Formation and constant volume process of sodium ion short blade battery
By optimizing the decomposition and capacity setting steps of sodium ion batteries, using constant current charging and charging and discharging treatment under specific temperature and negative pressure conditions, the problem of insufficient performance of sodium ion batteries in the prior art is solved, and the first capacity and cycle are significantly improved Lifespan improves battery performance.
Patent Information
- Application Number
- CN202411263293.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-09-10
AI Technical Summary
The existing sodium ion battery is mostly based on lithium ion batteries, which fails to effectively improve the performance of sodium ion batteries, especially the first capacity, charge and discharge efficiency and cycle life.
Using the sodium ion battery shaping process, including battery pretreatment, decomposition, standstill and capacity setting steps, the sodium ions are optimized in the positive and negative electrode materials through constant current charging and charging and discharging treatment under specific temperature and negative pressure conditions. The embedding and deintercalation behavior in the process exhaust gas is discharged and a stable sodium ion embedding layer is formed.
It significantly improves the first capacity, charge and discharge efficiency and cycle life of sodium ion batteries, improves battery performance, reduces gas production, and improves battery stability.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sodium ion batteries, and in particular relates to a formation and volume determination process of a sodium ion short blade battery. Background Art
[0002] Sodium-ion batteries are secondary batteries (rechargeable batteries) that rely mainly on the movement of sodium ions between the positive and negative electrodes to work, similar to the working principle of lithium-ion batteries. The electrode materials used in sodium-ion batteries are mainly sodium salts, which are more abundant and cheaper than lithium salts; therefore, sodium-ion batteries have broad application prospects in the fields of new energy storage and power. However, due to performance limitations such as energy density and cycle life, the commercialization process of sodium-ion batteries still faces great challenges.
[0003] As an important part of sodium-ion battery production, formation and volume determination directly affects the performance of the battery. Battery formation is the process of activating the internal positive and negative electrode materials through a specific charge and discharge method to improve the battery's charge and discharge performance. During the battery formation and volume determination process, exhaust is required to eliminate the gas generated by the battery during the formation process. At present, the formation and volume determination methods of sodium-ion batteries are mostly carried out with reference to the formation and volume determination methods of lithium-ion batteries. The application of lithium-ion formation and volume determination methods to sodium-ion production does not significantly improve the performance of sodium-ion batteries. Summary of the invention
[0004] The purpose of the present invention is to overcome the above problems existing in the prior art and provide a formation and volume determination process for a sodium ion short blade battery. By optimizing the formation and volume determination steps in the production of the sodium ion battery and optimizing the relevant parameters in the formation and volume determination steps, the initial capacity, charge and discharge efficiency and cycle life of the sodium ion battery can be significantly improved.
[0005] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:
[0006] A formation and volume determination process for a sodium ion short blade battery, the process comprising the following steps:
[0007] S1: Battery pre-conditioning
[0008] placing the sodium ion short blade battery at a first temperature and standing for a first time to obtain a first standing battery;
[0009] S2: Battery formation
[0010] Under the conditions of a first negative pressure and a second temperature, the first static battery is subjected to a constant current charging process to obtain a formed battery;
[0011] S3: Battery rest
[0012] leaving the formed battery at a third temperature for a second time to obtain a second left-still battery;
[0013] S4: Battery capacity setting
[0014] The second stationary battery is charged and discharged at the second negative pressure and the fourth temperature to obtain a constant-capacity battery.
[0015] Furthermore, in step S1, the first temperature is 40-60°C, and the first time is 20-30 hours.
[0016] Furthermore, in step S2, the first negative pressure is -60 to -100 Pa, and the second temperature is 40 to 60°C.
[0017] Furthermore, in step S2, the specific process of constant current charging is as follows:
[0018] S201: firstly perform constant current charging on the first static battery at a first current rate, so that the voltage of the first static battery rises to a first voltage, thereby obtaining a charged battery;
[0019] S202: performing constant current charging on the once-charged battery at a second current rate, so that the voltage of the once-charged battery rises to a second voltage, thereby obtaining a second-charged battery;
[0020] S203: Finally, the secondary charged battery is subjected to constant current charging at a third current rate, so that the voltage of the secondary charged battery is increased to a third voltage, thereby obtaining a formed battery.
[0021] Further, the first current magnification is smaller than the second current magnification, and the second current magnification is smaller than the third current magnification.
