High-heat-resistance lithium ion battery diaphragm and preparation method thereof

By using a combination of biomass cellulose ester and inorganic ceramic particles, combined with multi-stage solidification bath and non-solvent phase conversion method, the problems of insufficient heat resistance and high preparation cost of lithium-ion battery separators are solved, and high efficiency and low cost are achieved The high heat-resistant membrane preparation improves the safety performance and production efficiency of the battery.

CN118920014APending Publication Date: 2024-11-08HEFEI GUOXUAN HIGH TECH POWER ENERGY
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410975284.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing lithium-ion battery separators have insufficient heat resistance temperature and cannot meet the requirements of modern 3C products and power batteries. The high preparation cost and complex process of high heat resistance separators lead to industrialization obstacles.

Method used

Biomass cellulose ester is used as the separator material, and the separator coating solution is prepared by adding inorganic ceramic particles to the solution, and the pore-making and non-solvent phase conversion method is used to simplify the process and reduce costs.

Benefits of technology

The prepared separator has extremely low heat shrinkage, which improves the safety performance and production efficiency of the battery, reduces the production cost, and achieves high heat resistance and efficient production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118920014A_ABST
    Figure CN118920014A_ABST
Patent Text Reader

Abstract

The invention provides a high-heat-resistance lithium ion battery diaphragm and a preparation method thereof, and belongs to the technical field of lithium ion battery diaphragm materials. The preparation method comprises the following steps: preparing a first solution from biomass cellulose ester as a solute and a mixed solvent; adding inorganic ceramic particles into the first solution to prepare a second solution; adding a pore-forming agent, a viscosity modifier, a surfactant and / or a defoaming agent into the second solution to prepare a diaphragm coating solution; unwinding and coating the diaphragm coating liquid on a diaphragm base membrane to form a wet membrane; preparing a multi-stage coagulating bath, and extracting and pore-forming the wet film; and drying and rolling the wet film containing the poor solvent. According to the invention, the biomass polymer material with excellent heat resistance is selected as the diaphragm material, the source is wide, the cost is low, and the heat resistance is excellent; a non-solvent phase conversion method is adopted for pore forming, so that the production efficiency of the high-heat-resistance diaphragm is improved; and the prepared cellulose ester-based diaphragm is uniform in pore size and excellent in performance under high-rate and fast-charging conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium ion battery diaphragm materials, and in particular relates to a high heat-resistant lithium ion battery diaphragm and a preparation method thereof. Background Art

[0002] Since the 1990s, when Sony first commercialized lithium-ion batteries, lithium-ion batteries and lithium-ion power batteries have been used as the power source for new energy electric vehicles and play a role in driving vehicles. They are the core technologies of one of the "three electric (motor, electronic control and battery)" technologies. The four main materials of lithium-ion batteries include positive electrode, negative electrode, diaphragm and electrolyte. The diaphragm plays a key role in isolating positive and negative electrodes and transmitting lithium ions in lithium-ion batteries. It occupies an important position in lithium-ion batteries. Its physical and chemical properties and comprehensive cost are extremely important considerations for lithium-ion batteries. At present, the main commercial diaphragms are polyolefin diaphragms, including polyethylene (PE) and polypropylene (PP). The heat resistance temperature of polyolefin diaphragms is low. For example, the thermal deformation temperature of PE diaphragms is 80-100℃, the glass transition temperature is 135-140℃, and the thermal deformation temperature of PP diaphragms is about 100℃, the glass transition temperature is about 160℃, and its safety boundary temperature is generally below 170℃, which makes traditional polyolefin diaphragms unable to meet the use requirements of today's 3C products and power batteries. There is an urgent need to develop lithium battery separators with higher service temperatures.

[0003] The preparation of traditional high heat-resistant lithium battery separators includes high heat-resistant separator base films and coated high heat-resistant battery separators. Existing high heat-resistant base films include polyethylene terephthalate (PET), polyimide (PI), meta-aramid (PMIA), etc. However, due to the difficulty in synthesis, the complex pore-making process for preparing micropores with suitable pore sizes, the high difficulty of processing technology, and the high cost, these high heat-resistant separator base films have not been industrialized on a large scale. The coated high heat-resistant battery separator is based on a polyolefin separator base film and coated with a layer of meta-aramid, para-aramid, PVDF (polyvinylidene fluoride) organic material or ceramic (alumina, boehmite, etc.) inorganic material. The synthesis process of organic materials such as aramid and PVDF is complex and the process is long, and the price of raw materials is high. It is expensive, costing up to hundreds of thousands per ton, and the polymer has poor solubility. The dissolution process is time-consuming and power-consuming. After the solution is coated, it needs to go through a pore-making process to make the coating have a uniform and appropriate pore structure. Otherwise, the organic coating solution will cause the diaphragm to be blocked and cannot be used. The coating process of organic materials is long and the raw materials are expensive, resulting in high costs for the organic material coating process, which obviously hinders large-scale industrialization. Ceramic material coating diaphragms is currently a more commonly used modification method, but at the same time, the adhesion between ceramics and diaphragms is small, and they are easy to shed and fall off, and the bonding strength with the positive and negative electrodes is weak, resulting in the electrode and diaphragm not being completely close, which increases the lithium ion transmission distance. In view of the problems of the above two solutions, the development of a new type of high-temperature resistant diaphragm is particularly necessary. Summary of the invention

