Non-flammable phosphate-based electrolyte with fast ion transport capability and application of non-flammable phosphate-based electrolyte
By using a specific combination of non-combustible phosphate-based electrolyte in the lithium-ion battery electrolyte, the problem of existing electrolytes taking into account high ion conductivity and high lithium ion migration number is solved, and the rapid charging and discharge of graphite negative electrodes is achieved. The ratio performance meets the needs of commercial electrodes, and has non-combustible and excellent wetting properties.
Patent Information
- Application Number
- CN202410951939.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
AI Technical Summary
The existing lithium-ion battery electrolyte is difficult to take into account high ion conductivity and high lithium ion migration, resulting in poor rate performance of graphite negative electrodes and difficult to meet the use needs of commercial electrodes.
Using a non-combustible phosphate-based electrolyte, including lithium salt, an organic non-combustible phosphate solvent, a first organic carbonate, a second organic carbonate, a first organic additive and a second organic additive, the component molar ratio and The structure forms an efficient ion transport channel, improves the film forming and viscosity of the electrolyte and ensures rapid transport of lithium ions.
The high ionic conductivity of the electrolyte (>9mS/cm) and high lithium ion migration number (>0.5) are achieved, so that the graphite negative electrode can be quickly charged and discharged under conventional lithium salt concentration, improving the rate performance and meeting the commercial electrode and has non-combustible properties and excellent wetting properties.
Smart Images

Figure CN118919856A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of lithium-ion battery safety technology, and more specifically, relates to a non-flammable phosphate-based electrolyte with fast ion transport capability and its application. Background Art
[0002] Lithium-ion batteries are widely used in 3C electronic products, electric vehicles, energy storage and other fields. However, in recent years, lithium-ion battery accidents have occurred frequently, causing serious economic losses and adverse social impacts. Studies have shown that the highly flammable and volatile carbonate electrolyte in the battery is the root cause of battery fire and explosion. Therefore, the development of non-flammable electrolytes to reduce the risk of battery explosion can protect the application of lithium-ion batteries.
[0003] The development of non-flammable electrolytes is mainly achieved with the help of flame-retardant solvents. At present, the flame-retardant solvents developed mainly include two categories: one is lithium-phobic flame-retardant solvents, that is, solvents that do not react with lithium ions or weakly interact with them. For example, patent document CN116344935A provides an electrolyte containing phosphazene phosphate electrolyte additives. Such solvents are costly and difficult to use in large quantities commercially. In addition, the solvents themselves have poor solubility and require the addition of a large amount of organic co-solvents to improve their solubility; the other is phosphate-based lithium-philic flame-retardant solvents. Such solvents have the advantages of low cost and can be applied on a large scale, but they have a strong reaction with lithium ions, which causes such solvents to decompose when they enter the first solvation shell of lithium. In addition, the decomposition products of the above-mentioned solvents themselves have poor electron shielding ability and cannot prevent the subsequent decomposition of the solvent. Such electrolytes are incompatible with graphite negative electrodes, resulting in failure of the graphite electrode.
[0004] Patent documents CN108539274A, CN109216763A and CN114171794A successfully solved the graphite failure problem caused by phosphate by designing high-concentration and local high-concentration phosphate electrolytes by increasing salt concentration, but such high lithium salt concentration (>2 mol / L) electrolytes are costly and have low ion conductivity (<2 mS / cm), making them difficult to commercialize. Patent document CN116706242A improves the ion conductivity of phosphate-based electrolytes by compounding with carbonates, and can reach the level of commercial electrolytes (ion conductivity>9 mS / cm) at room temperature. However, the lithium ion migration number of the electrolyte is low (<0.3) and the rate performance of the graphite negative electrode is poor, which still cannot meet the use requirements of commercial electrodes.
[0005] Therefore, based on the current challenges, developing non-flammable phosphate-based electrolytes with high ionic conductivity and high lithium ion transference number is the key to promoting the application of low-cost phosphate flame-retardant solvents and an important support for improving battery safety. Summary of the invention
[0006] In view of the defects of the prior art, the purpose of the present application is to provide a non-flammable phosphate-based electrolyte and its application with fast ion transport capability, so as to solve the technical problems that the existing electrolyte cannot take into account both high ionic conductivity and high lithium ion migration number, the graphite negative electrode of the battery assembled with the electrolyte has poor rate performance and is difficult to meet the use requirements of commercial electrodes.
[0007] To achieve the above-mentioned object, the present application provides a non-flammable phosphate-based electrolyte having fast ion transport capability, comprising a lithium salt, an organic non-flammable phosphate solvent, a first organic carbonate, a second organic carbonate, a first organic additive, and a second organic additive;
[0008] The first organic carbonate is used to dissociate the lithium salt, the second organic carbonate is used to reduce the viscosity of the non-flammable phosphate-based electrolyte, the first organic additive is used to participate in the formation of an ion transport channel of the non-flammable phosphate-based electrolyte, and the second organic additive is used to improve the film-forming property of the non-flammable phosphate-based electrolyte;
[0009] The ionic conductivity of the non-flammable phosphate-based electrolyte is greater than 9 mS / cm, and the lithium ion migration number is greater than 0.5.
