Composite proton exchange membrane and preparation method thereof
By using a double-layer perfluorosulfonic acid resin structure in the proton exchange membrane, combining surfactant and solvent, the delamination and peeling of the porous polytetrafluoroethylene reinforcement layer under the wet and dry cycles is solved, and high conductivity and The balance of low swelling performance extends the service life of fuel cells.
Patent Information
- Application Number
- CN202411193185.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-08
AI Technical Summary
The existing porous polytetrafluoroethylene-reinforced perfluorosulfonic acid proton exchange membrane is delaminated and peeled from the reinforcement layer under dry and wet cycle conditions, resulting in a decrease in electrochemical and mechanical properties, making it difficult to ensure high conductivity and low swelling properties at the same time.
The first layer is formed by a first perfluorosulfonic acid resin with a smaller equivalent weight, and the porous polytetrafluoroethylene film is fully immersed and filled, and a second perfluorosulfonic acid resin layer with a larger equivalent weight is used on the outside of it to pass surface activity. The combination of the agent and the solvent forms a bilayer structure to improve the filling degree and deformation resistance.
The high conductivity, high strength and low swelling properties of the composite proton exchange membrane are achieved, which extends the service life of the fuel cell and simplifies the preparation process, making it convenient for industrial applications.
Smart Images

Figure CN118919753A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fuel cells, and in particular relates to a composite proton exchange membrane and a preparation method thereof. Background Art
[0002] Proton exchange membrane fuel cells have the advantages of high power density, high energy conversion efficiency, low operating temperature, clean and environmentally friendly, and have become one of the mainstream fuel cell technologies in the world. As the core key component of fuel cells, proton exchange membranes play the role of transmitting protons, separating reaction gases, and electronic insulation in the battery. The performance of proton exchange membranes directly affects the performance and service life of fuel cells.
[0003] At present, commercial proton exchange membranes all use expanded polytetrafluoroethylene (ePTFE) porous membrane composite reinforcement technology to reduce the membrane thickness while ensuring good mechanical strength of the proton membrane, improving the durability and mechanical stability of the proton membrane. However, since the introduced reinforcing material ePTFE is a non-proton conductor, the proton conductivity of the composite proton exchange membrane is reduced to a certain extent. At the same time, due to the incompatibility of the hydrophilic perfluorosulfonic acid resin and the extremely hydrophobic ePTFE support layer and the repeated expansion / contraction of the resin in the composite proton exchange membrane under wet / dry conditions, the volume changes, resulting in cracks, stratification and even peeling at the interface, which in turn causes the performance of the fuel cell to deteriorate.
[0004] Therefore, for ultra-thin proton exchange membranes reinforced with porous ePTFE, it is still an important challenge to ensure the high mechanical strength and low gas permeability of the proton exchange membrane while improving the compatibility between the resin and the reinforcement layer, reducing the swelling and shrinkage of the resin under repeated dry-wet cycles, improving the proton conductivity of the composite proton exchange membrane, and avoiding interface defects of the composite proton exchange membrane under complex working conditions. Summary of the invention
[0005] The present invention is based on the inventor's discovery and understanding of the following facts and problems:
[0006] The prior art often uses a method of modifying the reinforcing layer to improve the hydrophilicity of the reinforcing layer, such as obtaining a hydrophilic coating on the surface of the reinforcing layer by reacting tannic acid with 3-(aminopropyl)triethoxysilane, hydrophilizing polytetrafluoroethylene membrane (PTFE) with polydopamine, or plasma treating the surface of polytetrafluoroethylene nanofiber membrane. Although such methods can improve the compatibility between the resin and the porous reinforcing material, they will cause certain damage to the structure of the porous reinforcing material during the treatment process, resulting in changes in the pore size and porosity of the porous reinforcing material, thereby reducing the air permeability and strength of the material.
[0007] In addition, CN113861502A discloses a method for preparing a porous skeleton for a proton exchange membrane and a composite proton exchange membrane, wherein the porous skeleton is a porous polytetrafluoroethylene coated with polyimide obtained by impregnating and stretching a porous polytetrafluoroethylene sheet with polyamic acid, which has excellent dimensional stability, enhances the hydrophilicity of the porous skeleton, and improves the compatibility of the porous skeleton material with the proton exchange membrane resin. CN116053545A discloses a method for preparing a composite proton exchange membrane reinforced with polytetrafluoroethylene, comprising soaking a washed and soaked polytetrafluoroethylene membrane in a mixed solution in which polyvinyl chloride and polyvinyl pyrrolidone are dissolved, using polyvinyl pyrrolidone as a proton-conducting polymer in the proton exchange membrane, and polyvinyl chloride as a supporting material for the proton exchange membrane, and the two are blended and filled into the porous polytetrafluoroethylene membrane, and polyvinyl chloride and polyvinyl pyrrolidone can be fully filled into the polytetrafluoroethylene membrane to form a uniform composite membrane with excellent performance. In this type of method, the porous skeleton still has pores after hydrophilic treatment and cannot be filled with perfluorosulfonic acid resin, and the polyimide layer and polyvinyl chloride layer without proton transport ability occupy part of the pores of the porous skeleton, affecting the transmission of protons between the anode and cathode in the fuel cell, resulting in a decrease in the performance of the fuel cell prepared by the proton exchange membrane.
