 This is the GCD diagram of a zinc-air battery assembled with a Co@Fe-7-HNSC-900 electrocatalyst prepared in Example 1. DETAILED DESCRIPTION

[0045] The present invention is further described in detail below in conjunction with embodiments and drawings, but the embodiments of the present invention are not limited thereto.

[0046] Example 1

[0047] Step 1: Preparation of ZIF-8 nanocrystals

[0048] (1) First, according to the molar ratio of Zn(NO3)2·6H2O to 2-methylimidazole of 1:12, 1.19 g of Zn(NO3)2·6H2O and 4 g of 2-methylimidazole (2-MeIM) were weighed and dissolved in 100 ml of methanol solution to form a methanol solution of 2-methylimidazole (2-MeIM) and a methanol solution of Zn(NO3)2·6H2O, respectively. Subsequently, the methanol solution of 2-methylimidazole (2-MeIM) was added dropwise to the methanol solution of Zn(NO3)2·6H2O; after ultrasonic treatment for 10 min, the mixture was stirred for 1 h, and then the resulting mixed solution was allowed to stand at room temperature overnight; the precipitate was separated by centrifugation, washed with methanol solution several times, and then dried in a vacuum oven at 60°C to obtain ZIF-8 nanocrystals with a particle size of 200 nm.

[0049] Step 2: Preparation of ZIF-8@ZIF-67 nanocrystals

[0050] Weigh 150 mg of the ZIF-8 nanocrystals obtained in step 1 above and disperse them in 40 ml of methanol solution, and ultrasonicate for 20 min to obtain a methanol solution of ZIF-8 nanoparticles; add a methanol solution containing 0.175 g of Co(NO3)2·6H2O and 0.6 g of 2-methylimidazole (2-MeIM) dropwise into the methanol solution of ZIF-8 nanoparticles; stir at room temperature for 20 min, centrifuge and separate the precipitate, wash the precipitate with methanol solution 3 times, and then dry it in a vacuum oven at 60°C. Purple ZIF-8@ZIF-67 nanocrystals are obtained.

[0051] Step 3: Preparation of Co@Fe-7-HNSC-900 catalyst

[0052] Weigh 200 mg of the ZIF-8@ZIF-67 nanocrystals obtained in step 2 and disperse them in 40 ml of methanol solution. Ultrasonicate for 20 min, add 0.09 g of ferric nitrate nonahydrate, soak for 10 min, then add 7 mg of trithiocyanuric acid, stir for 20 min, centrifuge, dry, place in a porcelain boat in a tubular furnace, heat from 25 °C to 900 °C at a heating rate of 5 °C under argon atmosphere, anneal and carbonize to obtain the Co@Fe-7-HNSC-900 electrocatalyst.

[0053] Figure 1This is a scanning electron microscope image of the electrocatalyst prepared in this example;

[0054] Figure 2 This is the EDS element distribution diagram of the electrocatalyst prepared in this example;

[0055] Figure 4 This is a transmission electron microscopy image of the electrocatalyst prepared in this example.

[0056] The Co@Fe-7-HNSC-900 obtained in Example 1 was subjected to SEM scanning electron microscope test. Figure 1 As shown, there are a large number of carbon nanotubes, wherein the average particle size of the Co@Fe-7-HNSC-900 catalyst particles is 150-200 nm, and the average width of the carbon nanotubes is 10-30 nm.

[0057] The specific surface area and pore size distribution of the Co@Fe-7-HNSC-900 electrocatalyst prepared in Example 1 were obtained by using BET and DFT methods at 77K. Figure 7 As shown in Figure 8, all samples show type IV isotherms with H3 hysteresis loops, which indicates that the material has micropores and mesopores. From the test results of N2 adsorption and desorption, it can be seen that Co@Fe-7-HNSC-900 has a large specific surface area (797.316m 2 g -1 ), the pore structure is concentrated around 4 nm, which is conducive to the exposure and mass transfer of active sites.

[0058] The Co@Fe-7-HNSC-900 electrocatalyst prepared in Example 1 was subjected to an oxygen reduction test. Fig. 9 The Co@Fe-7-HNSC-900 electrocatalyst has good electrochemical performance. 2 The load capacity, half-wave potential is 0.88V, and the limiting current density is about 6.02mA / cm 2 , best performance;

[0059] After assembling into zinc-air battery, Fig.10 , 11 As shown in Figure 2, the ZAB peak power density of Co@Fe-7-HNSC-900 electrocatalyst reaches 169 mW / cm 2 , which is superior to the peak power density of 70 mW / cm based on Pt / C ZAB. 2 The ZAB of Co@Fe-7-HNSC-900 electrocatalyst exhibits excellent stability and can 2 Stable operation for more than 500h.