[0004] In the preparation process of high heat-resistant lithium-ion battery separators, it is necessary to comprehensively consider the process difficulty, production cost, and the best performance that can be achieved. The present invention provides a high heat-resistant lithium-ion battery separator and a preparation method thereof, which can effectively reduce the preparation cost of the high heat-resistant separator. At the same time, the lithium-ion battery separator provided by the present invention has an extremely low heat shrinkage rate at high temperatures. The separator adopts biomass polymer materials, which can improve the safety performance of the battery; and can increase the wettability of the surface, shorten the wetting time, and effectively improve the battery capacity and improve the safety performance of the battery under extreme heat conditions, solving the problems of high cost and difficult dissolution of slurry of traditional coated high temperature resistant separators. In order to achieve the above purpose, the present invention provides the following technical solutions:

[0005] In one aspect of the present invention, a method for preparing a high heat-resistant lithium-ion battery separator is provided, comprising the following steps:

[0006] The biomass cellulose ester is used as a solute and a mixed solvent is prepared into a first solution;

[0007] adding inorganic ceramic particles into the first solution to prepare a second solution;

[0008] Add a pore former, a viscosity regulator, a surfactant, and / or an antifoaming agent to the second solution to prepare a diaphragm coating solution;

[0009] Unwind and coat the diaphragm coating solution on the diaphragm base film to form a wet film;

[0010] Prepare a multi-stage coagulation bath to extract pores from the wet film;

[0011] Dry and wind up the wet film containing a poor solvent.

[0012] Furthermore, the biomass cellulose ester includes one of cellulose diacetate, cellulose triacetate, cellulose acetate propionate, cellulose acetate butyrate, cellulose propionate butyrate, cellulose propionate, cellulose butyrate, or cellulose benzoate;

[0013] The present invention selects a biomass polymer material with extremely excellent heat resistance as the diaphragm material. Its raw material, cellulose, is the most abundant resource in nature, with a wide source. Compared with synthetic high-heat-resistant materials, it has a low cost. In cellulose and its derivatives, due to the semi-rigid six-membered ring structure, which contains a large number of hydrogen bonds, its glass transition temperature and melting point are extremely high. Moreover, as the most abundant resource in nature, it has a wide source. Compared with synthetic high-heat-resistant materials, it has a low cost and can be used as an alternative material for high-heat-resistant materials. Pure cellulose is difficult to dissolve due to its too strong hydrogen bonds. However, after esterifying it with acid anhydride, biomass cellulose esters are formed, including cellulose diacetate, cellulose triacetate, cellulose acetate propionate, cellulose acetate butyrate, cellulose propionate butyrate, cellulose propionate, cellulose butyrate, cellulose benzoate, etc. The hydroxyl groups of the biomass cellulose ester are greatly reduced. At the same time, side groups such as acetyl, propionyl, butyryl, and benzoyl groups increase the distance between the cellulose main chains, weakening the hydrogen bond interaction. Under the normal temperature conditions in the laboratory, it can be dissolved using common ordinary solvents. Among them, side groups such as acetyl and propionyl with smaller side groups are preferred. Larger side chain groups will lead to a decrease in the regularity of the molecular chain, and thus the heat resistance of the material will drop sharply. There are three substitution sites on each six-membered sugar ring of the main chain. If all are substituted, the degree of substitution (DS) is 3. If only partially substituted, then 0 < DS < 3. When DS is close to 0, it is close to the structure of cellulose; when the degree of substitution is close to 3, it is close to the fully substituted cellulose ester. At this time, the molecular chain regularity is the best, the heat resistance is good, and the hydroxyl group content is low, and the water absorption of the material is small;

[0014] The biomass cellulose ester of the present invention preferably is cellulose triacetate, and the degree of substitution is preferably 2.8 < DS < 3, more preferably 2.9 < DS < 3, most preferably 2.95 < DS < 3, and most preferably 2.98 ≤ DS < 3. Its glass transition temperature is greater than 220 °C, and the melting point is close to 300 °C, showing excellent thermal properties.

[0015] Furthermore, the mass ratio of the solute to the mixed solvent is 5% to 15%;

[0016] The mixed solvent includes a good solvent and a poor solvent, and the poor solvent accounts for 0% to 10% of the mixed solvent.

[0017] Furthermore, the amount of the inorganic ceramic particles added is 0% to 20% of the second solution.