[0008] At present, the preparation technology of perfluorosulfonic acid proton exchange membrane reinforced with porous polytetrafluoroethylene is mostly focused on the study of hydrophilic modification of the reinforcing layer ePTFE, and the resin filling degree and proton conductivity are improved by improving the compatibility between the resin and the reinforcing layer. However, for the perfluorosulfonic acid proton exchange membrane reinforced with porous polytetrafluoroethylene, although the resin can be well filled in the pores of the reinforcing layer during the preparation process, the proton exchange membrane has higher conductivity and strength. However, the hydrophilic perfluorosulfonic acid resin in the composite proton exchange membrane will continue to shrink and swell under the repeated dry-wet cycle working conditions of the fuel cell, resulting in stratification and peeling of the resin and the reinforcing layer, which is manifested as large swelling of the composite proton exchange membrane on a macro scale, and the electrochemical and strength properties of the membrane are significantly reduced after repeated dry-wet cycles.
[0009] The present invention aims to solve one of the technical problems in the related art to at least a certain extent. To this end, the embodiment of the present invention proposes a composite proton exchange membrane, which ensures that the resin and the reinforcement layer are well filled, improves the swelling and shrinkage problem of the resin of the proton exchange membrane under long-term dry-wet cycle conditions, and has excellent proton conductivity and deformation resistance, thereby increasing the service life of the composite proton exchange membrane in the fuel cell.
[0010] The composite proton exchange membrane of the embodiment of the present invention comprises: a porous polytetrafluoroethylene membrane, a first perfluorosulfonic acid resin layer arranged on both sides of the porous polytetrafluoroethylene membrane, and a second perfluorosulfonic acid resin layer arranged on the side of the first perfluorosulfonic acid resin layer away from the porous polytetrafluoroethylene membrane; the equivalent weight of the first perfluorosulfonic acid resin is less than the equivalent weight of the second perfluorosulfonic acid resin.
[0011] Advantages and technical effects of the composite proton exchange membrane of the embodiment of the present invention:
[0012] (1) There is no need to modify the porous polytetrafluoroethylene membrane, thus avoiding damage to the structure of the porous polytetrafluoroethylene during the treatment process, thereby ensuring that the prepared composite proton exchange membrane has high permeability and strength;
[0013] (2) The composite proton exchange membrane provided by the embodiment of the present invention first uses a first perfluorosulfonic acid resin with a smaller equivalent weight to form a first perfluorosulfonic acid resin layer, thereby achieving sufficient infiltration and filling of the porous polytetrafluoroethylene membrane, so that the composite proton exchange membrane has a higher conductivity, and further uses a second perfluorosulfonic acid resin with a larger equivalent weight to form a second perfluorosulfonic acid resin layer, thereby solving the problem of delamination and peeling of the resin and the porous polytetrafluoroethylene membrane reinforcement layer caused by the continuous shrinkage and swelling of the composite proton exchange membrane under dry-wet cycle working conditions, and making the composite proton exchange membrane have a higher strength;
[0014] (3) The composite proton exchange membrane provided by the embodiment of the present invention solves the problem of swelling and shrinkage of the resin under long-term dry-wet cycle conditions while ensuring good filling of the perfluorosulfonic acid resin and the porous polytetrafluoroethylene reinforcement layer. This improves the dimensional stability of the composite proton exchange membrane as a whole and greatly improves the service life of the composite proton exchange membrane in the fuel cell.
[0015] In some embodiments, the equivalent weight of the first perfluorosulfonic acid resin is 300 to 900 g / mol; and / or the equivalent weight of the second perfluorosulfonic acid resin is 900 to 1500 g / mol.
[0016] In some embodiments, the thickness of the porous polytetrafluoroethylene membrane is 4 to 8 μm;
[0017] and / or, the thickness of the first perfluorosulfonic acid resin layer is 0.5 to 2.5 μm;
[0018] And / or, the second perfluorosulfonic acid resin layer has a thickness of 0.5 to 2.5 μm.
[0019] The present invention also provides a method for preparing a composite proton exchange membrane, which comprises the following steps:
[0020] (1) mixing a first perfluorosulfonic acid resin, a surfactant and a first solvent to obtain a first coating liquid, coating the first coating liquid on both sides of a porous polytetrafluoroethylene membrane, and drying to obtain a first perfluorosulfonic acid resin layer;
[0021] (2) A second perfluorosulfonic acid resin, a surfactant and a second solvent are mixed to obtain a second coating liquid, and the second coating liquid is applied to a side of the first perfluorosulfonic acid resin layer obtained in step (1) away from the porous polytetrafluoroethylene membrane, followed by drying to obtain a second perfluorosulfonic acid resin layer.
[0022] Advantages and technical effects of the method for preparing the composite proton exchange membrane according to the embodiment of the present invention:
[0023] (1) The method of the embodiment of the present invention does not introduce any material without proton conductivity, and while providing the composite proton exchange membrane with good dimensional stability, does not cause loss of the proton conductivity of the composite proton exchange membrane;
[0024] (2) The method of the embodiment of the present invention does not need to hydrophilically modify the surface of the porous polytetrafluoroethylene. By using a coating liquid containing a surfactant and a first perfluorosulfonic acid resin with a small equivalent weight and strong wetting ability, the resin and the porous polytetrafluoroethylene reinforcement layer are well filled without damaging the structure of the porous polytetrafluoroethylene membrane itself.
[0025] (3) The method of the embodiment of the present invention is to coat the outer side of the first perfluorosulfonic acid resin layer with a second perfluorosulfonic acid resin having a larger equivalent weight, and utilize the excellent anti-deformation property of the high equivalent weight perfluorosulfonic acid resin layer to resist the swelling and shrinkage of the internal low equivalent weight perfluorosulfonic acid resin layer, thereby ensuring the dimensional stability of the composite proton exchange membrane and solving the problem of the contradiction between high conductivity and low swelling performance existing in the current composite proton exchange membrane.
[0026] (4) The method of the embodiment of the present invention is simple and easy to operate. The prepared composite proton exchange membrane has high proton conductivity, high strength and low swelling, which is convenient for promotion and application in industrial production.
