Roll core and battery
By setting functional areas, arc zones and flat zones with different compression ratios on the separator of the lithium-ion battery core, and applying corresponding glue and ceramic layers on its surface, the arc zone separator glue during battery charging is solved. The problem of hole blockage in the layer ensures smooth transmission of lithium ions and avoids lithium decomposition in black spots.
Patent Information
- Application Number
- CN202411176547.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-29
- Publication Date
- 2024-11-08
AI Technical Summary
During the charging process of the lithium-ion battery coiled battery cell, the internal stress in the arc area is difficult to release, resulting in the hole blockage of the diaphragm glue layer, affecting the transmission of lithium ions, and causing the problem of lithium-ion excretion of black spots.
A roll core is designed, and different functional areas are provided on the diaphragm, the arc area and the flat area, and the compression ratio of the arc area is greater than that of the flat area. By coating the first glue layer and/or the ceramic layer on the surface of the arc area, The surface of the flat area is coated with a second glue layer and/or a ceramic layer to increase the compression ratio of the arc area to buffer the internal stress caused by the expansion of the electrode sheet, and to prevent the diaphragm glue layer from blocking holes.
It effectively avoids the hole blockage of the diaphragm glue layer in the arc area, ensures that the lithium ion transmission is not hindered, and solves the problem of lithium desegmentation in black spots.
Smart Images

Figure CN118920025A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium-ion batteries, and in particular to a winding core and a battery containing the winding core. Background Art
[0002] Lithium-ion batteries are a clean energy source with small size, light weight and high energy storage ratio. They are currently widely used in various fields. Lithium-ion batteries include wound cells, which are electrode assemblies formed by winding the positive electrode sheet, negative electrode sheet and separator after rolling through a winding machine. During the winding process, the separator separates the positive electrode sheet from the negative electrode sheet.
[0003] In a wound cell, the cell can be divided into an unbent flat area and a bent arc area. During the charging process of a wound cell, the pole piece will expand, and internal stress will be generated inside the cell. The flat area has low internal stress because it can expand outward in the thickness direction of the cell, while the arc area has a stable structure and its internal stress is difficult to release compared to the flat area. Therefore, when the pole piece expansion is suppressed, it will cause greater internal stress in the arc area; due to the compression of internal stress, the diaphragm in the arc area of the cell will be blocked by the glue layer, resulting in obstruction of lithium ion transmission, and then black spot lithium precipitation.
[0004] Therefore, it is of great significance to develop a battery separator that can solve the problem of black spot lithium precipitation. Summary of the invention
[0005] The purpose of the present invention is to overcome the above problems existing in the prior art and provide a winding core and a battery containing the winding core. In the winding core, different functional areas (arc area and flat area) are arranged on the diaphragm, and the compression ratio of the arc area is greater than that of the flat area, so that the battery containing the winding core can avoid the problem of the arc area diaphragm blocking by the glue layer during the charging process, and will not affect the obstruction of lithium ion transmission, thereby effectively solving the problem of black spot lithium precipitation.
[0006] In order to achieve the above-mentioned objectives, the first aspect of the present invention provides a winding core, wherein the winding core is a winding structure formed by a first diaphragm, a first pole piece, a second diaphragm and a second pole piece stacked in sequence, and the first diaphragm and the second diaphragm are the same or different; the first diaphragm and the second diaphragm include a substrate, and the substrate is divided into an arc area and a flat area; at least one surface of the arc area is provided with a first glue layer and / or a first ceramic layer, and at least one surface of the flat area is provided with a second glue layer and / or a second ceramic layer; wherein the compression ratio of the arc area is greater than the compression ratio of the flat area.
[0007] A second aspect of the present invention provides a battery, which comprises the winding core described in the first aspect of the present invention.
[0008] The present invention adopts the above technical solution to achieve the following beneficial effects:
[0009] In the winding core provided by the present invention, the winding core is a winding structure formed by sequentially stacking a first diaphragm, a first pole piece, a second diaphragm and a second pole piece. Different functional areas (arc area and flat area) are arranged on the first diaphragm and the second diaphragm. The compression ratio of the arc area is greater than that of the flat area. The battery containing the diaphragm can avoid the problem of glue layer clogging of the diaphragm in the arc area during charging, and will not affect the obstruction of lithium ion transmission, thereby effectively solving the problem of black spot lithium precipitation.