[0010] Preferably, the concentration of lithium salt in the non-flammable phosphate-based electrolyte is 0.8 to 1.5 mol / L; and / or,
[0011] In the above-mentioned non-flammable phosphate-based electrolyte, the molar ratio of the above-mentioned lithium salt, organic non-flammable phosphate solvent, first organic carbonate, second organic carbonate, first organic additive and second organic additive is 1:(2-2.5):(0.5-3):(1-4):(1-3):(0.1-3).
[0012] Preferably, the lithium salt is selected from at least one of lithium hexafluorophosphate, lithium bis(trifluoromethylsulfonyl)imide and lithium bis(fluorosulfonyl)imide.
[0013] Preferably, the general structural formula of the organic non-flammable phosphate solvent is
[0014]
[0015] Wherein, R1 and R2 are each independently one of an alkyl group having 1 to 10 carbon atoms and a halogenated alkyl group having 1 to 10 carbon atoms, and R3 is an alkyl group having 1 to 10 carbon atoms or an alkoxy group having 1 to 10 carbon atoms.
[0016] More preferably, the above-mentioned organic non-flammable phosphate solvent is selected from one or more of triethyl phosphate, trimethyl phosphate, dimethyl methylphosphonate and tris(2,2,2-trifluoroethyl) phosphate.
[0017] Preferably, the first organic carbonate is selected from one or more of ethylene carbonate, propylene carbonate and fluoroethylene carbonate.
[0018] Preferably, the second organic carbonate is selected from one or more of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, dipropyl carbonate, methyl trifluoroethyl carbonate and di(2,2,2-trifluoroethyl) carbonate.
[0019] Preferably, the first organic additive is selected from one or more of ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, cyclopentyl methyl ether, tetrahydrofuran and 2-methyltetrahydrofuran.
[0020] Preferably, the second organic additive is selected from one or more of ethylene carbonate, vinyl sulfate, 1,3-propane sultone, lithium difluorooxalatoborate, lithium dioxalatoborate and lithium difluorodioxyphosphine.
[0021] The present application also provides a lithium-ion battery, comprising a positive electrode, a negative electrode and an electrolyte, wherein the electrolyte is the above-mentioned non-flammable phosphate-based electrolyte.
[0022] Preferably, the negative electrode is graphite.
[0023] In general, the above technical solutions conceived by this application have the following technical advantages compared with the prior art:
[0024] (1) The non-flammable phosphate-based electrolyte provided in the present application uses a low-cost first organic carbonate as the core backbone solvent. By compounding a first organic additive with a lithium salt, an organic non-flammable phosphate flame-retardant solvent, a first organic carbonate, a second organic carbonate, and a second organic additive and controlling the molar ratio between the components within a suitable range, the ion transport channel in the electrolyte is regulated, and the obtained electrolyte has both high ionic conductivity and high lithium ion migration number, so that lithium ions can be transported quickly.
[0025] (2) The non-flammable phosphate-based electrolyte provided by the present application utilizes the first organic carbonate to dissolve and dissociate lithium salts and controls its concentration within a suitable range to ensure the high ionic conductivity of the electrolyte. At the same time, the first organic additive in the electrolyte can weaken the interaction between the first organic carbonate and lithium ions, and play a role in connecting various solvation structures, thereby forming an ion transmission channel and realizing rapid lithium ion transport. In addition, the above-mentioned first organic carbonate and the first organic additive cooperate with the organic non-flammable phosphate flame retardant solvent, the second organic carbonate, and the second organic additive to realize the non-flammable characteristics of the electrolyte, and at the same time regulate the viscosity of the non-flammable phosphate-based electrolyte, improve the film-forming property, and make the non-flammable phosphate-based electrolyte compatible with the graphite negative electrode. Through the synergistic effect between the components, the non-flammable phosphate-based electrolyte can take into account both high ionic conductivity and high lithium ion migration number at conventional lithium salt concentrations, and has excellent fast ion transport capacity, good wettability and is non-flammable.
[0026] (3) The non-flammable phosphate-based electrolyte provided in the present application has an ion conductivity greater than 9mS / cm and a lithium ion migration number greater than 0.5. The battery assembled with the above non-flammable phosphate-based electrolyte can achieve compatibility between the phosphate-based non-flammable electrolyte and the graphite negative electrode at conventional electrolyte concentrations (about 1 mol / L), and the high ion conductivity and high lithium ion migration number enable the battery graphite negative electrode to achieve rapid charge and discharge, and for the first time, the rate performance of the graphite negative electrode is improved to the level of commercial carbonate electrolytes. The design breaks the design bottleneck of the low lithium ion migration number of the non-flammable phosphate electrolyte, and has excellent practical prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The flammability test results of the electrolytes provided in Example 1 (experimental group) and Comparative Example 1 (control group) of the present application are shown in FIG.
[0028] Figure 2 It is a direct observation of the ion transport channels in the electrolyte provided by Example 1 (experimental group) and Comparative Example 2 (control group) of the present application under infrared light irradiation;
[0029] Figure 3 This is the first cycle charge and discharge curve of the graphite negative electrode of the battery assembled with the electrolyte provided in Example 1 of the present application;
[0030] Figure 4 The first cycle charge and discharge curve of the graphite negative electrode of the battery assembled with the electrolyte provided in Comparative Example 3 of the present application. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solution and advantages of the present application more clear, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described here are only used to explain the present application and are not used to limit the present application.