[0018] Furthermore, the good solvent includes a chlorine-based good solvent and a non-chlorine-based good solvent;

[0019] The chlorine-based good solvent includes dichloromethane or chloroform; the non-chlorine-based good solvent includes ethyl formate, propyl formate, pentyl formate, methyl acetate, ethyl acetate, pentyl acetate, acetone, methyl ethyl ketone, diethyl ketone, diisopropyl ether or tetrahydrofuran;

[0020] The poor solvent includes methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, tert-butanol, 1-pentanol or 2-methyl-2-butanol or cyclohexanol;

[0021] The boiling point of the poor solvent is 50 to 120°C, more preferably less than 90°C.

[0022] Further, the inorganic ceramic particles include aluminum oxide (Al2O3, including α, β and γ types), boehmite (AlOOH), silicon oxide (SiO2), titanium dioxide (TiO2, rutile or anatase), magnesium oxide (MgO), magnesium hydroxide (Mg(OH)2), zirconium oxide (ZrO2), barium sulfate (BaSO4), barium oxide (BaO), copper oxide (CuO), lithium aluminate (LiAlO2), zirconium oxide (ZrO2), boron nitride (BN), silicon carbide (SiC), silicon nitride (Si3N4), tungsten carbide (WC), boron carbide (BC), aluminum nitride (AlN), iron oxide (Fe2O3), barium titanate (BaTiO3), molybdenum disulfide (MoS2), vanadium pentoxide (α-V2O5), lead titanate (PbTiO3), titanium diboride (TiB2), calcium silicate (CaSiO3), molecular sieve (ZSM-5), clay or kaolin;

[0023] From the perspective of cost, the inorganic ceramic of the present invention is preferably α-alumina with good chemical stability, high purity and uniform particle size distribution; the average particle size of the inorganic ceramic is 0.1nm to 5μm, more preferably 50nm to 0.9μm.

[0024] Further, the viscosity modifier includes one or a combination of ethanol, N,N-dimethylacetamide, dimethyl carbonate, and diphenyl carbonate;

[0025] The surfactant includes one or a combination of fluorocarbon surfactants, nonionic surfactants, cationic surfactants, anionic surfactants (perfluoroalkyl ether alcohol amine salts, perfluoroalkyl ether quaternary ammonium salts, perfluoroalkyl ether carboxylic acid potassium fluorocarbon surfactants and polyethylene glycol type, polyol type, block copolyether, special polyether nonionic surfactants);

[0026] The defoaming agent comprises one or a combination of diethylhexanol, n-octanol, isooctyl alcohol or isoamyl alcohol;

[0027] The pore-forming agent includes any one of polyethylene glycol, dimethyl carbonate, dibutyl phthalate, petroleum ether, polyvinyl pyrrolidone and polyvinyl alcohol.

[0028] Furthermore, the coating method is selected from one of a roller coating process, a spray coating process, a dip coating process, and an extrusion coating process, and the coating layer is selected from one of a single-layer coating or a double-layer coating, as long as the ultimate beneficial effect of the present invention can be achieved;

[0029] The coating layer density is 1 to 6 g / m 2 , preferably 1.5 to 3 g / m 2 ;

[0030] The base film has a thickness of 5 to 15 μm, preferably 7 to 12 μm;

[0031] The base film comprises a polyethylene base film or a polypropylene base film;

[0032] The wet thickness of the coating is 3 to 15 μm, preferably 4 to 12 μm; the dry thickness of the coating is 1 to 5 μm, preferably 2 to 4 μm.

[0033] The cellulose ester-based diaphragm prepared by the present invention has uniform pore size, and the porosity, air permeability and wettability have reached or exceeded the level of commercial polyolefin diaphragms, and has obvious physical property advantages. After being assembled into a battery, it can reduce the time required for the liquid injection and formation steps in the battery manufacturing process, and improve the production efficiency of lithium-ion batteries. The diaphragm prepared by this method has a larger pore size than the polyolefin diaphragm, at the order of hundreds of nanometers, while the polyolefin diaphragm is at the order of tens of nanometers. Its performance under high-rate fast charging (greater than 3C) conditions may be even better.

[0034] Furthermore, the number of stages of the multi-stage coagulation bath is 3 to 7, specifically 3, 4, 5, 6 or 7;

[0035] The multi-stage coagulation bath is prepared with a good solvent and a poor solvent in a proportional gradient, wherein the proportion of the good solvent decreases as the number of stages increases, and the proportion of the poor solvent increases as the number of stages increases; wherein the poor solvent and the good solvent should be completely miscible, and the boiling point of the poor solvent should be relatively low, so as to facilitate the subsequent volatilization and drying step to remove the poor solvent, and the boiling point of the poor solvent is preferably less than 120°C, more preferably less than 90°C.

[0036] Furthermore, during the extraction process, the wet film is subjected to a relatively long time in the first coagulation bath, preferably greater than 5 minutes, and most of the solvent in the coating is removed by solvent exchange. The coagulation bath times of each stage after the second stage may be equal or decrease, and the time is preferably less than 60 to 150 seconds, and more preferably less than 60 to 120 seconds.