[0010] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 Shown is a schematic diagram of a winding core structure in an example of the present invention.
[0012] Figure 2 Shown is a schematic diagram of a winding core structure in an example of the present invention.
[0013] Figure 3 It is a schematic diagram of the structure of the diaphragm in the width direction of the present invention (the two ends are not shown).
[0014] Description of Reference Numerals
[0015] 101: arc area; 102: flat area; 103: positive electrode; 104: negative electrode. DETAILED DESCRIPTION
[0016] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0017] Unless otherwise defined, all scientific and technical terms used in the present invention have the same meanings as commonly understood by one of ordinary skill in the art to which the present invention relates.
[0018] A first aspect of the present invention provides a winding core, wherein the winding core is a winding structure formed by sequentially stacking a first diaphragm, a first pole piece, a second diaphragm, and a second pole piece, wherein the first diaphragm and the second diaphragm are the same or different; the first diaphragm and the second diaphragm include a substrate, and the substrate is divided into an arc region and a flat region; at least one surface of the arc region is provided with a first glue layer and / or a first ceramic layer, and at least one surface of the flat region is provided with a second glue layer and / or a second ceramic layer;
[0019] The compression ratio of the arc area is greater than the compression ratio of the flat area.
[0020] When the diaphragm and the pole piece are wound to form a core structure, different areas of the diaphragm substrate will present two states: a bent state and an unbent state. Correspondingly, the diaphragm substrate will have a bent area and an unbent area. In the present invention, the "arc area" may be a part of the bent area of the diaphragm substrate and the part includes the inflection point of the bend. The "arc area" may also be the entire bent area of the diaphragm substrate. The "flat area" may be the entire unbent area and a partial bent area of the diaphragm substrate, and the partial bent area does not include the inflection point of the bend. The "flat area" may also be the entire unbent area of the diaphragm substrate.
[0021] In the present invention, under a certain ambient temperature, a certain pressure is applied to the diaphragm for a period of time, and the thickness of the diaphragm will change. The "compression ratio" refers to the ratio of the difference in thickness change of the diaphragm after compression to the thickness before compression, that is, compression ratio = (thickness before compression - thickness after compression) / thickness before compression * 100%.
[0022] Specifically, in the present invention, the test conditions for the "compression ratio" of the diaphragm include: compressing the diaphragm continuously for 30 minutes at a pressure of 1 MPa under an environment of 80°C.
[0023] The inventor of the present invention found that after testing the compression ratio of different materials for screening, the first glue layer and / or the first ceramic layer are coated on at least one surface of the arc area, and the first glue layer and / or the first ceramic layer are selected from materials with a large compression ratio; the second glue layer and / or the second ceramic layer are coated on at least one surface of the flat area, and the second glue layer and / or the second ceramic layer are selected from materials with a small compression ratio. In this way, the compression ratio of the arc area is greater than that of the flat area, so that the diaphragm in the arc area has a larger compression ratio, which can buffer the internal stress caused by the expansion of the pole piece bonded in the arc area, thereby avoiding the pores of the diaphragm glue layer in the arc area being squeezed and blocked, which will not affect the obstruction of lithium ion transmission, and effectively solve the problem of black spot lithium precipitation.
[0024] In one example, a surface of the arc region is coated with a first glue layer, and a surface of the same side of the flat region is coated with a second ceramic layer, and the compression ratio of the arc region is greater than that of the flat region.
[0025] In one example, the two opposite largest surfaces of the arc area are coated with a first glue layer, the two opposite largest surfaces of the flat area are coated with a second ceramic layer, and the compression ratio of the arc area is greater than that of the flat area.
[0026] In one example, a surface of the arc area is coated with a first glue layer, a surface on the same side of the flat area is coated with a second ceramic layer, a surface of the second ceramic layer away from the substrate is coated with a second glue layer, and the compression ratio of the arc area is greater than that of the flat area.