[0032] The present application provides a non-flammable phosphate-based electrolyte having fast ion transport capability, comprising a lithium salt, an organic non-flammable phosphate solvent, a first organic carbonate, a second organic carbonate, a first organic additive, and a second organic additive;
[0033] The first organic carbonate is used to dissociate lithium salt, the second organic carbonate is used to reduce the viscosity of the non-flammable phosphate-based electrolyte, the first organic additive is used to participate in the formation of an ion transport channel of the non-flammable phosphate-based electrolyte, and the second organic additive is used to improve the film-forming property of the non-flammable phosphate-based electrolyte;
[0034] The ionic conductivity of the non-flammable phosphate-based electrolyte is greater than 9 mS / cm, and the lithium ion migration number is greater than 0.5.
[0035] The electrolyte provided in the present application can be applied to various conventional lithium salts. In some embodiments, the lithium salt is selected from at least one of lithium hexafluorophosphate, lithium bis(trifluoromethylsulfonyl)imide and lithium bis(fluorosulfonyl)imide.
[0036] In some embodiments, the concentration of lithium salt in the non-flammable phosphate-based electrolyte is 0.8 mol / L to 1.5 mol / L.
[0037] In some embodiments, in the above-mentioned non-flammable phosphate-based electrolyte, the molar ratio of the lithium salt, the organic non-flammable phosphate solvent, the first organic carbonate, the second organic carbonate, the first organic additive and the second organic additive is 1:(2~2.5):(0.5~3):(1~4):(1~3):(0.1~3).
[0038] The components of the non-flammable phosphate-based electrolyte provided in the present application work synergistically. Experiments have found that the amount of each component in the electrolyte relative to the lithium salt is controlled within a suitable range, so that the above-mentioned electrolyte has both high ionic conductivity and high lithium ion migration number, and is compatible with the graphite negative electrode, thereby achieving rapid charging and discharging of the graphite negative electrode and significantly improving the rate performance of the graphite negative electrode.
[0039] In some embodiments, the above-mentioned organic non-flammable phosphate solvent has the general structural formula:
[0040]
[0041] Wherein, R1 and R2 are each independently one of an alkyl group having 1 to 10 carbon atoms and a halogenated alkyl group having 1 to 10 carbon atoms, and R3 is an alkyl group having 1 to 10 carbon atoms or an alkoxy group having 1 to 10 carbon atoms.
[0042] In a preferred embodiment, the organic non-flammable phosphate solvent is selected from one or more of triethyl phosphate, trimethyl phosphate, dimethyl methylphosphonate and tris(2,2,2-trifluoroethyl) phosphate.
[0043] In some embodiments, the first organic carbonate is selected from one or more of ethylene carbonate, propylene carbonate and fluoroethylene carbonate.
[0044] In some embodiments, the second organic carbonate is selected from one or more of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, dipropyl carbonate, methyl trifluoroethyl carbonate and di(2,2,2-trifluoroethyl) carbonate.
[0045] In some embodiments, the first organic additive is selected from one or more of ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, cyclopentyl methyl ether, tetrahydrofuran and 2-methyltetrahydrofuran.
[0046] In some embodiments, the second organic additive is selected from one or more of ethylene carbonate, vinyl sulfate, 1,3-propane sultone, lithium difluorooxalatoborate, lithium dioxalatoborate and lithium difluorodioxyphosphine.
[0047] The present application also provides the use of the above-mentioned non-flammable phosphate-based electrolyte in a lithium-ion battery.
[0048] The present application also provides a lithium-ion battery, comprising a positive electrode, a negative electrode and an electrolyte; wherein the electrolyte is the above-mentioned non-flammable phosphate-based electrolyte.
[0049] In some embodiments, the negative electrode is graphite.
[0050] The above technical solutions are described in detail below in conjunction with specific embodiments. It should be understood that these are merely exemplary and are not intended to limit the present application. Materials identical or similar to the types, models, qualities, properties or functions of the following reagents and instruments can be used to implement the present application. The experimental methods used in the following embodiments are conventional methods unless otherwise specified. The materials, reagents, etc. used in the following embodiments, unless otherwise specified, can all be obtained from commercial sources.
[0051] The following are examples and comparative examples:
[0052] Example 1
[0053] The electrolyte provided in this embodiment includes lithium hexafluorophosphate, triethyl phosphate, ethylene carbonate, dimethyl carbonate, ethylene glycol dimethyl ether and ethylene carbonate in a molar ratio of 1:2:0.5:4:1:3, and the concentration of lithium hexafluorophosphate in the electrolyte is 1.1 mol / L.
[0054] Preparation method of electrolyte: dissolve the above lithium hexafluorophosphate in triethyl phosphate, ethylene carbonate, ethylene glycol dimethyl ether and ethylene carbonate according to proportion, stir and mix at room temperature, then add dimethyl carbonate and mix to obtain electrolyte.