[0027] In some embodiments, the first solvent and the second solvent are each independently selected from a mixture of at least one of methanol, ethanol, isopropanol, and n-propanol and water;
[0028] And / or, the surfactant is a nonionic surfactant;
[0029] And / or, the mass content of the surfactant in the first coating liquid or the second coating liquid is 0.1 to 10%;
[0030] And / or, in step (1), the porous polytetrafluoroethylene membrane has a thickness of 5 to 10 μm, a pore size of 50 to 500 nm, and a porosity of 50 to 90%.
[0031] In some embodiments, in step (1), the mass percentage of the first perfluorosulfonic acid resin in the first coating solution is 1 to 50%;
[0032] And / or, in the step (2), the mass percentage of the second perfluorosulfonic acid resin in the second coating solution is 1 to 50%.
[0033] In some embodiments, in step (1), the method for preparing the first coating liquid comprises: heating and dissolving a first perfluorosulfonic acid resin in a first solvent to obtain a first resin dispersion, and adding a surfactant to the first resin dispersion for dispersion treatment to obtain a first coating liquid;
[0034] And / or, in the step (2), the preparation method of the second coating liquid comprises: heating and dissolving a second perfluorosulfonic acid resin in a second solvent to obtain a second resin dispersion, and adding a surfactant to the second resin dispersion for dispersion treatment to obtain a second coating liquid.
[0035] In some embodiments, in step (1), the heating and dissolving temperature is 60 to 200° C., and the heating and dissolving time is 3 to 72 hours;
[0036] And / or, in the step (1), the heating and dissolving temperature is 60 to 300° C., and the heating and dissolving time is 3 to 72 hours;
[0037] And / or, the heating and dissolving is performed in an inert atmosphere.
[0038] In some embodiments, in step (1) and / or step (2), the dispersion treatment adopts sealed high-speed shearing; preferably, the time of the sealed high-speed shearing dispersion is 2 to 30 minutes, the linear speed of the sealed high-speed shearing is 10 to 50 m / s, and the temperature of the sealed high-speed shearing dispersion is 20 to 40°C.
[0039] In some embodiments, in step (1) and / or step (2), the drying treatment is carried out in stages, and the drying temperature in the first stage is 60-100°C, and the drying time is 0.1-1h; the drying temperature in the second stage is 140-220°C, and the drying time is 0.1-1h. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 is a cross-sectional electron microscope image of the composite proton exchange membrane of Example 2, Comparative Example 1 and Comparative Example 2;
[0041] Figure 2 3 is a diagram of the humidity expansion coefficient of the composite proton exchange membrane of Example 2 and Comparative Example 1. DETAILED DESCRIPTION
[0042] Embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to be used to explain the present invention, but should not be understood as limiting the present invention.
[0043] The composite proton exchange membrane of the embodiment of the present invention includes: a porous polytetrafluoroethylene membrane, a first perfluorosulfonic acid resin layer arranged on both sides of the porous polytetrafluoroethylene membrane, and a second perfluorosulfonic acid resin layer arranged on the side of the first perfluorosulfonic acid resin layer away from the porous polytetrafluoroethylene membrane; the equivalent weight (EW) of the first perfluorosulfonic acid resin is less than the equivalent weight (EW) of the second perfluorosulfonic acid resin.
[0044] The composite proton exchange membrane of the embodiment of the present invention does not need to be modified for the porous polytetrafluoroethylene membrane, thus avoiding damage to the structure of the porous polytetrafluoroethylene during the treatment process, thereby ensuring that the prepared composite proton exchange membrane has high air permeability and strength; the composite proton exchange membrane provided by the embodiment of the present invention first uses a first perfluorosulfonic acid resin with a smaller EW value to form a first perfluorosulfonic acid resin layer, thereby achieving sufficient infiltration and filling of the porous polytetrafluoroethylene membrane, so that the composite proton exchange membrane has a higher conductivity, and further uses a second perfluorosulfonic acid resin with a larger EW value to form a second perfluorosulfonic acid resin layer. The resin layer solves the problem of delamination and peeling of the resin and the porous polytetrafluoroethylene membrane reinforcement layer caused by the continuous shrinkage and swelling of the composite proton exchange membrane under dry-wet cycle working conditions, and makes the composite proton exchange membrane have higher strength; the composite proton exchange membrane provided by the embodiment of the present invention solves the swelling and shrinkage problem of the resin of the composite proton exchange membrane under long-term dry-wet cycle conditions while ensuring good filling of the perfluorosulfonic acid resin and the porous polytetrafluoroethylene reinforcement layer, thereby improving the dimensional stability of the composite proton exchange membrane as a whole, and greatly improving the service life of the composite proton exchange membrane in the fuel cell.
[0045] Mechanism of action: The composite proton exchange membranes made of perfluorosulfonic acid resins with different EW values show great differences in conductivity, swelling properties and mechanical properties. The resin coating liquid prepared with perfluorosulfonic acid resins with lower EW values can quickly infiltrate and fill porous polytetrafluoroethylene (ePTFE), and the prepared composite proton exchange membrane has very high conductivity, but poor strength and swelling properties. This is mainly because the perfluorosulfonic acid resins with low EW values have a large number of hydrophilic sulfonate groups on the side chains, which have strong water absorption and proton conductivity, but this also causes the perfluorosulfonic acid resin to have a large volume change during water absorption and dehydration. The perfluorosulfonic acid resin continues to shrink and swell under repeated dry-wet changes, while the ePTFE with strong hydrophobicity does not undergo significant deformation under such dry-wet changes. This difference will cause the perfluorosulfonic acid resin to gradually detach from the ePTFE pores, resulting in a large swelling stress, which is manifested macroscopically as poor dimensional stability of the composite proton exchange membrane. On the other hand, the resin coating liquid prepared by using the perfluorosulfonic acid resin with a high EW value has a slower wetting rate with ePTFE, and the conductivity performance of the composite proton exchange membrane is not as good as that of the composite proton exchange membrane prepared by using the perfluorosulfonic acid resin with a low EW value. However, the composite membrane prepared by the perfluorosulfonic acid resin with a high EW value has a strong deformation resistance, which is mainly due to the fewer sulfonate groups on the side chains of the perfluorosulfonic acid resin with a high EW value and the higher molecular weight and modulus.