[0027] In one example, the two largest surfaces opposite to each other in the arc zone are coated with a first glue layer, the two largest surfaces opposite to each other in the flat zone are coated with a second ceramic layer, the surface of the second ceramic layer away from the substrate is coated with a second glue layer, and the compression ratio of the arc zone is greater than that of the flat zone.
[0028] In one example, a surface of the arc area is coated with a first ceramic layer, and a surface of the first ceramic layer away from the substrate is coated with a first glue layer; a surface on the same side of the flat area is coated with a second ceramic layer, and a surface of the second ceramic layer away from the substrate is coated with a second glue layer; the compression ratio of the arc area is greater than that of the flat area.
[0029] In one example, the two largest surfaces opposite to each other in the arc zone are coated with a first ceramic layer, and the surface of the first ceramic layer away from the substrate is coated with a first glue layer; the two largest surfaces opposite to each other in the flat zone are coated with a second ceramic layer, and the surface of the second ceramic layer away from the substrate is coated with a second glue layer; the compression ratio of the arc zone is greater than that of the flat zone.
[0030] In one example, the separator substrate is a porous substrate, and any separator substrate conventionally used in the art may be selected.
[0031] Exemplarily, the porous substrate is selected from at least one of polyethylene, polypropylene, multilayer polyethylene polypropylene, polyethylene polypropylene blend, polyimide, polyetherimide, polyamide, meta-aramid, para-aramid and meta-para blended aramid.
[0032] In order to better solve the problem of black spots and lithium plating in batteries, one or more of the technical features may be further optimized.
[0033] In a preferred embodiment, Figure 1 As shown, the arc area 101 is the entire curved area of the diaphragm substrate, and the flat area 102 is the entire uncurved area of the diaphragm substrate.
[0034] In one example, a ratio of the compression ratio of the arc area to the flat area is A, and A satisfies: 1.5≤A≤5.
[0035] Exemplarily, the compression ratio of the arc area to the flat area may be 1.6, 1.8, 2, 2.2, 2.5, 2.8, 3, 3.2, 3.5, 3.8, 4, 4.2, 4.5, 4.8 and 5 or any point value in the range consisting of any two of the above point values.
[0036] Preferably, A satisfies: 1.8≤A≤3.
[0037] More preferably, A satisfies: 2≤A≤2.5.
[0038] In one example, the compression ratio of the arc region is 10-35%.
[0039] Exemplarily, the compression ratio of the arc area can be 10%, 12%, 15%, 18%, 20%, 22%, 25%, 28%, 30%, 32%, 35% or any point value in the range consisting of any two of the above point values.
[0040] Preferably, the compression ratio of the arc area is 20-30%.
[0041] In the present invention, the compression ratio of the arc region refers to the compression ratio data tested after the surface of the diaphragm substrate in the arc region is coated with the first glue layer and / or the first ceramic layer.
[0042] In one example, the compression ratio of the flat area is 2-30%.
[0043] Exemplarily, the compression ratio of the flat area can be 2%, 5%, 8%, 10%, 12%, 15%, 18%, 20%, 22%, 25%, 28%, 30% or any point value in the range consisting of any two of the above point values.
[0044] Preferably, the compression ratio of the flat area is 5-15%.
[0045] In the present invention, the compression ratio of the flat area refers to the compression ratio data tested after the second glue layer and / or the second ceramic layer is coated on the surface of the flat area.
[0046] In one example, the thickness of the first adhesive layer is 0.5 μm-20 μm, for example, 0.5 μm, 1 μm, 2 μm, 3 μm, 5 μm, 8 μm, 10 μm, 12 μm, 15 μm, 18 μm, 20 μm or any value in the range consisting of any two of the above values.
[0047] Preferably, the thickness of the first adhesive layer is 1 μm-10 μm.
[0048] In one example, the thickness of the second adhesive layer is 0.5 μm-20 μm, for example, 0.5 μm, 1 μm, 2 μm, 3 μm, 5 μm, 8 μm, 10 μm, 12 μm, 15 μm, 18 μm, 20 μm or any value in the range consisting of any two of the above values.
[0049] Preferably, the second adhesive layer has a thickness of 1 μm-10 μm.