[0055] Example 2
[0056] The electrolyte provided in this embodiment includes lithium hexafluorophosphate, triethyl phosphate, propylene carbonate, ethyl methyl carbonate, ethylene glycol dimethyl ether and ethylene carbonate in a molar ratio of 1:2:0.5:4:1:3, and the concentration of lithium hexafluorophosphate in the electrolyte is 0.98 mol / L.
[0057] Preparation method of electrolyte: dissolve the above lithium hexafluorophosphate in triethyl phosphate, propylene carbonate, ethylene glycol dimethyl ether and ethylene carbonate according to proportion, stir and mix at room temperature, then add ethyl methyl carbonate and mix to obtain electrolyte.
[0058] Example 3
[0059] The electrolyte provided in this embodiment includes lithium hexafluorophosphate, triethyl phosphate, fluoroethylene carbonate, ethyl methyl carbonate, ethylene glycol dimethyl ether and ethylene carbonate in a molar ratio of 1:2:0.5:4:1:3, and the concentration of lithium hexafluorophosphate in the electrolyte is 0.95 mol / L.
[0060] Preparation method of electrolyte: dissolve the above lithium hexafluorophosphate in triethyl phosphate, fluoroethylene carbonate, ethylene glycol dimethyl ether and ethylene carbonate according to proportion, stir and mix at room temperature, then add ethyl methyl carbonate and mix to obtain electrolyte.
[0061] Example 4
[0062] The electrolyte provided in this embodiment includes lithium hexafluorophosphate, triethyl phosphate, ethylene carbonate, dimethyl carbonate, diethylene glycol dimethyl ether and ethylene carbonate in a molar ratio of 1:2:0.5:4:1:3, and the concentration of lithium hexafluorophosphate in the electrolyte is 1.05 mol / L.
[0063] Preparation method of electrolyte: dissolve the above lithium hexafluorophosphate in triethyl phosphate, ethylene carbonate, diethylene glycol dimethyl ether and ethylene carbonate according to proportion, stir and mix at room temperature, then add dimethyl carbonate and mix to obtain electrolyte.
[0064] Example 5
[0065] The electrolyte provided in this embodiment includes lithium hexafluorophosphate, triethyl phosphate, ethylene carbonate, dimethyl carbonate, tetraethylene glycol dimethyl ether and ethylene carbonate in a molar ratio of 1:2:0.5:4:1:3, and the concentration of lithium hexafluorophosphate in the electrolyte is 0.96 mol / L.
[0066] Preparation method of electrolyte: dissolve the above lithium hexafluorophosphate in triethyl phosphate, ethylene carbonate, tetraethylene glycol dimethyl ether and ethylene carbonate according to proportion, stir and mix at room temperature, then add dimethyl carbonate and mix to obtain electrolyte.
[0067] Example 6
[0068] The electrolyte provided in this embodiment includes lithium hexafluorophosphate, triethyl phosphate, ethylene carbonate, dimethyl carbonate, diethylene glycol dimethyl ether and vinyl sulfate in a molar ratio of 1:2:0.5:4:1:3, and the concentration of lithium hexafluorophosphate in the electrolyte is 1 mol / L.
[0069] Preparation method of electrolyte: dissolve the above lithium hexafluorophosphate in triethyl phosphate, ethylene carbonate, diethylene glycol dimethyl ether and vinyl sulfate according to proportion, stir and mix at room temperature, then add dimethyl carbonate and mix to obtain electrolyte.
[0070] Example 7
[0071] The electrolyte provided in this embodiment includes lithium hexafluorophosphate, triethyl phosphate, ethylene carbonate, dimethyl carbonate, tetraethylene glycol dimethyl ether and vinyl sulfate in a molar ratio of 1:2:0.5:4:1:3, and the concentration of lithium hexafluorophosphate in the electrolyte is 1.02 mol / L.
[0072] Preparation method of electrolyte: dissolve the above lithium hexafluorophosphate in triethyl phosphate, ethylene carbonate, tetraethylene glycol dimethyl ether and vinyl sulfate according to proportion, stir and mix at room temperature, then add dimethyl carbonate and mix to obtain electrolyte.
[0073] Example 8
[0074] The electrolyte provided in this embodiment includes lithium hexafluorophosphate, triethyl phosphate, ethylene carbonate, dimethyl carbonate, diethylene glycol dimethyl ether and ethylene carbonate in a molar ratio of 1:2.5:0.5:4:1:3, and the concentration of lithium hexafluorophosphate in the electrolyte is 1.0 mol / L.
[0075] Preparation method of electrolyte: dissolve the above lithium hexafluorophosphate in triethyl phosphate, ethylene carbonate, ethylene glycol dimethyl ether and ethylene carbonate according to proportion, stir and mix at room temperature, then add dimethyl carbonate and mix to obtain electrolyte.
[0076] Example 9
[0077] The electrolyte provided in this embodiment includes lithium hexafluorophosphate, triethyl phosphate, ethylene carbonate, dimethyl carbonate, diethylene glycol dimethyl ether and ethylene carbonate in a molar ratio of 1:2.5:0.5:1:3:3, and the concentration of lithium hexafluorophosphate in the electrolyte is 1.0 mol / L.