[0022] Further, the first current magnification is 0.01 to 0.05C, the second current magnification is 0.09 to 0.15C, and the third current magnification is 0.19 to 0.25C;
[0023] The first voltage is 2.8 to 3.2V, the second voltage is 3.4 to 3.8V, and the third voltage is 3.9 to 4.2V.
[0024] Further, in step S3, the third temperature is room temperature, and the second time is 40 to 60 hours;
[0025] In step S4, the second negative pressure is -60 to -100 Pa, and the fourth temperature is room temperature.
[0026] Furthermore, in step S4, the specific process of the charge and discharge process is as follows:
[0027] S401: charging the second stationary battery at a fourth current rate constant current constant voltage to a fourth voltage, to obtain a tertiary charged battery;
[0028] S402: discharging the thrice-charged battery at a fifth current rate constant current to a fifth voltage to obtain a once-discharged battery;
[0029] S403: Repeat steps S401 to S402 1 to 2 times to obtain a processed battery;
[0030] S404: charging the treated battery at a sixth current rate and constant current and constant voltage to a sixth voltage to obtain a fixed capacity battery.
[0031] Further, the fourth current multiplier is smaller than the fifth current multiplier;
[0032] The fourth current multiplier is smaller than the sixth current multiplier.
[0033] Further, the fourth current magnification is 0.20-0.40C, the fifth current magnification is 0.45-0.60C, and the sixth current magnification is 0.45-0.60C;
[0034] The fourth voltage is 4.0-4.4V, the fifth voltage is 1.8-3.0V, and the sixth voltage is 3.7-3.9V.
[0035] Compared with the prior art, the present invention has the following beneficial effects:
[0036] 1. The present invention provides a formation and capacity determination process for a sodium ion short blade battery, which significantly improves the initial capacity, charge and discharge efficiency and cycle life of the sodium ion battery by optimizing the formation and capacity determination steps and parameters.
[0037] 2. In the present invention, in the pretreatment step, the battery is allowed to stand for a period of time at a specific temperature to allow the inside of the battery to reach a stable state; in the formation step, sodium ions are gradually embedded from the positive electrode material into the negative electrode material, and the waste gas generated in this process is extracted by negative pressure, and finally a stable sodium ion embedding layer is formed; in the standing step, the battery is allowed to stand at room temperature, which helps to further optimize the embedding and de-embedding behavior of sodium ions in the positive and negative electrode materials, and improve the charge and discharge efficiency and cycle life of the battery; in the final constant volume step, it is carried out under negative pressure and room temperature conditions, so that the inside of the battery reaches a new stable state, and the waste gas is discharged by negative pressure, which can further improve the battery performance.
[0038] 3. By optimizing the sodium ion battery formation process, the present invention can significantly improve the initial capacity of the sodium ion short blade battery, and the cycle life and gas production phenomenon can also be significantly improved. DETAILED DESCRIPTION
[0039] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0040] A formation and volume determination process for a sodium ion short blade battery, the process comprising the following steps:
[0041] S1: Battery pre-conditioning
[0042] placing the sodium ion short blade battery at a first temperature and standing for a first time to obtain a first standing battery;
[0043] In step S1, the first temperature is 40-60°C, preferably 45°C;
[0044] The first time is 20 to 30 hours, preferably 24 hours;
[0045] S2: Battery formation
[0046] Under the conditions of a first negative pressure and a second temperature, the first static battery is subjected to a constant current charging process to obtain a formed battery;
[0047] In step S2, the first negative pressure is -60 to -100 Pa, preferably -75 Pa;
[0048] The second temperature is 40-60°C, preferably 45°C;
[0049] In step S2, the specific process of constant current charging is as follows:
[0050] S201: firstly perform constant current charging on the first static battery at a first current rate, so that the voltage of the first static battery rises to a first voltage, thereby obtaining a charged battery;
[0051] S202: performing constant current charging on the once-charged battery at a second current rate, so that the voltage of the once-charged battery rises to a second voltage, thereby obtaining a second-charged battery;
[0052] S203: finally, the secondary charged battery is subjected to constant current charging at a third current rate, so that the voltage of the secondary charged battery is increased to a third voltage, thereby obtaining a formed battery;