[0050] In one example, the thickness of the first ceramic layer is 0.5 μm-20 μm, for example, 0.5 μm, 1 μm, 2 μm, 3 μm, 5 μm, 8 μm, 10 μm, 12 μm, 15 μm, 18 μm, 20 μm or any point value in the range consisting of any two of the above point values.
[0051] Preferably, the thickness of the first ceramic layer is 1 μm-10 μm.
[0052] In one example, the thickness of the second ceramic layer is 0.5 μm-20 μm, for example, 0.5 μm, 1 μm, 2 μm, 3 μm, 5 μm, 8 μm, 10 μm, 12 μm, 15 μm, 18 μm, 20 μm or any point value in the range consisting of any two of the above point values.
[0053] Preferably, the second ceramic layer has a thickness of 1 μm-10 μm.
[0054] In some embodiments, the first adhesive layer and the second adhesive layer have different thicknesses.
[0055] In some embodiments, the total thickness of the first glue layer and the first ceramic layer is the same as the total thickness of the second glue layer and the second ceramic layer.
[0056] In one example, the first adhesive layer includes a first polymer, and the second adhesive layer includes a second polymer.
[0057] In one example, the first polymer and the second polymer are each independently selected from at least one of homopolymers or copolymers of olefinic monomers, halogen-substituted olefinic monomers, and acrylic monomers.
[0058] Illustratively, the olefin monomers include, but are not limited to, butadiene, ethylene, propylene, acrylonitrile styrene, and methyl styrene.
[0059] Illustratively, the halogen-substituted olefin monomers include, but are not limited to, vinylidene fluoride, hexafluoropropylene, difluoroethylene, tetrafluoroethylene, and trichloroethylene.
[0060] Illustratively, the acrylic monomers include, but are not limited to, methyl acrylate, methyl methacrylate, ethyl acrylate, butyl acrylate, ethyl methacrylate, acrylic acid, acrylamide, and methacrylic acid.
[0061] Exemplarily, the first polymer and the second polymer are each independently selected from one or more of a copolymer of vinylidene fluoride-hexafluoropropylene, a copolymer of vinylidene fluoride-trichloroethylene, polystyrene, polyacrylate, polyacrylic acid, polyacrylonitrile, polyvinyl pyrrolidone, polyvinyl acetate, a copolymer of ethylene-vinyl acetate, polyimide, polyphenylene phthalate, a copolymer of acrylonitrile-styrene-butadiene, polyvinyl alcohol, a copolymer of styrene-butadiene and polyvinylidene fluoride.
[0062] In the present invention, the first polymer and the second polymer may be the same or different.
[0063] In one example, the first ceramic layer includes first ceramic particles and a first binder, and the second ceramic layer includes second ceramic particles and a second binder.
[0064] In one example, based on the total mass of the first ceramic layer, the content of the first ceramic particles is 50-99.9 wt %, and the content of the first binder is 0.1-50 wt %.
[0065] In one example, based on the total mass of the second ceramic layer, the content of the second ceramic particles is 50-99.9 wt %, and the content of the second binder is 0.1-50 wt %.
[0066] In one example, the first ceramic particles and the second ceramic particles are each independently selected from at least one of metal oxides, inorganic metal salts, metal nitrides, and inorganic ceramic solid electrolytes.
[0067] Illustratively, the metal oxides include, but are not limited to, aluminum oxide, magnesium oxide, calcium oxide, titanium dioxide, silicon dioxide, zirconium dioxide, tin dioxide, boehmite, and zinc oxide.
[0068] Illustratively, the inorganic metal salt includes, but is not limited to, barium sulfate, calcium carbonate, and magnesium sulfate.
[0069] Illustratively, metal nitrides include, but are not limited to, tungsten nitride, silicon carbide, boron nitride, aluminum nitride, titanium nitride, and magnesium nitride.
[0070] Exemplarily, the inorganic ceramic solid electrolyte includes, but is not limited to, at least one of solid electrolyte particles having a NASICON structure, a perovskite structure, an antiperovskite structure, a thio-LISICON structure, and a garnet structure.