[0046] More importantly, although the proton conductivity of the high EW value perfluorosulfonic acid resin layer itself is lost to a certain extent compared with the low EW value perfluorosulfonic acid resin layer, the effect on the overall proton conduction internal resistance of the composite proton exchange membrane is negligible, because for the composite proton exchange membrane, the proton conduction internal resistance mainly depends on the filling effect of the resin and ePTFE.
[0047] It should be noted that the pore structure of the porous polytetrafluoroethylene membrane is filled with a first perfluorosulfonic acid resin, and a second perfluorosulfonic acid resin layer is provided on the side of the first perfluorosulfonic acid resin layer on both sides away from the porous polytetrafluoroethylene membrane.
[0048] In some embodiments, the EW value of the first perfluorosulfonic acid resin is 300-900 g / mol, such as 300 g / mol, 400 g / mol, 500 g / mol, 600 g / mol, 700 g / mol, 800 g / mol, 900 g / mol, etc. Preferably, the EW value of the first perfluorosulfonic acid resin is 700-850 g / mol. The perfluorosulfonic acid resin with a lower EW value is easier to infiltrate and fill in the pore structure of the porous polytetrafluoroethylene, so that the prepared composite proton exchange membrane has a higher conductivity.
[0049] In some embodiments, the EW value of the second perfluorosulfonic acid resin is 900-1500 g / mol, such as 900 g / mol, 1000 g / mol, 1100 g / mol, 1200 g / mol, 1300 g / mol, 1400 g / mol, 1500 g / mol, etc. Preferably, the EW value of the second perfluorosulfonic acid resin is 1000-1200 g / mol. The perfluorosulfonic acid resin with a higher EW value has fewer sulfonic acid groups on the side chain and has a higher modulus, which can give the composite proton exchange membrane a strong deformation resistance.
[0050] In some embodiments, the thickness of the porous polytetrafluoroethylene membrane is 4 to 8 μm, such as 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, etc.
[0051] In some embodiments, the thickness of the first perfluorosulfonic acid resin layer is 0.5 to 2.5 μm, such as 0.5 μm, 0.7 μm, 0.9 μm, 1.1 μm, 1.3 μm, 1.5 μm, 1.7 μm, 1.9 μm, 2.1 μm, 2.3 μm, 2.5 μm, etc.
[0052] In some embodiments, the thickness of the second perfluorosulfonic acid resin layer is 0.5 to 2.5 μm, such as 0.5 μm, 0.7 μm, 0.9 μm, 1.1 μm, 1.3 μm, 1.5 μm, 1.7 μm, 1.9 μm, 2.1 μm, 2.3 μm, 2.5 μm, etc.
[0053] The present invention also provides a method for preparing a composite proton exchange membrane, which comprises the following steps:
[0054] (1) mixing a first perfluorosulfonic acid resin, a surfactant and a first solvent to obtain a first coating liquid, coating the first coating liquid on both sides of a porous polytetrafluoroethylene membrane, and drying to obtain a first perfluorosulfonic acid resin layer;
[0055] (2) Mixing a second perfluorosulfonic acid resin, a surfactant and a second solvent to obtain a second coating liquid, coating the second coating liquid on a side of the first perfluorosulfonic acid resin layer obtained in step (1) away from the porous polytetrafluoroethylene membrane, and drying to obtain a first perfluorosulfonic acid resin layer.
[0056] The preparation method of the composite proton exchange membrane of the embodiment of the present invention does not introduce any material without proton conductivity, and does not cause loss of proton conductivity of the composite proton exchange membrane while providing good dimensional stability of the composite proton exchange membrane; there is no need to perform hydrophilic modification on the surface of the porous polytetrafluoroethylene, and good filling of the resin and the porous polytetrafluoroethylene reinforcement layer is achieved by using a coating liquid of a first perfluorosulfonic acid resin with a small equivalent weight and a strong wetting ability, and the structure of the porous polytetrafluoroethylene membrane itself will not be damaged; a second perfluorosulfonic acid resin with a large equivalent weight is coated on the outer side of the first perfluorosulfonic acid resin layer, and the excellent anti-deformation property of the high equivalent weight perfluorosulfonic acid resin layer is used to resist the swelling and shrinkage of the internal low equivalent weight perfluorosulfonic acid resin layer, so that the dimensional stability of the composite proton exchange membrane can be ensured, and the problem of the contradiction between high conductivity and low swelling performance existing in the current composite proton exchange membrane is solved; the method is simple in process and easy to operate, and the prepared composite proton exchange membrane has high proton conductivity, high strength and low swelling at the same time, which is convenient for popularization and application in industrial production.
[0057] In some embodiments, the first solvent and the second solvent are each independently selected from a mixture of at least one of methanol, ethanol, isopropanol, and n-propanol and water. Preferably, in the first solvent and / or the second solvent, the mass percentage of water is 20 to 80%, more preferably 25 to 60wt%, and more preferably 30 to 50wt%. The first solvent and / or the second solvent do not need to be particularly limited, as long as they can dissolve perfluorosulfonic acid resin and dispersing surfactant. Selecting a mixture of low-boiling alcohols and water as a solvent is conducive to obtaining a more uniform coating solution, and it is easier to remove later to avoid solvent residues in the composite proton exchange membrane.