[0037] The present invention adopts a non-solvent phase conversion method to form pores. After the coating film-forming slurry is coated on the base film, it can be supported by the substrate and continuously pass through a multi-stage coagulation bath to form pores. The coating and pore forming can be a continuous process. The preparation process is simple and the production process is efficient, which is conducive to improving the production efficiency of high heat-resistant diaphragms and increasing the added value of products.

[0038] Furthermore, the drying method is selected from one of hot air drying, infrared heating drying, and microwave drying; the drying temperature is selected near the boiling point of the poor solvent (50-120°C).

[0039] Another aspect of the present invention provides a high heat-resistant lithium-ion battery separator, which is prepared by the above preparation method. Compared with the prior art, the present invention has the following beneficial effects:

[0040] (1) The present invention selects biomass polymer materials with excellent heat resistance as the diaphragm material. The raw material cellulose is the most abundant resource in nature and has a wide range of sources. Compared with synthetic high-heat-resistant materials, it is low in cost. The diaphragm prepared from this material has excellent heat resistance and very little thermal shrinkage at high temperatures.

[0041] (2) The cellulose ester-based diaphragm prepared by the present invention has uniform pore size, and its porosity, air permeability and wettability have reached or exceeded the level of commercial polyolefin diaphragms. It can reduce the time required for the liquid injection and formation steps in the battery manufacturing process, improve the production efficiency of lithium-ion batteries, and perform better under high-rate fast charging conditions.

[0042] (3) The present invention adopts a non-solvent phase conversion method to form pores. Coating and pore formation can be a continuous process. The preparation process is simple, which is conducive to improving the production efficiency of high-heat-resistant diaphragms and increasing the added value of products. There is currently no precedent for using such a method to prepare cellulose-based diaphragms. The present invention is original.

[0043] Other features and advantages of the present invention will be described in the following description, and partly become obvious from the description, or be understood by implementing the present invention. The purpose and other advantages of the present invention can be realized and obtained by the structures pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 A schematic diagram of the steps for preparing the lithium-ion battery separator provided by the present invention;

[0045] Figure 2 The following are scanning electron microscope (SEM) photos of the surfaces of the diaphragms prepared in the embodiments and comparative examples provided by the present invention. DETAILED DESCRIPTION

[0046] In order to make the purpose, technical scheme and advantages of the present invention clearer, the implementation scheme of the present application will be described in detail below in conjunction with specific examples. The technical terms and scientific terms used in the present invention have the meanings generally understood by ordinary technicians in the technical field to which the present invention belongs, without other definitions. Without departing from the concept of the present invention, those skilled in the art may make various improvements and changes to the specific implementation methods of the present invention specification, which all belong to the protection scope of the present invention. The raw materials involved in the following content can be obtained from commercial channels unless otherwise specified.

[0047] Figure 1 The schematic diagram of the preparation steps of the lithium ion battery separator provided by the present invention shows the following embodiments in combination with the preparation steps:

[0048] Example 1

[0049] A high heat-resistant lithium-ion battery separator and a preparation method thereof, comprising the following steps:

[0050] Step 1: prepare the first solution. The biomass cellulose ester selected in Example 1 is cellulose triacetate with an acetyl substitution degree of 2.98 (DS=2.98). The solvent of the first solution is composed of a mixture of a good solvent and a poor solvent. The good solvent is dichloromethane, a chlorine-based good solvent, and the poor solvent is methanol. The mass ratio of dichloromethane to methanol is 95:5. According to the calculated slurry solid content, weigh cellulose triacetate, and add dichloromethane and methanol, wherein the cellulose triacetate accounts for 8% of the solution mass. The dissolution temperature is preferably 30°C, the stirring rate is 200rpm, and the stirring is for more than 5h. The sealing of the dissolving kettle is good. Under the above conditions, stir and mix to form the first solution.

[0051] Step 2: Prepare the second solution, add α-alumina powder into a sand mill and grind it to reduce its particle size, grind its size range to 0.1 to 0.9 μm, weigh the sand-ground slurry in proportion and add it to the first solution in step 1, the mass of alumina accounts for 16% of the solution, stir at a rate of 200 rpm, control the mixing temperature at 30°C, and stir and mix for more than 2 hours to form the second solution.

[0052] Step 3: Prepare the diaphragm coating liquid. Add a certain amount of pore-forming agent, viscosity regulator and surfactant to the second solution prepared in step 2. The addition ratio is shown in Table 1 (CA is biomass cellulose ester). The mass of the pore-forming agent accounts for 5% of the biomass cellulose ester, the viscosity regulator accounts for 0.5% of the coating liquid, and the surfactant accounts for 0.2% of the coating liquid. The pore-forming agent is preferably a low molecular weight polyethylene glycol, the viscosity regulator is preferably NN-dimethylacetamide, and the surfactant is preferably a polyol type. Mix and stir for 2 hours, then let it stand for 2 hours to defoam, and the diaphragm coating liquid is prepared.