[0078] Preparation method of electrolyte: dissolve the above lithium hexafluorophosphate in triethyl phosphate, ethylene carbonate, ethylene glycol dimethyl ether and ethylene carbonate according to proportion, stir and mix at room temperature, then add dimethyl carbonate and mix to obtain electrolyte.
[0079] Example 10
[0080] The electrolyte provided in this embodiment includes lithium hexafluorophosphate, triethyl phosphate, ethylene carbonate, dimethyl carbonate, diethylene glycol dimethyl ether and ethylene carbonate in a molar ratio of 1:2.5:3:1:3:0.1, and the concentration of lithium hexafluorophosphate in the electrolyte is 1.02 mol / L.
[0081] Preparation method of electrolyte: dissolve the above lithium hexafluorophosphate in triethyl phosphate, ethylene carbonate, ethylene glycol dimethyl ether and ethylene carbonate according to proportion, stir and mix at room temperature, then add dimethyl carbonate and mix to obtain electrolyte.
[0082] Embodiment 11
[0083] The electrolyte provided in this embodiment includes lithium hexafluorophosphate, trimethyl phosphate, ethylene carbonate, dimethyl carbonate, diethylene glycol dimethyl ether and ethylene carbonate in a molar ratio of 1:2:0.5:4:1:3, and the concentration of lithium hexafluorophosphate in the electrolyte is 1.1 mol / L.
[0084] Preparation method of electrolyte: dissolve the above lithium hexafluorophosphate in trimethyl phosphate, ethylene carbonate, diethylene glycol dimethyl ether and ethylene carbonate according to proportion, stir and mix at room temperature, then add dimethyl carbonate and mix to obtain electrolyte.
[0085] Example 12
[0086] The electrolyte provided in this embodiment includes lithium hexafluorophosphate, dimethyl methylphosphonate, ethylene carbonate, dimethyl carbonate, ethylene glycol dimethyl ether and ethylene carbonate in a molar ratio of 1:2:0.5:4:1:3, and the concentration of lithium hexafluorophosphate in the electrolyte is 1.1 mol / L.
[0087] Preparation method of electrolyte: dissolve the above lithium hexafluorophosphate in dimethyl methylphosphonate, ethylene carbonate, ethylene glycol dimethyl ether and ethylene carbonate according to proportion, stir and mix at room temperature, then add dimethyl carbonate and mix to obtain electrolyte.
[0088] Example 13
[0089] The electrolyte provided in this embodiment includes lithium bis(fluorosulfonyl)imide, triethyl phosphate, ethylene carbonate, dimethyl carbonate, ethylene glycol dimethyl ether and ethylene carbonate in a molar ratio of 1:2:0.5:4:1:3, and the concentration of lithium hexafluorophosphate in the electrolyte is 1.1 mol / L.
[0090] Preparation method of electrolyte: dissolve the above-mentioned lithium bis(fluorosulfonyl)imide in triethyl phosphate, ethylene carbonate, ethylene glycol dimethyl ether and ethylene carbonate according to proportion, stir and mix at room temperature, then add dimethyl carbonate and mix to obtain electrolyte.
[0091] Comparative Example 1 (without organic non-flammable phosphate solvent)
[0092] The electrolyte provided in this comparative example includes lithium hexafluorophosphate, ethylene carbonate, dimethyl carbonate, ethylene glycol dimethyl ether and ethylene carbonate in a molar ratio of 1:0.5:4:2:0.5, and the concentration of lithium hexafluorophosphate in the electrolyte is 1.2 mol / L.
[0093] Preparation method of electrolyte: dissolve the above lithium hexafluorophosphate in ethylene carbonate, triethyl phosphate, ethylene glycol dimethyl ether and ethylene carbonate according to proportion, stir and mix at room temperature, then add dimethyl carbonate and mix to obtain electrolyte.
[0094] Comparative Example 2 (without the first organic additive)
[0095] The electrolyte provided in this comparative example includes lithium hexafluorophosphate, triethyl phosphate, ethylene carbonate, dimethyl carbonate and ethylene carbonate in a molar ratio of 1:2:0.5:4:0.5, and the concentration of lithium hexafluorophosphate in the electrolyte is 1.3 mol / L.
[0096] Preparation method of electrolyte: dissolve the above lithium hexafluorophosphate in triethyl phosphate, ethylene carbonate and ethylene carbonate according to proportion, stir and mix at room temperature, then add dimethyl carbonate and mix to obtain electrolyte.
[0097] Comparative Example 3 (without the second organic additive)
[0098] The electrolyte provided in this comparative example includes lithium hexafluorophosphate, triethyl phosphate, ethylene carbonate, dimethyl carbonate and ethylene glycol dimethyl ether in a molar ratio of 1:2:0.5:4:2, and the concentration of lithium hexafluorophosphate in the electrolyte is 1.15 mol / L.
[0099] Preparation method of electrolyte: dissolve the above lithium hexafluorophosphate in triethyl phosphate, ethylene carbonate and ethylene glycol dimethyl ether according to proportion, stir and mix at room temperature, then add dimethyl carbonate and mix to obtain electrolyte.