[0058] In some embodiments, the surfactant is a nonionic surfactant. Preferably, the surfactant is a fatty alcohol polyoxyethylene ether, and surfactants with brands of AE05, AE06, AE09 or AE010 can be directly purchased.
[0059] In some embodiments, the mass content of the surfactant in the first coating liquid or the second coating liquid is 0.1-10%, such as 0.1%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, etc. Preferably, it is 0.5-5wt%; more preferably, it is 1-4wt%. The appropriate amount of surfactant can promote the low EW value resin coating liquid to achieve good filling with the tetrafluoroethylene reinforcement layer.
[0060] In some embodiments, in step (1), the thickness of the porous polytetrafluoroethylene membrane is 5 to 10 μm, such as 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, etc.; the pore size is 50 to 500 nm, such as 50 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm, 500 nm, etc.; the porosity is 50 to 90%, such as 50%, 60%, 70%, 80%, 90%, etc. Preferably, the pore size is 200 to 300 nm, and the porosity is 70 to 85%. The porous polytetrafluoroethylene membrane with suitable thickness, pore size and porosity is more conducive to the infiltration and filling of the first perfluorosulfonic acid resin, and can improve the conductivity of the composite proton exchange membrane.
[0061] It should be noted that since there are a large number of pores in the ePTFE membrane, the pores will shrink after being filled with perfluorosulfonic acid resin and dried to form a membrane, and the ePTFE will become dense. Therefore, the thickness of the ePTFE layer in the composite proton exchange membrane is thinner than the initial thickness of the raw material ePTFE.
[0062] In some embodiments, in step (1), the mass percentage of the first perfluorosulfonic acid resin in the first coating solution is 1-50%, such as 1%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, etc. Preferably, it is 2-30wt%, and more preferably, it is 5-15wt%.
[0063] In some embodiments, in step (2), the mass percentage of the second perfluorosulfonic acid resin in the second coating solution is 1-50%, such as 1%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, etc. Preferably, it is 2-30wt%; more preferably, it is 5-15wt%.
[0064] In some embodiments, in step (1), the method for preparing the first coating liquid comprises: heating and dissolving a first perfluorosulfonic acid resin in a first solvent to obtain a first resin dispersion, and adding a surfactant to the first resin dispersion for dispersion treatment to obtain a first coating liquid;
[0065] And / or, in the step (2), the preparation method of the second coating liquid comprises: heating and dissolving a second perfluorosulfonic acid resin in a second solvent to obtain a second resin dispersion, and adding a surfactant to the second resin dispersion for dispersion treatment to obtain a second coating liquid.
[0066] In some embodiments, in step (1), the heating and dissolving temperature is 60-200°C, such as 60°C, 80°C, 100°C, 120°C, 140°C, 160°C, 180°C, 200°C, etc. Preferably, the heating and dissolving temperature is 80-150°C. More preferably, the heating and dissolving temperature is 100-130°C.
[0067] In some embodiments, in step (2), the heating and dissolving temperature is 60 to 300°C, such as 60°C, 90°C, 120°C, 150°C, 180°C, 210°C, 240°C, 270°C, 300°C, etc. Preferably, the heating and dissolving temperature is 100 to 280°C. More preferably, the heating and dissolving temperature is 150 to 230°C.
[0068] It can be understood that, since the second perfluorosulfonic acid resin having a higher EW value is heated and dissolved in step (2), a relatively high temperature can promote its dissolution.
[0069] In some embodiments, in step (1) and / or step (2), the heating and dissolving time is 3 to 72 hours; such as 3 hours, 5 hours, 10 hours, 15 hours, 20 hours, 25 hours, 30 hours, 35 hours, 40 hours, 45 hours, 50 hours, 55 hours, 60 hours, 65 hours, 70 hours, 72 hours, etc. Preferably, the heating and dissolving time is 4 to 24 hours. More preferably, the heating and dissolving time is 6 to 12 hours.
[0070] In some embodiments, the heating and dissolving is performed in an inert atmosphere. Preferably, the inert gas includes at least one of nitrogen or argon. Considering the production cost, the inert gas is nitrogen.
[0071] In some embodiments, in step (1) and / or step (2), the dispersion treatment adopts sealed high-speed shearing. Compared with the traditional dispersion method, the dispersion treatment adopts sealed high-speed shearing method, which is more conducive to obtaining a homogeneous, high-quality and stable product.
[0072] In some embodiments, the time of the sealed high-speed shear dispersion is 2 to 30 min, such as 2 min, 4 min, 6 min, 8 min, 10 min, 12 min, 14 min, 16 min, 18 min, 20 min, 22 min, 24 min, 26 min, 28 min, 30 min, etc., the linear speed of the sealed high-speed shear is 10 to 50 m / s, such as 10 m / s, 15 m / s, 20 m / s, 25 m / s, 30 m / s, 35 m / s, 40 m / s, 45 m / s, 50 m / s, etc., and the temperature of the sealed high-speed shear dispersion is 20 to 40°C, such as 20°C, 22°C, 24°C, 26°C, 28°C, 30°C, 32°C, 34°C, 36°C, 38°C, 40°C, etc. Preferably, the sealed high-speed shear dispersion time is 5 to 10 minutes, the sealed high-speed shear linear speed is 20 to 30 m / s, and the sealed high-speed shear dispersion temperature is 25 to 30°C.
[0073] In some embodiments, in step (1) and / or step (2), the coating method includes at least one of dipping, spraying, and scraping.