[0053] Step 4: Unwinding and coating: The membrane coating liquid prepared in step 3 is evenly coated on both sides of the wet polyethylene base film by double-sided roller coating. The polyethylene base film thickness is 9 μm and the coating surface density is 2.2 g / m 2 The coating wet thickness is 8 μm, the coating dry thickness is 1.5 μm, and the coating vehicle speed is preferably greater than 40 m / min. In this embodiment, the coating vehicle speed is 45 m / min.

[0054] Step 5: Multi-stage extraction and pore making, prepare a multi-stage coagulation bath. The coagulation bath can be prepared according to the gradient ratio of good solvent and poor solvent. The good solvent of the coagulation bath is dichloromethane, and the poor solvent of the coagulation bath is ethanol. The boiling point of dichloromethane is 39.8°C, and the boiling point of ethanol is 78°C. The boiling points of both are lower than 80°C, which is convenient for subsequent drying. In this embodiment, four coagulation baths are prepared: the first stage, dichloromethane: ethanol = 70:30; the second stage, dichloromethane: ethanol = 40:60; the third stage, dichloromethane: ethanol = 10:90; the fourth stage, dichloromethane: ethanol = 0:100; after the wet film prepared in step 4 is coated, it can enter the four coagulation baths in sequence, the first stage coagulation bath residence time is 10min; the second stage coagulation bath residence time is 100s; the third stage coagulation bath residence time is 100s; the fourth stage coagulation bath residence time is 60s; in this process, ethanol continuously diffuses into the coating, and dichloromethane continuously diffuses into the coagulation bath, and the cellulose triacetate in the coating will undergo uneven phase separation. After the four-stage coagulation bath, the solvent exchange process is basically completed, and finally a two-phase region of pores and a polymer containing a poor solvent is formed, and from Figure 2 The electron microscope photograph shows that the micropores are distributed very evenly.

[0055] Step 6: Drying and rolling up. The wet film containing the poor solvent in step 5 is dried with hot air at a drying temperature of 50° C. for 80 seconds. After drying, the coated diaphragm is rolled up to complete the preparation.

[0056] Example 2

[0057] Step 1: prepare the first solution. The biomass cellulose ester selected in Example 2 is cellulose triacetate with an acetyl substitution degree of 2.98 (DS=2.98). The first solution is composed of a mixture of a good solvent and a poor solvent. The good solvent is dichloromethane, a chlorine-based good solvent, and the poor solvent is methanol. The mass ratio of dichloromethane to methanol is 95:5. According to the calculated slurry solid content, a certain mass of cellulose triacetate is weighed, and a certain volume of dichloromethane and methanol are added. The cellulose triacetate accounts for 8% of the total coating liquid mass. The dissolution temperature is preferably 30°C, the stirring rate is 200rpm, and the stirring is for more than 5h. The sealing of the dissolving kettle is good. Under the above conditions, the mixture is stirred and mixed into the first solution.

[0058] Step 2: In this step, the second solution is prepared without using inorganic ceramic particles.

[0059] Step 3: Prepare the diaphragm coating liquid. Add a certain amount of pore-forming agent, viscosity regulator and surfactant to the first solution prepared in step 1. The addition ratio is shown in Table 1. The mass of the pore-forming agent accounts for 8% of the biomass cellulose ester, the viscosity regulator accounts for 0.3% of the coating liquid, and the surfactant accounts for 0.24% of the coating liquid. The pore-forming agent is preferably a low molecular weight polyethylene glycol, the viscosity regulator is preferably NN-dimethylacetamide, and the surfactant is preferably a polyol type. Mix and stir for 2 hours, then let it stand for 2 hours to defoam, and the diaphragm coating liquid is prepared.

[0060] Step 4: Unwinding and coating: The membrane coating liquid prepared in step 3 is evenly coated on both sides of the wet polyethylene base film by double-sided roller coating. The polyethylene base film thickness is 9 μm and the coating surface density is 1.2 g / m 2 The coating wet thickness is 8 μm, the coating dry thickness is 1.5 μm, and the coating vehicle speed is preferably greater than 40 m / min. In this embodiment, the coating vehicle speed is 45 m / min.

[0061] Step 5: Multi-stage extraction pore formation, preparing a multi-stage coagulation bath. The coagulation bath can be prepared according to the gradient ratio of the good solvent and the poor solvent. The good solvent of the coagulation bath is selected from dichloromethane, and the poor solvent of the coagulation bath is selected from ethanol. The boiling point of dichloromethane is 39.8°C, and the boiling point of ethanol is 78°C. Both boiling points are lower than 80°C, which is convenient for subsequent drying. In this embodiment, a 4-stage coagulation bath is prepared: the first stage, dichloromethane: ethanol = 70:30; the second stage, dichloromethane: ethanol = 40:60; the third stage, dichloromethane: ethanol = 10:90; the fourth stage, dichloromethane: ethanol = 0:100; after the wet film prepared in step 3 is coated, it can enter the four-stage coagulation bath in sequence, the first-stage coagulation bath residence time is 10min; the second-stage coagulation bath residence time is 100s; the third-stage coagulation bath residence time is 100s; the fourth-stage coagulation bath residence time is 60s; in this process, ethanol continuously diffuses into the coating, and dichloromethane continuously diffuses into the coagulation bath, and the cellulose triacetate in the coating will undergo uneven phase separation. After the four-stage coagulation bath, the solvent exchange process is basically completed, and finally a two-phase region of pores and a polymer containing a poor solvent is formed, and from Figure 2 The electron microscope photograph shows that the micropores are distributed very evenly.