[0100] Comparative Example 4 (electrolyte prepared by patent CN116706242A)
[0101] The electrolyte provided in this comparative example is prepared according to the method and formula provided in patent CN116706242A, and includes lithium hexafluorophosphate, triethyl phosphate, ethylene carbonate and dimethyl carbonate in a molar ratio of 1:2:2:3, and the concentration of lithium hexafluorophosphate in the electrolyte is 1.37 mol / L.
[0102] Preparation method of electrolyte: In a glove box, first dissolve lithium hexafluorophosphate in ethylene carbonate and triethyl phosphate, stir and mix at room temperature, then add dimethyl carbonate and mix to obtain electrolyte.
[0103] Comparative Example 5 (the first organic additive is 1,1,1,3,3,3-hexafluoroisopropyl methyl ether)
[0104] The electrolyte provided in this comparative example includes lithium hexafluorophosphate, triethyl phosphate, ethylene carbonate, dimethyl carbonate, 1,1,1,3,3,3-hexafluoroisopropyl methyl ether and ethylene carbonate in a molar ratio of 1:2:0.5:4:1:3, and the concentration of lithium hexafluorophosphate in the electrolyte is 1.05 mol / L.
[0105] Preparation method of electrolyte: dissolve the above lithium hexafluorophosphate in triethyl phosphate, ethylene carbonate, 1,1,1,3,3,3-hexafluoroisopropyl methyl ether and ethylene carbonate according to proportion, stir and mix at room temperature, then add dimethyl carbonate and mix to obtain electrolyte.
[0106] Comparative Example 6 (the first organic additive is 1,1,2,2-tetrafluoroethyl ether-2,2,3,3-tetrafluoropropyl ether)
[0107] The electrolyte provided in this comparative example includes lithium hexafluorophosphate, ethylene carbonate, triethyl phosphate, dimethyl carbonate, 1,1,2,2-tetrafluoroethyl ether-2,2,3,3-tetrafluoropropyl ether and ethylene carbonate in a molar ratio of 1:0.5:2:4:1:3, and the concentration of lithium hexafluorophosphate in the electrolyte is 1.02 mol / L.
[0108] Preparation method of electrolyte: dissolve the above lithium hexafluorophosphate in ethylene carbonate, triethyl phosphate, 1,1,2,2-tetrafluoroethyl ether-2,2,3,3-tetrafluoropropyl ether and ethylene carbonate according to proportion, stir and mix at room temperature, then add dimethyl carbonate and mix to obtain electrolyte.
[0109] Comparative Example 7 (the first organic additive is 1,3-dioxolane)
[0110] The electrolyte provided in this comparative example includes lithium hexafluorophosphate, triethyl phosphate, ethylene carbonate, dimethyl carbonate, 1,3-dioxolane and ethylene carbonate in a molar ratio of 1:2:0.5:4:1:3, and the concentration of lithium hexafluorophosphate in the electrolyte is 1.08 mol / L.
[0111] Preparation method of electrolyte: dissolve the above lithium hexafluorophosphate in triethyl phosphate, ethylene carbonate, 1,3-dioxolane and ethylene carbonate according to proportion, stir and mix at room temperature, then add dimethyl carbonate and mix to obtain electrolyte.
[0112] Comparative Example 8 (the first organic additive is sulfolane)
[0113] The electrolyte provided in this comparative example includes lithium hexafluorophosphate, triethyl phosphate, ethylene carbonate, dimethyl carbonate, cyclopentane sulfone and ethylene carbonate in a molar ratio of 1:2:0.5:4:1:3, and the concentration of lithium hexafluorophosphate in the electrolyte is 1.1 mol / L.
[0114] Preparation method of electrolyte: dissolve the above lithium hexafluorophosphate in triethyl phosphate, ethylene carbonate, cyclopentane sulfone and ethylene carbonate according to proportion, stir and mix at room temperature, then add dimethyl carbonate and mix to obtain electrolyte.
[0115] Comparative Example 9
[0116] The electrolyte provided in this comparative example includes lithium hexafluorophosphate, triethyl phosphate, ethylene carbonate, dimethyl carbonate, ethylene glycol dimethyl ether and ethylene carbonate in a molar ratio of 1:2:0.5:4:0.5:3, and the concentration of lithium hexafluorophosphate in the electrolyte is 1.2 mol / L.
[0117] Preparation method of electrolyte: dissolve the above lithium hexafluorophosphate in ethylene carbonate, triethyl phosphate, ethylene glycol dimethyl ether and ethylene carbonate according to proportion, stir and mix at room temperature, then add dimethyl carbonate and mix to obtain electrolyte.
[0118] Comparative Example 10
[0119] The electrolyte provided in this comparative example includes lithium hexafluorophosphate, triethyl phosphate, ethylene carbonate, dimethyl carbonate, ethylene glycol dimethyl ether and ethylene carbonate in a molar ratio of 1:2:0.5:4:3.5:3, and the concentration of lithium hexafluorophosphate in the electrolyte is 1.05 mol / L.
[0120] Preparation method of electrolyte: dissolve the above lithium hexafluorophosphate in triethyl phosphate, ethylene carbonate, ethylene glycol dimethyl ether and ethylene carbonate according to proportion, stir and mix at room temperature, then add dimethyl carbonate and mix to obtain electrolyte.