[0074] In some embodiments, in step (1) and / or step (2), the drying process includes two stages. The drying temperature of the first stage is 60-100°C, such as 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, etc., and the drying time is 0.1-1h, such as 0.1h, 0.2h, 0.3h, 0.4h, 0.5h, 0.6h, The second stage drying temperature is 140-220°C, such as 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, etc., and the drying time is 0.1-1h, such as 0.1h, 0.2h, 0.3h, 0.4h, 0.5h, 0.6h, 0.7h, 0.8h, 0.9h, etc. The drying treatment is carried out in stages. The drying treatment is first carried out at a low temperature, which can slowly evaporate the solvent inside the composite proton exchange membrane. The subsequent drying treatment is carried out at a higher temperature to avoid defects such as cracks inside the composite proton exchange membrane due to excessively fast drying.
[0075] The technical solution of the present invention is described in detail below in conjunction with specific embodiments and drawings.
[0076] Example 1
[0077] (1) 200 g of a mixed solvent of water and ethanol, wherein the mass fraction of water is 50%, and 20 g of a first perfluorosulfonic acid resin particle having an EW value of 790 g / mol are added to a reaction kettle in sequence. After the reaction kettle is sealed, nitrogen is introduced to replace the air three times and stirring is started. The reaction kettle is heated to 130° C. and then kept warm for 6 h. After the kettle is cooled to room temperature, the resin solution is taken out to obtain a first resin dispersion with low EW.
[0078] (2) 200 g of a mixed solvent of water and ethanol, wherein the mass fraction of water is 40%, and 10 g of a second perfluorosulfonic acid resin particle having an EW value of 1100 g / mol are added to the reactor in sequence. After the reactor is sealed, nitrogen is introduced to replace the air three times and stirring is started. The reactor is heated to 210° C. and then kept warm for 8 h. After the reactor is cooled to room temperature, the resin solution is taken out to obtain a second resin dispersion with high EW.
[0079] (3) Add 4 wt% of AE05 to the first resin dispersion and the second resin dispersion, respectively, and then use sealed high-speed shear dispersion for 10 minutes, with a shear line speed of 30 m / s and a shear temperature of 25°C to obtain the desired first coating liquid with a low EW value and the second coating liquid with a high EW value, respectively.
[0080] (4) ePTFE with a thickness of 10 μm, a pore size of 250 nm, and a porosity of 75% was selected, and the first coating liquid with a low EW value was coated on the upper and lower sides of the ePTFE, and then transferred to the first stage oven for drying at 80°C for 10 minutes, and then transferred to the second stage oven for drying at 160°C for 20 minutes to solidify into a film, thereby obtaining an ePTFE layer with a thickness of 6 μm and a first perfluorosulfonic acid resin layer with a thickness of 0.5 μm on both sides of the ePTFE (the total thickness of the first perfluorosulfonic acid resin layer on the upper and lower sides of the ePTFE is 1 μm).
[0081] (5) The second coating liquid with a high EW value is coated on the side of the first perfluorosulfonic acid resin layer away from the ePTFE layer, and then transferred to the first stage oven for drying at 80°C for 10 minutes, and then transferred to the second stage oven for drying at 180°C for 30 minutes, and finally a composite proton exchange membrane with a dry thickness of 12 μm is prepared, wherein the thickness of the ePTFE layer is 6 μm, the thickness of the first perfluorosulfonic acid resin layer is 0.5 μm, and the thickness of the second perfluorosulfonic acid resin layer is 2.5 μm (the total thickness of the first perfluorosulfonic acid resin layer on both sides of the ePTFE is 1 μm, and the total thickness of the second perfluorosulfonic acid resin layer on the side of the first perfluorosulfonic acid resin layer away from the ePTFE is 5 μm).
[0082] Example 2
[0083] The preparation method is the same as that in Example 1, except that in steps (4) and (5), a composite proton exchange membrane with a dry thickness of 12 μm is obtained by controlling the coating thickness, wherein the ePTFE layer has a thickness of 6 μm, the first perfluorosulfonic acid resin layer has a thickness of 1 μm, and the second perfluorosulfonic acid resin layer has a thickness of 2 μm (the total thickness of the first perfluorosulfonic acid resin layer on both sides of the ePTFE is 2 μm, and the total thickness of the second perfluorosulfonic acid resin layer on the side of the first perfluorosulfonic acid resin layer away from the ePTFE is 4 μm).
[0084] Example 3
[0085] The preparation method is the same as that in Example 1, except that in steps (4) and (5), a composite proton exchange membrane with a dry thickness of 12 μm is obtained by controlling the coating thickness, wherein the ePTFE layer has a thickness of 6 μm, the first perfluorosulfonic acid resin layer has a thickness of 1.5 μm, and the second perfluorosulfonic acid resin layer has a thickness of 1.5 μm (the total thickness of the first perfluorosulfonic acid resin layer on both sides of the ePTFE is 3 μm, and the total thickness of the second perfluorosulfonic acid resin layer on the side of the first perfluorosulfonic acid resin layer away from the ePTFE is 3 μm).
[0086] Example 4
[0087] The preparation method is the same as that in Example 1, except that in steps (4) and (5), a composite proton exchange membrane with a dry thickness of 12 μm is obtained by controlling the coating thickness, wherein the ePTFE layer has a thickness of 6 μm, the first perfluorosulfonic acid resin layer has a thickness of 2 μm, and the second perfluorosulfonic acid resin layer has a thickness of 1 μm (the total thickness of the first perfluorosulfonic acid resin layer on both sides of the ePTFE is 4 μm, and the total thickness of the second perfluorosulfonic acid resin layer on the side of the first perfluorosulfonic acid resin layer away from the ePTFE is 2 μm).