[0062] Step 6: Drying and rolling up. The wet film containing the poor solvent in step 5 is dried with hot air at a drying temperature of 50° C. for 80 seconds. After drying, the coated diaphragm is rolled up to complete the preparation.

[0063] Example 3

[0064] Step 1: prepare the first solution. The biomass cellulose ester selected in Example 3 is cellulose triacetate with an acetyl substitution degree of 2.98 (DS=2.98). The first solution is composed of a mixture of a good solvent and a poor solvent. The good solvent is dichloromethane, a chlorine-based good solvent, and the poor solvent is methanol. The mass ratio of dichloromethane to methanol is 95:5. According to the calculated slurry solid content, a certain mass of cellulose triacetate is weighed, and a certain volume of dichloromethane and methanol are added. The cellulose triacetate accounts for 8% of the total coating liquid mass. The dissolution temperature is preferably 30°C, the stirring rate is 200rpm, and the stirring is for more than 5h. The sealing of the dissolving kettle is good. Under the above conditions, the mixture is stirred and mixed into the first solution.

[0065] Step 2: Prepare the second solution, add α-alumina powder into a sand mill and grind it to reduce its particle size, grind its size range to 0.1 to 0.9 μm, weigh the sand-ground slurry according to proportion and add it to the first solution in step 1, the mass of alumina accounts for 8% of the total coating liquid, stir at a rate of 200 rpm, control the mixing temperature at 30°C, and stir and mix for more than 2 hours to form the second solution.

[0066] Step 3: Prepare the diaphragm coating liquid. Add a certain amount of pore-forming agent, viscosity regulator and surfactant to the second solution prepared in step 2. The addition ratio is shown in Table 1. The mass of the pore-forming agent accounts for 5% of the biomass cellulose ester, the viscosity regulator accounts for 0.2% of the coating liquid, and the surfactant accounts for 0.2% of the coating liquid. The pore-forming agent is preferably a low molecular weight polyethylene glycol, the viscosity regulator is preferably NN-dimethylacetamide, and the surfactant is preferably a polyol type. Mix and stir for 2 hours, then let it stand for 2 hours to defoam, and the diaphragm coating liquid is prepared.

[0067] Step 4: Unwinding and coating: The membrane coating liquid prepared in step 3 is evenly coated on both sides of the wet polyethylene base film by double-sided roller coating. The polyethylene base film thickness is 9 μm and the coating surface density is 1.8 g / m 2 The coating wet thickness is 8 μm, the coating dry thickness is 1.5 μm, and the coating vehicle speed is preferably greater than 40 m / min. In this embodiment, the coating vehicle speed is 45 m / min.

[0068] Step 5: Multi-stage extraction pore formation, preparing a multi-stage coagulation bath, the coagulation bath can be prepared according to the gradient ratio of good solvent and poor solvent, the good solvent of the coagulation bath is selected from dichloromethane, and the poor solvent of the coagulation bath is selected from ethanol, the boiling point of dichloromethane is 39.8°C, and the boiling point of ethanol is 78°C, both of which are lower than 80°C, which is convenient for subsequent drying. In this embodiment, a 4-stage coagulation bath is prepared: the first stage, dichloromethane: ethanol = 70:30; the second stage, dichloromethane: ethanol = 40:60; the third stage, dichloromethane: ethanol = 10:90; the fourth stage, dichloromethane: ethanol Alcohol = 0:100; after the wet film prepared in step 4 is coated, it can enter the four-stage coagulation bath in sequence, the first-stage coagulation bath residence time is 10min; the second-stage coagulation bath residence time is 100s; the third-stage coagulation bath residence time is 100s; the fourth-stage coagulation bath residence time is 60s; in this process, ethanol continuously diffuses into the coating, dichloromethane continuously diffuses into the coagulation bath, and the cellulose triacetate in the coating will undergo uneven phase separation. After the four-stage coagulation bath, the solvent exchange process is basically completed, and finally a two-phase region of pores and a polymer containing a poor solvent is formed.

[0069] Step 6: Drying and rolling up. The wet film containing the poor solvent in step 5 is dried by hot air at a drying temperature of 50° C. for 80 seconds. After drying, the coated diaphragm is rolled up to complete the preparation.