[0060] Example 2

[0061] The difference between this embodiment and embodiment 1 is that the molar amount of trithiocyanuric acid is reduced.

[0062] Step 1: Preparation of ZIF-8 nanocrystals

[0063] (1) First, according to the molar ratio of Zn(NO3)2·6H2O to 2-methylimidazole of 1:12, 1.19 g of Zn(NO3)2·6H2O and 4 g of 2-methylimidazole (2-MeIM) were weighed and dissolved in 100 ml of methanol solution to form a methanol solution of 2-methylimidazole (2-MeIM) and a methanol solution of Zn(NO3)2·6H2O, respectively. Subsequently, the methanol solution of 2-methylimidazole (2-MeIM) was added dropwise to the methanol solution of zinc nitrate; after ultrasonication for 10 min, the mixture was stirred for 1 h, and then allowed to stand at room temperature overnight; the precipitate was separated by centrifugation, washed several times with methanol solution, and then dried in a vacuum oven at 60°C to obtain ZIF-8 nanocrystals with a particle size of 200 nm.

[0064] Step 2: Preparation of ZIF-8@ZIF-67 nanocrystals

[0065] Weigh 150 mg of the ZIF-8 nanocrystals obtained in the above step 1 and disperse them in 40 ml of methanol solution, and ultrasonicate for 20 minutes; add methanol solutions containing 0.175 g of Co(NO3)2·6H2O and 0.6 g of 2-methylimidazole (2-MeIM) drop by drop into the methanol solution of ZIF-8 nanoparticles; after stirring at room temperature for 20 minutes, centrifuge and separate the precipitate, wash it three times with methanol solution, and then dry it in a vacuum oven at 60°C to obtain purple ZIF-8@ZIF-67 nanocrystals.

[0066] Step 3: Preparation of Co@Fe-2-HNSC-900 catalyst

[0067] Weigh 200 mg of the ZIF-8@ZIF-67 nanocrystals obtained in step 2 and disperse them in 40 ml of methanol solution. Ultrasonicate for 20 min, add 0.09 g of ferric nitrate nonahydrate, soak for 10 min, then add 2 mg of trithiocyanuric acid, stir for 20 min, centrifuge, dry, place in a tubular furnace porcelain boat, heat from 25 ° C to 900 ° C at a heating rate of 5 ° C in an argon atmosphere, anneal and carbonize to obtain the Co@Fe-2-HNSC-900 electrocatalyst.

[0068] The Co@Fe-2-HNSC-900 electrocatalyst prepared in Example 2 was subjected to an oxygen reduction test. Fig. 9As shown, under 0.1M KOH alkaline conditions, at 0.191 mg / cm 2 The load capacity, half-wave potential is about 0.85V, and the limiting current density is about 5.4mA / cm 2 .

[0069] Example 3

[0070] The difference between this embodiment and embodiment 1 is that the molar amount of trithiocyanuric acid is increased.

[0071] Step 1: Preparation of ZIF-8 nanocrystals

[0072] (1) First, according to the molar ratio of Zn(NO3)2·6H2O to 2-methylimidazole of 1:12, 1.19g of Zn(NO3)2·6H2O and 4g of 2-methylimidazole (2-MeIM) were weighed and dissolved in 100ml of methanol solution to form 2-methylimidazole (2-MeIM) methanol solution and Zn(NO3)2·6H2O methanol solution respectively; then, the 2-methylimidazole (2-MeIM) methanol solution was added dropwise to the zinc nitrate methanol solution; after ultrasonication for 10min, the mixture was stirred for 1h, and then allowed to stand at room temperature overnight; the precipitate was separated by centrifugation, washed with methanol solution several times, and then dried in a vacuum oven at 60℃. ZIF-8 nanocrystals with a particle size of 200nm were obtained.

[0073] Step 2: Preparation of ZIF-8@ZIF-67 nanocrystals

[0074] Weigh 150 mg of the ZIF-8 nanocrystals obtained in step 1 and disperse them in 40 ml of methanol solution, and ultrasonicate for 20 min; add methanol solutions containing 0.175 g of Co(NO3)2·6H2O and 0.6 g of 2-methylimidazole (2-MeIM) dropwise into the methanol solution of ZIF-8 nanoparticles; after stirring at room temperature for 20 min, centrifuge and separate the precipitate, wash it 3 times with methanol solution, and then dry it in a vacuum oven at 60°C to obtain purple ZIF-8@ZIF-67 nanocrystals.