[0121] The properties of the electrolytes prepared in Examples 1 to 13 and Comparative Examples 1 to 10 were tested as follows:
[0122] 1) Determination of ionic conductivity: direct reading using a Lei-Magnetic DDS-307A conductivity meter.
[0123] 2) Determination of lithium ion migration number: DC polarization and AC impedance spectroscopy.
[0124] 3) Non-flammability test: diaphragm ignition method.
[0125] 4) Wettability test: contact angle tester.
[0126] 5) Whether an ion transmission channel is formed: infrared light irradiation.
[0127] The properties of the electrolytes prepared in Examples 1 to 13 and Comparative Examples 1 to 10 are shown in Table 1.
[0128] Table 1 Characteristics of the electrolytes prepared in Examples 1 to 13 and Comparative Examples 1 to 10
[0129]
[0130]
[0131] In Table 1, the concentration of lithium salt in the electrolytes prepared in Examples 1 to 13 is 0.8 to 1.5 mol / L, the ion conductivity is greater than 9 mS / cm, the contact angle with the diaphragm is less than 45°, and the non-flammability test results show that the above electrolytes are non-flammable. In addition, the lithium ion migration number in the electrolytes prepared in Examples 1 to 13 is greater than 0.5, and has excellent fast ion transport capacity. The electrolyte prepared in this application can have high ionic conductivity and improve the lithium ion migration number at conventional lithium salt concentrations, and has non-flammable properties and good wettability to the diaphragm.
[0132] The electrolyte prepared in Comparative Example 1 did not contain an organic non-flammable phosphate solvent, and the results of the flammability test showed that the electrolyte was flammable ( Figure 1 ), when the electrolyte prepared in Example 1 was subjected to a flammability test, the electrolyte could not be ignited, indicating that the electrolyte prepared in Example 1 has a non-flammable property.
[0133] Lithium ion transport in the electrolyte is carried out in the form of solvated structures. When the size of the solvated structure clusters formed in the electrolyte is large, a bright path can be seen when the electrolyte is irradiated with infrared light. The electrolyte prepared in Comparative Example 2 does not contain the first organic additive, and its ion conductivity is 6mS / cm, and the lithium ion migration number is only 0.25, which is significantly lower than that in Example 1. When the electrolytes prepared in Example 1 and Comparative Example 2 are irradiated with infrared light, it can be seen that ( Figure 2), the electrolyte prepared in Example 1 shows obvious bright path, while the electrolyte prepared in Comparative Example 2 shows no bright path, indicating that Example 1 forms an ion transmission channel compared with Comparative Example 2. The reason for this may be that the first organic additive added in Example 1 can weaken the interaction between the first organic carbonate and lithium ions, and plays a role in connecting various solvation structures, thereby forming an ion transmission channel with a large size of the solvation structure, and a large number of lithium ion migrations, and having excellent fast ion transport capacity, while the first organic additive is not added to the electrolyte prepared in Comparative Example 2, and the solvation structures in the electrolyte cannot be effectively connected, thereby failing to form an ion transmission channel.
[0134] Comparative Example 4 is an electrolyte prepared according to the method and formula provided in patent CN116706242A. Its lithium ion migration number is significantly lower than that of Example 1. The reason may be that the lack of the first organic additive in the electrolyte prepared in patent document CN116706242A causes the solvation structure in the electrolyte to be unable to be effectively connected, and unable to form a channel that is conducive to lithium ion transmission.
[0135] The first organic additives in the electrolytes prepared in Comparative Examples 5, 6, 7 and 8 are 1,1,1,3,3,3-hexafluoroisopropyl methyl ether, 1,1,2,2-tetrafluoroethyl ether-2,2,3,3-tetrafluoropropyl ether, 1,3-dioxolane and cyclopentane sulfone, respectively. The lithium ion migration numbers of the prepared electrolytes are all lower than those in Example 1, indicating that 1,1,1,3,3,3-hexafluoroisopropyl methyl ether, 1,1,2,2-tetrafluoroethyl ether-2,2,3,3-tetrafluoropropyl ether, 1,3-dioxolane and cyclopentane sulfone cannot form coordination with lithium ions and form ion transport channels, so that the lithium ion migration number of the electrolyte cannot be improved.
[0136] The molar ratio of the first organic additive ethylene glycol dimethyl ether to other raw materials in the electrolyte prepared in Comparative Example 9 is lower than that in Example 1, and the test shows that the electrolyte has high ionic conductivity, but the lithium ion migration number is low; the molar ratio of the first organic additive ethylene glycol dimethyl ether to other raw materials in the electrolyte prepared in Comparative Example 10 is higher than that in Example 1, and the test shows that the lithium ion migration number of the electrolyte is lower than that in Example 1. It may be that when the amount of the first organic additive added to the electrolyte is too large, although an ion transmission channel can be formed, the effect of the first organic additive on lithium ions is too strong, which makes it difficult for lithium ions to migrate quickly, thereby significantly reducing the lithium ion migration number.