[0088] Example 5
[0089] The preparation method is the same as that in Example 1, except that in steps (4) and (5), a composite proton exchange membrane with a dry thickness of 12 μm is obtained by controlling the coating thickness, wherein the ePTFE layer thickness is 6 μm, the first perfluorosulfonic acid resin layer thickness is 2.5 μm, and the second perfluorosulfonic acid resin layer thickness is 0.5 μm (the total thickness of the first perfluorosulfonic acid resin layer on both sides of the ePTFE is 5 μm, and the total thickness of the second perfluorosulfonic acid resin layer on the side of the first perfluorosulfonic acid resin layer away from the ePTFE is 1 μm).
[0090] Comparative Example 1
[0091] The preparation method of this comparative example is the same as that of Example 1, except that: step (2) and step (5) are eliminated, and only the first coating liquid is used to prepare a composite proton exchange membrane with a dry thickness of 12 μm, wherein the thickness of the ePTFE layer is 6 μm, and the thickness of the first perfluorosulfonic acid resin layer is 3 μm (the total thickness of the first perfluorosulfonic acid resin layer on both sides of the ePTFE is 6 μm).
[0092] Comparative Example 2
[0093] The preparation method of this comparative example is the same as that of Example 1, except that: step (1) and step (4) are eliminated, and only the second coating liquid is used to prepare a composite proton exchange membrane with a dry thickness of 12 μm, wherein the thickness of the ePTFE layer is 6 μm, and the thickness of the second perfluorosulfonic acid resin layer is 3 μm (the total thickness of the second perfluorosulfonic acid resin layer on both sides of the ePTFE is 6 μm).
[0094] Performance test: The performance test was performed on the composite proton exchange membranes prepared in Examples 1 to 5 and Comparative Examples 1 to 2.
[0095] (1) Scanning electron microscope cross-sectional image: Scanning electron microscope images of the cross-section of the sample were taken, wherein the SEM images of the cross-section of the composite proton exchange membranes prepared in Example 2, Comparative Example 1 and Comparative Example 2 are as follows: Figure 1 shown.
[0096] (2) Swelling rate test: The composite proton exchange membrane was immersed in a constant temperature water bath of 80±2℃ deionized water for 8h and then taken out. The water on the membrane surface was quickly wiped dry, and the membrane size was weighed and measured. The swelling rate is the linear change rate of the membrane in the TD and MD directions after the membrane absorbs water and reaches equilibrium. The results are shown in Table 1.
[0097] (3) Proton conductivity test: The four-electrode method was used to measure the proton conductivity using AC impedance spectroscopy. The test conditions were a temperature of 80±2°C and a relative humidity of 80±5%RH. The proton conductivity was calculated using the formula σ=L / RA, where L is the membrane thickness (cm), R is the membrane impedance (Ω), and A is the cross-sectional area of the effective membrane in contact with the electrode (cm 2 ), and the results are shown in Table 1.
[0098] (4) Tensile property test: The test conditions are temperature 25°C ± 2°C, relative humidity 50 ± 5% RH, gauge length 50 mm, and tensile speed 50 mm / min. The results are shown in Table 1.
[0099] (5) Humidity expansion coefficient test: Using the dynamic thermal stability analyzer DMA creep test method, the sample to be tested was cut into strips with a width of 5.3 mm and a length of >20 mm. The sample was fixed on the fixture and the torque was set to 3.5 N·m and the tensile force was set to 3×10 -4N, taking the sample length as the starting point at 80°C and 0% RH, the hydrothermal strain ε% of the sample under the dry-wet cycle program of 20%-0%-30%-0%-50%-0%-70%-0%-80%-0% was tested at this temperature. The strain ε% was linearly fitted with the water content λ, and its slope × 100 was the humidity expansion coefficient of the sample. The test results of the composite proton exchange membranes prepared in Example 2 and Comparative Example 1 are shown as follows: Figure 2 shown.
[0100] Table 1
[0101]
[0102] It can be seen from the data in Table 1 that Comparative Example 1 is a composite proton exchange membrane prepared using only a low EW value resin coating liquid, and Comparative Example 2 is a composite proton exchange membrane prepared using only a high EW value resin coating liquid. As can be seen from Table 1, the composite proton exchange membranes prepared in Examples 2 and 3 simultaneously have good swelling rate, tensile strength and conductivity performance, among which Example 2 has the best performance in all aspects. When the low EW value perfluorosulfonic acid resin layer accounts for too little, such as Example 1, although the composite proton exchange membrane has a good swelling rate, the filling degree of the composite proton exchange membrane is too poor, which is manifested as a significantly low conductivity and a certain degree of decrease in tensile strength. When the low EW perfluorosulfonic acid value resin layer accounts for too much, such as Examples 4 and 5, although the composite proton exchange membrane has excellent conductivity performance, the swelling and mechanical properties of the composite proton exchange membrane are significantly reduced. By comparing the conductivity performance of Examples 1 to 5, it can be seen that the size of the proton conduction internal resistance of the composite proton exchange membrane mainly depends on the filling effect of the perfluorosulfonic acid resin and ePTFE. When the proportion of the low EW value resin layer reaches the level of Example 2, the pore structure in the ePTFE has been completely filled with perfluorosulfonic acid. Continuing to increase the proportion of the low EW value perfluorosulfonic acid resin layer will no longer improve the conductivity performance of the composite proton exchange membrane, which also indirectly indicates that after the resin and ePTFE are fully filled, the proportion of the high EW value resin layer has almost no effect on the conductivity of the composite proton exchange membrane. In addition, by comparing Example 2 and Comparative Example 1, it can be clearly seen that the composite proton exchange membrane prepared by the method provided by the present invention can greatly improve its swelling performance and mechanical properties while maintaining the same level of conductivity performance.