[0070] Example 4

[0071] In this embodiment, biomass cellulose ester is not used to prepare the first solution;

[0072] Preparation of coating liquid: Add α-alumina powder to a sand mill to reduce its particle size, and grind its size range to 0.1 to 0.9 μm. Weigh the sand-ground slurry in proportion and add it to deionized water. Add a certain proportion of viscosity regulator and surfactant, wherein the content of alumina accounts for 16% of the coating slurry, the viscosity regulator accounts for 0.15% of the coating liquid, and the surfactant accounts for 0.32% of the coating liquid. Adjust the overall viscosity of the slurry to between 300 and 600 mPa·s. After the slurry is prepared, let it stand for 2 hours to defoam. Figure 2 Uniform and clear micropores can be seen in the electron microscope photograph. This embodiment does not require multi-stage extraction to form pores, because the inorganic coating used to prepare the coating liquid is granular in itself and naturally forms pores during the accumulation process. Examples 1-3 are organic coatings and therefore require pore formation.

[0073] Coating and drying: The prepared diaphragm coating slurry is applied to the surface of the diaphragm base film by roller coating. The thickness of the polyethylene base film is 9μm and double-sided coating is performed. After coating, hot air drying is performed at a drying temperature of 60°C and a drying time of 3 minutes. The final dry thickness of the coating is 1.5μm on both sides.

[0074] Comparative Example 1 is a commercial wet-process biaxially oriented polyethylene diaphragm, and the thickness of the polyethylene diaphragm is 9 μm.

[0075] Comparative Example 2 is a dry-stretched polypropylene diaphragm, and the thickness of the polypropylene diaphragm is 12 μm.

[0076] The formulation parameters of the membrane coating liquid of Examples 1-4 and Comparative Examples 1-2 are shown in Table 1 (CA is cellulose triacetate):

[0077] Table 1 Coating liquid formula

[0078]

[0079] The high temperature heat shrinkage performance and interface performance test data of Examples 1-4 and Comparative Examples 1-2 are shown in Table 2 (MD longitudinal direction, TD transverse direction):

[0080] Table 2 High temperature heat shrinkage and interface properties of examples and comparative examples

[0081]

[0082] It can be seen from Table 2 that the thermal shrinkage of the polyethylene-based film and the polypropylene-based film in Comparative Examples 1 and 2 at 150°C is already relatively large. The melting point of ultra-high molecular weight polyethylene is about 138°C, and that of polypropylene is about 165°C. They are both in a molten state at 180°C and have no mechanical strength. The diaphragm coated only with α-alumina in Example 4 can greatly reduce its thermal shrinkage at 130°C and 150°C compared to Comparative Examples 1 and 2, but there is no bonding effect between the alumina particles. At higher temperatures such as 180°C, the diaphragm will pulverize and break. Only the diaphragm with the composite coating (Example 1 and Example 3) and the diaphragm coated with biomass cellulose ester alone (Example 2) can still maintain the diaphragm morphology at high temperatures, and have a small thermal shrinkage. Among them, the composite coating diaphragm (Example 1 and Example 3) has a better effect, and the composite coating diaphragm with a higher alumina ratio (Example 1) is particularly excellent. In terms of interface performance, polyethylene and polypropylene separators are formed by polymerization of non-polar monomers, and their interfaces are generally hydrophobic, with a large electrolyte contact angle of 50°. However, due to the presence of some hydroxyl groups in biomass cellulose triacetate and α-alumina, their hydrophilicity is greatly improved, and the electrolyte contact angle in Examples 1-3 is reduced to 12-13°, indicating that the separator has excellent electrolyte wettability in the subsequent battery assembly process, effectively shortening the electrolyte infiltration time and reducing the time required for battery injection and formation. In addition, the density of biomass cellulose triacetate (1.29 g / cm 3 ) is much smaller than inorganic ceramic materials (such as α-alumina, with a density of 3.9 g / cm 3 ) density, so for the same volume of diaphragm, the mass of the diaphragm using cellulose triacetate organic coating or organic-inorganic composite coating is much smaller than the mass of the diaphragm coated with inorganic materials. The use of organic coating or composite coating diaphragm to assemble into a battery will greatly improve the unit energy density of the battery. In summary, the preparation method of the present invention can reduce the preparation cost of high heat-resistant diaphragms. At the same time, the lithium-ion battery diaphragm provided by the present invention has an extremely low thermal shrinkage rate at high temperatures, which can improve the safety performance of the battery; and can increase the wettability of the surface, which can shorten the wetting time; due to the significant density difference between organic materials and inorganic materials, the use of the battery of the present invention can effectively improve the battery energy density.

[0083] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a highly heat-resistant lithium-ion battery separator, It is characterized in that The following steps are involved: The biomass cellulose ester is used as a solute and a mixed solvent is prepared into a first solution; adding inorganic ceramic particles into the first solution to prepare a second solution; Adding a pore former, a viscosity modifier, a surfactant and / or a defoaming agent to the second solution to prepare a diaphragm coating liquid; Unwinding the diaphragm coating liquid and applying it on the diaphragm base film to form a wet film; Prepare multi-stage coagulation bath to extract pores in wet membrane; The wet film containing the poor solvent is dried and rolled up.