[0137] The electrolytes prepared in the above examples and comparative examples, the metal lithium positive electrode, and the graphite negative electrode were assembled into a battery, and the first cycle coulomb efficiency of the graphite negative electrode and the rate performance of the graphite negative electrode of the battery were tested by charging and discharging the battery on the battery test channel. The test results are shown in Table 2.
[0138] Table 2 Performance of batteries assembled with electrolytes prepared in Examples 1 to 13 and Comparative Examples 1 to 10
[0139]
[0140]
[0141] It can be seen from Table 2 that the first-cycle coulombic efficiency of the graphite negative electrode of the battery assembled with the electrolyte prepared in the embodiment is 85% or more, and the capacity retention rate of the graphite negative electrode at 2C is 92% or more, indicating that the graphite negative electrode of the battery assembled in the embodiment can achieve rapid charge and discharge at a high rate, has excellent rate performance, and can meet the use requirements of commercial electrodes. Figure 3 The first cycle charge and discharge curve of the graphite negative electrode of the battery assembled in Example 1 shows that the first cycle coulombic efficiency of the graphite negative electrode is 88%, and there is no solvent decomposition side reaction.
[0142] The graphite negative electrode of the battery assembled with the electrolyte prepared in the comparative example exhibited poor rate performance, and could not achieve rapid charge and discharge at high rates, and could not meet the use requirements of commercial electrodes. The electrolyte prepared in comparative example 3 did not contain the second organic additive, and when it was assembled into a battery, the graphite negative electrode could not achieve normal charge and discharge reactions ( Figure 4 ), obvious solvent decomposition occurs during the charge and discharge process, and the first-cycle coulomb efficiency of the graphite negative electrode is low, only 60%. Considering that the graphite negative electrode cannot be charged and discharged normally, the rate performance of the graphite negative electrode is not tested, and is indicated by “-”.
[0143] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application shall be included in the scope of protection of the present application.
Claims
1. A non-flammable phosphate-based electrolyte having fast ion transport capability, characterized in that: comprising a lithium salt, an organic non-flammable phosphate solvent, a first organic carbonate, a second organic carbonate, a first organic additive, and a second organic additive; Wherein, the first organic carbonate is used to dissociate the lithium salt, the second organic carbonate is used to reduce the viscosity of the non-flammable phosphate-based electrolyte, the first organic additive is used to participate in the formation of an ion transport channel of the non-flammable phosphate-based electrolyte, and the second organic additive is used to improve the film-forming property of the non-flammable phosphate-based electrolyte; The non-flammable phosphate-based electrolyte has an ion conductivity greater than 9 mS / cm and a lithium ion transference number greater than 0.
5.
2. The non-flammable phosphate-based electrolyte according to claim 1, characterized in that: The concentration of lithium salt in the non-flammable phosphate-based electrolyte is 0.8 mol / L to 1.5 mol / L; and / or, In the non-flammable phosphate-based electrolyte, the molar ratio of the lithium salt, the organic non-flammable phosphate solvent, the first organic carbonate, the second organic carbonate, the first organic additive and the second organic additive is 1:(2-2.5):(0.5-3):(1-4):(1-3):(0.1-3).
3. The non-flammable phosphate-based electrolyte according to claim 1 or 2, characterized in that: The lithium salt is selected from at least one of lithium hexafluorophosphate, lithium bis(trifluoromethylsulfonyl)imide and lithium bis(fluorosulfonyl)imide.
4. The non-flammable phosphate-based electrolyte according to claim 1, characterized in that: The general structural formula of the organic non-flammable phosphate solvent is: Wherein, R1 and R2 are each independently one of an alkyl group having 1 to 10 carbon atoms and a halogenated alkyl group having 1 to 10 carbon atoms, and R3 is an alkyl group having 1 to 10 carbon atoms or an alkoxy group having 1 to 10 carbon atoms.
5. The non-flammable phosphate-based electrolyte according to claim 1, characterized in that: The first organic carbonate is selected from one or more of ethylene carbonate, propylene carbonate and fluoroethylene carbonate.
6. The non-flammable phosphate-based electrolyte according to claim 1, characterized in that: The second organic carbonate is selected from one or more of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, dipropyl carbonate, methyl trifluoroethyl carbonate and di(2,2,2-trifluoroethyl) carbonate.
7. The non-flammable phosphate-based electrolyte according to claim 1, characterized in that: The first organic additive is selected from one or more of ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, cyclopentyl methyl ether, tetrahydrofuran and 2-methyltetrahydrofuran.
8. The non-flammable phosphate-based electrolyte according to claim 1, characterized in that: The second organic additive is selected from one or more of ethylene carbonate, vinyl sulfate, 1,3-propane sultone, lithium difluorooxalatoborate, lithium dioxalatoborate and lithium difluorodioxophosphine.
9. A lithium ion battery, characterized in that: The invention comprises a positive electrode, a negative electrode and an electrolyte, wherein the electrolyte is the non-flammable phosphate-based electrolyte according to any one of claims 1 to 8.
10. The lithium ion battery according to claim 9, characterized in that: The negative electrode is graphite.
Citation Information
Cited By
Method for designing non-combustible phosphate electrolyte compatible with graphite cathode by utilizing machine learning
CN119541702A