[0103] from Figure 1 It can be seen that the perfluorosulfonic acid resin and ePTFE in the cross-sectional view of Comparative Example 2 are clearly separated, and there are large gaps in the ePTFE layer that are not completely filled with the resin, which is the main reason for the decrease in the conductivity and mechanical properties of the composite proton exchange membrane. The filling effect of the composite proton exchange membrane of Example 2 is exactly the same as that of Comparative Example 1, which can ensure the excellent conductivity performance of the composite proton exchange membrane.
[0104] from Figure 2 It can be seen that the humidity expansion coefficient of the composite proton exchange membrane of comparative example 1 is significantly higher than that of the composite proton exchange membrane of embodiment 2 of the present invention, which indicates that under repeated dry-wet cycle conditions, the composite proton exchange membrane of embodiment 2 is more resistant to the deformation of the composite proton exchange membrane caused by humidity changes than comparative example 1. Therefore, the composite proton exchange membrane prepared by the present invention has stronger dimensional stability under dry-wet cycle conditions.
[0105] In the present invention, the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" etc. mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the described specific features, structures, materials or characteristics may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0106] Although the above embodiments have been shown and described, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. Changes, modifications, substitutions and variations of the above embodiments by those of ordinary skill in the art are all within the scope of protection of the present invention.
Claims
1. A composite proton exchange membrane, characterized in that: include: A porous polytetrafluoroethylene membrane, a first perfluorosulfonic acid resin layer disposed on both sides of the porous polytetrafluoroethylene membrane, and a second perfluorosulfonic acid resin layer disposed on a side of the first perfluorosulfonic acid resin layer away from the porous polytetrafluoroethylene membrane; The equivalent weight of the first perfluorosulfonic acid resin is less than the equivalent weight of the second perfluorosulfonic acid resin.
2. The composite proton exchange membrane according to claim 1, characterized in that: The equivalent weight of the first perfluorosulfonic acid resin is 300 to 900 g / mol; and / or the equivalent weight of the second perfluorosulfonic acid resin is 900 to 1500 g / mol.
3. The composite proton exchange membrane according to claim 1 or 2, characterized in that: The thickness of the porous polytetrafluoroethylene membrane is 4 to 8 μm; and / or, the thickness of the first perfluorosulfonic acid resin layer is 0.5 to 2.5 μm; And / or, the second perfluorosulfonic acid resin layer has a thickness of 0.5 to 2.5 μm.
4. The method for preparing a composite proton exchange membrane according to any one of claims 1 to 3, characterized in that: The following steps are involved: (1) mixing a first perfluorosulfonic acid resin, a surfactant and a first solvent to obtain a first coating liquid, coating the first coating liquid on both sides of a porous polytetrafluoroethylene membrane, and drying to obtain a first perfluorosulfonic acid resin layer; (2) A second perfluorosulfonic acid resin, a surfactant and a second solvent are mixed to obtain a second coating liquid, and the second coating liquid is applied to a side of the first perfluorosulfonic acid resin layer obtained in step (1) away from the porous polytetrafluoroethylene membrane, followed by drying to obtain a second perfluorosulfonic acid resin layer.
5. The method for preparing a composite proton exchange membrane according to claim 4, characterized in that: The first solvent and the second solvent are each independently selected from a mixture of at least one of methanol, ethanol, isopropanol, and n-propanol and water; And / or, the surfactant is a nonionic surfactant; And / or, the mass content of the surfactant in the first coating liquid or the second coating liquid is 0.1 to 10%; And / or, in step (1), the porous polytetrafluoroethylene membrane has a thickness of 5 to 10 μm, a pore size of 50 to 500 nm, and a porosity of 50 to 90%.
6. The method for preparing a composite proton exchange membrane according to claim 4, characterized in that: In the step (1), the mass percentage of the first perfluorosulfonic acid resin in the first coating solution is 1 to 50%; And / or, in the step (2), the mass percentage of the second perfluorosulfonic acid resin in the second coating solution is 1 to 50%.
7. The method for preparing a composite proton exchange membrane according to claim 4, characterized in that: In the step (1), the preparation method of the first coating liquid comprises: heating and dissolving a first perfluorosulfonic acid resin in a first solvent to obtain a first resin dispersion, and adding a surfactant to the first resin dispersion for dispersion treatment to obtain a first coating liquid; And / or, in the step (2), the preparation method of the second coating liquid comprises: heating and dissolving a second perfluorosulfonic acid resin in a second solvent to obtain a second resin dispersion, and adding a surfactant to the second resin dispersion for dispersion treatment to obtain a second coating liquid.
8. The method for preparing a composite proton exchange membrane according to claim 7, characterized in that: In the step (1), the heating and dissolving temperature is 60 to 200° C., and the heating and dissolving time is 3 to 72 hours; And / or, in the step (2), the heating and dissolving temperature is 60 to 300° C., and the heating and dissolving time is 3 to 72 hours; And / or, the heating and dissolving is performed in an inert atmosphere.
9. The method for preparing a composite proton exchange membrane according to claim 7, characterized in that: In the step (1) and / or the step (2), the dispersion treatment adopts sealed high-speed shearing; Preferably, the sealed high-speed shear dispersion time is 2 to 30 minutes, the sealed high-speed shear linear speed is 10 to 50 m / s, and the sealed high-speed shear dispersion temperature is 20 to 40°C.
10. The method for preparing a composite proton exchange membrane according to claim 4, characterized in that: In step (1) and / or step (2), the drying process includes two stages, the drying temperature of the first stage is 60-100°C, and the drying time is 0.1-1h; the drying temperature of the second stage is 140-220°C, and the drying time is 0.1-1h.
Citation Information
Cited By
Composite proton exchange membrane as well as preparation method and application thereof
CN121282265A
Composite proton exchange membrane and preparation method and application thereof
CN121282265B