2. A method for preparing a high heat-resistant lithium-ion battery separator according to claim 1, It is characterized in that The biomass cellulose ester includes one of cellulose diacetate, cellulose triacetate, cellulose acetate propionate, cellulose acetate butyrate, cellulose propionate butyrate, cellulose propionate, cellulose butyrate or cellulose benzoate, and the degree of substitution is 0 <DS<3。 3. The method for preparing a highly heat-resistant lithium-ion battery separator according to claim 1, It is characterized in that The mass ratio of the solute to the mixed solvent is 5% to 15%; The mixed solvent includes a good solvent and a poor solvent, and the poor solvent accounts for 0% to 10% of the mixed solvent.

4. The method for preparing a high heat-resistant lithium-ion battery separator according to claim 1, It is characterized in that The added amount of the inorganic ceramic particles accounts for 0% to 20% of the second solution.

5. The method for preparing a highly heat-resistant lithium-ion battery separator according to claim 3, It is characterized in that The good solvent includes a chlorine-based good solvent and a non-chlorine-based good solvent.

6. A method for preparing a high heat-resistant lithium-ion battery separator according to claim 5, It is characterized in that The chlorine-based good solvent includes dichloromethane or chloroform; the non-chlorine-based good solvent includes ethyl formate, propyl formate, pentyl formate, methyl acetate, ethyl acetate, pentyl acetate, acetone, methyl ethyl ketone, diethyl ketone, diisopropyl ether or tetrahydrofuran.

7. The method for preparing a highly heat-resistant lithium-ion battery separator according to claim 3, It is characterized in that The poor solvent includes methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, tert-butanol, 1-pentanol or 2-methyl-2-butanol or cyclohexanol.

8. The method for preparing a high heat-resistant lithium-ion battery separator according to claim 1, It is characterized in that The inorganic ceramic particles include one or more of aluminum oxide, boehmite, silicon oxide, titanium dioxide, magnesium oxide, magnesium hydroxide, zirconium oxide, barium sulfate, barium oxide, copper oxide, lithium aluminate, zirconium oxide, boron nitride, silicon carbide, silicon nitride, tungsten carbide, boron carbide, aluminum nitride, iron oxide, barium titanate, molybdenum disulfide, vanadium pentoxide, lead titanate, titanium diboride, calcium silicate, molecular sieves, clay or kaolin.

9. The method for preparing a high heat-resistant lithium-ion battery separator according to claim 1, It is characterized in that The viscosity modifier includes one or a combination of ethanol, N,N-dimethylacetamide, dimethyl carbonate, and diphenyl carbonate; The surfactant includes one or a combination of a fluorocarbon surfactant, a nonionic surfactant, a cationic surfactant, and an anionic surfactant; The defoaming agent comprises one or a combination of diethylhexanol, n-octanol, isooctyl alcohol or isoamyl alcohol; The pore-forming agent includes any one of polyethylene glycol, dimethyl carbonate, dibutyl phthalate, petroleum ether, polyvinyl pyrrolidone and polyvinyl alcohol.

10. The method for preparing a high heat-resistant lithium-ion battery separator according to claim 1, It is characterized in that The coating method is selected from one of roller coating, spray coating, dip coating and extrusion coating, and the coating layer is selected from one of single-layer coating and double-layer coating.

11. The method for preparing a high heat-resistant lithium-ion battery separator according to claim 1, It is characterized in that The coating layer density is 1 to 6 g / m 2 ; The base film has a thickness of 5 to 15 μm; The base film comprises a polyethylene base film or a polypropylene base film; The dry thickness of the coating is 1 to 5 μm, and the wet thickness of the coating is 3 to 15 μm.

12. A method for preparing a highly heat-resistant lithium-ion battery separator according to claim 1 or 3, It is characterized in that The number of stages of the multi-stage coagulation bath is 3 to 7; The multi-stage coagulation bath is prepared with good solvent and poor solvent in a gradient ratio, the proportion of good solvent decreases with the increase of the stage number, and the proportion of poor solvent increases with the increase of the stage number.

13. The method for preparing a high heat-resistant lithium-ion battery separator according to claim 1, It is characterized in that During the extraction process, the wet film is subjected to the first-level coagulation bath for 5 to 10 minutes, and the coagulation bath times after the second level are equal or decrease, ranging from 60 to 150 seconds.

14. The method for preparing a high heat-resistant lithium-ion battery separator according to claim 1, It is characterized in that The drying method is selected from hot air drying, infrared heating drying and microwave drying.

15. A high heat-resistant lithium-ion battery separator, prepared by the preparation method according to any one of claims 1 to 14.

Citation Information

Patent Citations

  • Porous membrane for secondary battery, slurry for secondary battery porous membrane and secondary battery

    CN103403919A

  • Polyvinylidene fluoride / cyanoethyl cellulose composite lithium ion battery diaphragm and preparation method thereof

    CN107256936A

  • Separation film and production method therefor

    CN110475606A

  • Lithium ion battery diaphragm with high-temperature-resistant coating, and preparation method of lithium ion battery diaphragm

    CN111509168A

  • Modified aramid polymer, aramid membrane casting solution, lithium battery diaphragm, preparation methods and lithium battery