[0075] Step 3: Preparation of Co@Fe-12-HNSC-900 catalyst

[0076] Weigh 200 mg of the ZIF-8@ZIF-67 nanocrystals obtained in step 2 and disperse them in 40 ml of methanol solution. Ultrasonicate for 20 min, add 0.09 g of ferric nitrate nonahydrate, soak for 10 min, then add 12 mg of trithiocyanuric acid, stir for 20 min, centrifuge, dry, place in a tubular furnace porcelain boat, heat from 25 ° C to 900 ° C at a heating rate of 5 ° C in an argon atmosphere, anneal and carbonize to obtain the Co@Fe-12-HNSC-900 electrocatalyst.

[0077] The Co@Fe-12-HNSC-900 electrocatalyst prepared in Example 3 was subjected to an oxygen reduction test. Fig. 9 As shown, under 0.1M KOH alkaline conditions, at 0.191 mg / cm 2 The load capacity, half-wave potential is about 0.86V, and the limiting current density is about 5.6mA / cm 2 .

[0078] Example 4

[0079] The difference between this embodiment and embodiment 1 is that trithiocyanuric acid and iron source are not added.

[0080] Step 1: Preparation of ZIF-8 nanocrystals

[0081] (1) First, according to the molar ratio of Zn(NO3)2·6H2O to 2-methylimidazole of 1:12, 1.19 g of Zn(NO3)2·6H2O and 4 g of 2-methylimidazole (2-MeIM) were weighed and dissolved in 100 ml of methanol solution to form a methanol solution of 2-methylimidazole (2-MeIM) and a methanol solution of Zn(NO3)2·6H2O, respectively; then, the methanol solution of 2-methylimidazole (2-MeIM) was added dropwise to the methanol solution of zinc nitrate; after ultrasonic treatment for 10 min, the mixture was stirred for 1 h, and then allowed to stand at room temperature overnight; the precipitate was separated by centrifugation, washed with methanol solution several times, and then dried in a vacuum oven at 60°C to obtain ZIF-8 nanocrystals with a particle size of 200 nm. .

[0082] Step 2: Preparation of Co-HNC

[0083] Weigh 150 mg of the ZIF-8 nanocrystals obtained in step 1 and disperse them in 40 ml of methanol solution, and ultrasonicate for 20 minutes; add methanol solutions containing 0.175 g of Co(NO3)2·6H2O and 0.6 g of 2-methylimidazole (2-MeIM) drop by drop into the methanol solution of ZIF-8 nanoparticles; after stirring at room temperature for 20 minutes, centrifuge and separate the precipitate, wash it three times with methanol solution, and then dry it in a vacuum oven at 60°C to obtain purple ZIF-8@ZIF-67 nanocrystals; then place the ZIF-8@ZIF-67 nanocrystals in a tubular furnace porcelain boat, heat it from 25°C to 900°C at a heating rate of 5°C under argon atmosphere, and anneal and carbonize to obtain the Co-HNC electrocatalyst.

[0084] like Figure 3 , 5 As shown, its morphology and structure are somewhat different from those of Example 1, and no carbon nanotubes are generated. Figure 6 It is the X-ray diffraction pattern of the electrocatalyst prepared in Examples 1 and 4. It can be clearly seen that the catalyst obtained in Example 1 after pyrolysis contains not only a small amount of metal cobalt nanoparticles, but also peaks of FeS and Co9S8, while Example 4 only has the characteristic peaks of metal cobalt nanoparticles.

[0085] The Co-HNC electrocatalyst prepared in Example 4 was subjected to an oxygen reduction test. Fig. 9 As shown in the figure, under 0.1M KOH alkaline conditions, the 2 The load capacity, half-wave potential is about 0.85V, and the limiting current density is about 5.1mA / cm 2 .