[0053] Wherein, the first current magnification is smaller than the second current magnification, and the second current magnification is smaller than the third current magnification;
[0054] The first current ratio is 0.01 to 0.05C, preferably 0.05C;
[0055] The second current ratio is 0.09 to 0.15C, preferably 0.1C;
[0056] The third current ratio is 0.19-0.25C, preferably 0.2C;
[0057] The first voltage is 2.8 to 3.2 V, preferably 3.0 V;
[0058] The second voltage is 3.4 to 3.8 V, preferably 3.5 V;
[0059] The third voltage is 3.9 to 4.2 V, preferably 3.95 V;
[0060] S3: Battery rest
[0061] leaving the formed battery at a third temperature for a second time to obtain a second left-still battery;
[0062] In step S3, the third temperature is room temperature;
[0063] The second time is 40 to 60 hours, preferably 45 hours;
[0064] S4: Battery capacity setting
[0065] At a second negative pressure and a fourth temperature, the second static battery is subjected to charge and discharge treatment to obtain a constant-capacity battery;
[0066] Wherein, in step S4, the second negative pressure is -60 to -100 Pa, preferably -75 Pa;
[0067] The fourth temperature is normal temperature;
[0068] In step S4, the specific process of charge and discharge processing is as follows:
[0069] S401: charging the second stationary battery at a fourth current rate constant current constant voltage to a fourth voltage, to obtain a tertiary charged battery;
[0070] S402: discharging the thrice-charged battery at a fifth current rate constant current to a fifth voltage to obtain a once-discharged battery;
[0071] S403: Repeat steps S401 to S402 1 to 2 times to obtain a processed battery;
[0072] S404: charging the treated battery at a sixth current rate and constant current and constant voltage to a sixth voltage to obtain a fixed capacity battery;
[0073] In the specific process of the charge and discharge process, the fourth current rate is smaller than the fifth current rate, and the fourth current rate is smaller than the sixth current rate;
[0074] Specifically, the fourth current magnification is 0.20-0.40C, preferably 0.33C;
[0075] The fifth current ratio is 0.45-0.60C, preferably 0.5C;
[0076] The sixth current ratio is 0.45-0.60C, preferably 0.5C;
[0077] The fourth voltage is 4.0-4.4V, preferably 4.2V;
[0078] The fifth voltage is 1.8-3.0V, preferably 2.0V;
[0079] The sixth voltage is 3.7-3.9V, preferably 3.85V.
[0080] The following are specific examples.
[0081] Example
[0082] The sodium-ion short blade battery was placed in a 45°C environment for 24 hours for pretreatment. Then, under the conditions of negative pressure of -75Pa and temperature of 45°C, it was first charged to 3.0V at 0.05C constant current, then charged to 3.5V at 0.1C constant current, and finally charged to 3.95V at 0.2C constant current. Then it was placed at room temperature for 48 hours. Finally, the battery was fixed at a negative pressure of -75Pa and room temperature, charged to 4.2V at 0.33C constant current and constant voltage, and then discharged to 2.0V at 0.5C constant current. After 2 cycles, it was charged to 3.85V at 0.5C constant current and constant voltage to complete the formation and fixed capacity process.
[0083] Comparative Example
[0084] The sodium-ion short blade battery was placed in a 45°C environment for 24 hours for pretreatment. Then, under negative pressure of -75Pa and temperature of 45°C, it was first charged to 3.0V at 0.05C constant current, then charged to 3.5V at 0.1C constant current, and finally charged to 3.95V at 0.2C constant current. Then it was left to stand at room temperature for 48 hours. Finally, the battery was fixed at room temperature, charged to 4.2V at 0.33C constant current and constant voltage, and then discharged to 2.0V at 0.5C constant current. After 2 cycles, it was charged to 3.85V at 0.5C constant current and constant voltage to complete the formation and fixed capacity process.
[0085] Experimental example
[0086] The sodium ion short blade batteries after the formation and constant volume process in the embodiment and the comparative example were subjected to performance tests, and the test results are shown in Table 1;
[0087] Table 1
[0088] Performance parameters Example Comparative Example Battery thickness after constant capacity 20.4mm 22.5mm Constant capacity 69Ah 65Ah Cycle life 1000 laps 80% 200 laps 80%
[0089] It can be seen from the data in Table 1 that after constant capacity, the battery thickness in the embodiment is smaller than the battery thickness in the comparative example, and its capacity and cycle life are also improved, indicating that the performance of the sodium ion short blade battery prepared by this process is improved.
[0090] Moreover, the sodium ion short blade battery prepared in the embodiment has a smooth outer surface without abnormalities; while the sodium ion short blade battery prepared in the comparative example has obvious sodium precipitation on its outer surface; this indicates that the sodium ion short blade battery prepared by the formation and constant capacity process provided by the present invention has excellent appearance.
[0091] The invention provides a formation and volume determination process for a sodium ion short blade battery. By optimizing the formation and volume determination steps in the production of the sodium ion battery and optimizing the relevant parameters in the formation and volume determination steps, the initial capacity, charge and discharge efficiency and cycle life of the sodium ion battery can be significantly improved, and the invention can be widely used in the production and manufacture of the sodium ion battery.
[0092] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0093] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.
Claims
1. A formation and volume determination process for sodium ion short blade batteries. It is characterized in that The process includes the following steps: S1: Battery pre-conditioning placing the sodium ion short blade battery at a first temperature and standing for a first time to obtain a first standing battery; S2: Battery formation Under the conditions of a first negative pressure and a second temperature, the first static battery is subjected to a constant current charging process to obtain a formed battery; S3: Battery rest leaving the formed battery at a third temperature for a second time to obtain a second left-still battery; S4: Battery capacity setting The second stationary battery is charged and discharged at the second negative pressure and the fourth temperature to obtain a constant-capacity battery.
2. A formation and volume determination process for a sodium ion short blade battery according to claim 1, It is characterized in that In step S1, the first temperature is 40-60°C, and the first time is 20-30 hours.
3. A formation and volume determination process for a sodium ion short blade battery according to claim 1, It is characterized in that In step S2, the first negative pressure is -60 to -100 Pa, and the second temperature is 40 to 60°C.
4. A formation and volume determination process for a sodium ion short blade battery according to claim 1, It is characterized in that In step S2, the specific process of constant current charging is as follows: S201: firstly perform constant current charging on the first static battery at a first current rate, so that the voltage of the first static battery rises to a first voltage, thereby obtaining a charged battery; S202: performing constant current charging on the once-charged battery at a second current rate so that the voltage of the once-charged battery rises to a second voltage, thereby obtaining a second-charged battery; S203: Finally, the secondary charged battery is subjected to constant current charging at a third current rate, so that the voltage of the secondary charged battery is increased to a third voltage, thereby obtaining a formed battery.
5. A formation and volume determination process for a sodium ion short blade battery according to claim 4, It is characterized in that The first current magnification is smaller than the second current magnification, and the second current magnification is smaller than the third current magnification.
6. A formation and volume determination process for a sodium ion short blade battery according to claim 4, It is characterized in that The first current magnification is 0.01 to 0.05C, the second current magnification is 0.09 to 0.15C, and the third current magnification is 0.19 to 0.25C; The first voltage is 2.8 to 3.2V, the second voltage is 3.4 to 3.8V, and the third voltage is 3.9 to 4.2V.
7. A formation and volume determination process for a sodium ion short blade battery according to claim 1, It is characterized in that In step S3, the third temperature is room temperature, and the second time is 40 to 60 hours; In step S4, the second negative pressure is -60 to -100 Pa, and the fourth temperature is room temperature.
8. A formation and volume determination process for a sodium ion short blade battery according to claim 1, It is characterized in that In step S4, the specific process of charge and discharge processing is as follows: S401: charging the second stationary battery at a fourth current rate constant current constant voltage to a fourth voltage, to obtain a tertiary charged battery; S402: discharging the thrice-charged battery at a fifth current rate constant current to a fifth voltage to obtain a once-discharged battery; S403: Repeat steps S401 to S402 1 to 2 times to obtain a processed battery; S404: charging the treated battery at a sixth current rate and constant current and constant voltage to a sixth voltage to obtain a fixed capacity battery.
9. A formation and volume determination process for a sodium ion short blade battery according to claim 8, It is characterized in that The fourth current multiplier is smaller than the fifth current multiplier; The fourth current multiplier is smaller than the sixth current multiplier.
10. A formation and volume determination process for a sodium ion short blade battery according to claim 8, It is characterized in that The fourth current magnification is 0.20-0.40C, the fifth current magnification is 0.45-0.60C, and the sixth current magnification is 0.45-0.60C; The fourth voltage is 4.0-4.4V, the fifth voltage is 1.8-3.0V, and the sixth voltage is 3.7-3.9V.
Citation Information
Patent Citations
Formation method of sodium ion battery and sodium ion battery
CN116565358A
Sodium ion battery formation method
CN117154259A
Preparation method of sodium ion battery
CN117199502A
Formation method of sodium ion battery and sodium ion battery
CN118054108A
Formation method of sodium ion battery
CN118099572A