[0086] The above embodiments are relatively suitable implementation modes of the present invention. The implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations and simplifications made without departing from the spirit and principle of the present invention shall be equivalent replacement modes and shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a nitrogen-sulfur co-doped core-shell porous carbon electrocatalyst, characterized in that Follow these steps: S1. Preparation of ZIF-8 nanocrystals: Dissolve zinc nitrate and 2-methylimidazole in a methanol solution to form a zinc nitrate methanol solution and a 2-methylimidazole methanol solution; then, dropwise add the 2-methylimidazole methanol solution to the zinc nitrate methanol solution; after ultrasonic treatment for 10 minutes, stir for 1 hour, and then let the resulting mixed solution stand at room temperature overnight; centrifuge to separate the precipitate, wash the precipitate with a methanol solution several times, and then dry it in a vacuum oven at 60°C to obtain ZIF-8 nanocrystals; S2. Preparation of ZIF-8@ZIF-67 nanocrystals: Weigh 150 mg of the ZIF-8 nanocrystals obtained in step S1 and disperse them in 40 ml of a methanol solution, and perform ultrasonic treatment for 20 min to obtain a methanol solution of ZIF-8 nanoparticles; dropwise add methanol solutions containing cobalt salt and 2-methylimidazole to the methanol solution of ZIF-8 nanoparticles; stir at room temperature, centrifuge to separate the precipitate, wash the precipitate with a methanol solution, and then dry it in a vacuum oven at 60° C. to obtain ZIF-8@ZIF-67 nanocrystals; Preparation of S3 and Co@Fe-HNSC catalysts Weigh 150 mg of the ZIF-8@ZIF-67 nanocrystals obtained in step S2 and disperse them in 40 ml of methanol solution. Ultrasonicate for 20 min, add an iron source, immerse, add trithiocyanuric acid, stir, centrifuge, dry, place in a tubular furnace porcelain boat, heat from 20-30 ° C to 800-950 ° C under an inert gas atmosphere, anneal and carbonize to obtain a Co@Fe-HNSC catalyst, which is a nitrogen-sulfur co-doped core-shell porous carbon electrocatalyst.

2. The method for preparing a nitrogen-sulfur co-doped core-shell porous carbon electrocatalyst according to claim 1, characterized in that: The molar ratio of zinc nitrate to 2-methylimidazole in step S1 is 1:4-1:

12.

3. The method for preparing a nitrogen-sulfur co-doped core-shell porous carbon electrocatalyst according to claim 1, characterized in that: The particle size of the ZIF-8 nanocrystals in step S1 is 150-200 nm.

4. The method for preparing a nitrogen-sulfur co-doped core-shell porous carbon electrocatalyst according to claim 1, characterized in that: In step S2, the cobalt salt is one or more of cobalt nitrate, cobalt chloride, cobalt sulfate, and cobalt acetate; and the stirring time is 10 min-60 min.

5. The method for preparing a hollow core-shell electrocatalyst according to claim 1, characterized in that: In step S3, the iron source is ferric nitrate nonahydrate; and the inert gas is one or both of nitrogen and argon.

6. The method for preparing a hollow core-shell electrocatalyst according to claim 1, characterized in that: In step S3, the immersion time is 10 min-20 min; the stirring time is 10 min-60 min; and the heating is carried out at a heating rate of 2-10°C.

7. A nitrogen-sulfur co-doped core-shell porous carbon electrocatalyst prepared by the preparation method according to any one of claims 1 to 6.

8. The nitrogen-sulfur co-doped core-shell porous carbon electrocatalyst according to claim 7, characterized in that: The electrocatalyst has a conductivity of 0.191 mg / cm under 0.1 M KOH alkaline conditions. 2 The load capacity, half-wave potential is 0.88, and the limiting current density is 6.02 mA / cm 2 .

9. The use of the nitrogen-sulfur co-doped core-shell porous carbon electrocatalyst according to claim 7 in a zinc-air battery, characterized in that: The zinc-air battery assembled with the electrocatalyst was heated at 5 mA / cm 2 Stable operation for more than 500h.

Citation Information

Patent Citations

  • Double-shell hollow porous nitrogen-rich carbon material, preparation method and application thereof

    CN110289425A

  • Electrocatalytic oxygen evolution catalyst and preparation method thereof

    CN113403638A

  • Preparation method and application of Fe and Co bimetallic monatomic oxygen reduction catalyst

    CN115566206A

  • Fuel cell electro-catalytic material and preparation method and application thereof

    CN116130673A

  • Iron-cobalt diatomic catalyst applied to oxygen reduction reaction as well as preparation method and application of iron-cobalt diatomic catalyst

    CN116826085A

Cited By

  • Sulfur-doped iron Fe-S-N-C cathode oxygen reduction catalyst as well as preparation method and application thereof

    CN119581581A

  • Preparation method and application of MOF (Metal Organic Framework) derived carbon catalyst for regulating and controlling oxygen reduction catalytic performance based on surface strain