[0071] In one example, the first ceramic particles and the second ceramic particles are each independently selected from one or more of aluminum oxide, magnesium oxide, silicon dioxide, titanium dioxide, zirconium dioxide, zinc oxide, barium sulfate, boron nitride, aluminum nitride, magnesium nitride, tin dioxide, magnesium hydroxide, boehmite and calcium carbonate.
[0072] In the present invention, the first ceramic particles and the second ceramic particles may be the same or different.
[0073] In one example, the first binder and the second binder are each independently selected from one or more of a copolymer of vinylidene fluoride and hexafluoropropylene, a copolymer of vinylidene fluoride and trichloroethylene, polystyrene, polyacrylate, polyacrylic acid, polyacrylonitrile, polyvinyl pyrrolidone, polyvinyl acetate, a copolymer of ethylene-vinyl acetate, polyimide, polyphenylene phthalide, a copolymer of acrylonitrile-styrene-butadiene, polyvinyl alcohol, a copolymer of styrene-butadiene and polyvinylidene fluoride.
[0074] In the present invention, the first binder and the second binder may be the same or different.
[0075] In some embodiments, along the direction in which the winding core is stretched, the width of the arc area is not greater than the bent portion of the winding structure, and the width of the flat area is not less than the unbent portion of the winding structure.
[0076] In the present invention, the first diaphragm and the second diaphragm may be the same or different, and preferably the first diaphragm and the second diaphragm are the same.
[0077] like Figure 1 and Figure 3 As shown, the winding core is a winding structure formed by sequentially stacking a first separator, a negative electrode sheet 104, a second separator and a positive electrode sheet 103. Along the direction of the winding core stretching, the width of the arc area 101 is the bending part of the winding structure, and the width of the flat area 102 is the unbent part of the winding structure.
[0078] In the present invention, the width direction of the separator is the same as the direction in which the winding core is stretched.
[0079] The inventors of the present invention have found that in the winding structure of the winding core, the inflection point of the bending area is the part subject to the greatest internal stress, and black spot lithium precipitation is more likely to occur there. Therefore, increasing the compression ratio of the diaphragm at the inflection point of the bending area can achieve the effect of suppressing the black spot lithium precipitation. In order to achieve a better effect of suppressing the black spot lithium precipitation, the compression ratio of the diaphragm in the bending area including the inflection point of the bending area, or the compression ratio of the diaphragm in the entire bending area can also be increased.
[0080] In one example, if Figure 2As shown, the arc area 101 is a part of the diaphragm bending area and includes the bending inflection point (for example, the bending part in the black dotted box), and the flat area 102 is the entire unbent area and partial bent area of the diaphragm and does not include the bending inflection point.
[0081] In the present invention, the inflection point of the bend is the intersection of the center line of the winding core and the bending area.
[0082] In one example, if Figure 1 As shown, the arc area 101 is the entire curved area of the diaphragm substrate, and the flat area 102 is the entire uncurved area of the diaphragm substrate.
[0083] In one example, the width L of the arc region is Wherein, d is the thickness of the winding core.
[0084] In the present invention, the core bending area is set to a semicircular structure with the core thickness d as the diameter, and the arc length of the semicircle is the maximum width of the arc area, but the actual shape of the arc area is not limited to a standard semicircle. For example, the structure of the core is actually similar to the bending part formed by winding multiple layers of cloth, and the bending part is not a standard semicircle.
[0085] In one example, the minimum width of the arc region of 0.01 mm refers to the minimum width of the inflection point of the bending region of the diaphragm.
[0086] In one example, the maximum width of the arc region is It refers to the arc length of a semicircle with the core thickness d as the diameter.
[0087] The structures of the battery except the winding core can be manufactured in accordance with the methods in the art, and can achieve the effect of suppressing the lithium precipitation of black spots.
[0088] A second aspect of the present invention provides a battery, which comprises the winding core described in the first aspect of the present invention.
[0089] In one example, the battery includes a positive electrode sheet, a negative electrode sheet, a non-aqueous electrolyte, and the separator described in the first aspect of the present invention, and the separator is disposed between the positive electrode sheet and the negative electrode sheet.
[0090] In one example, the battery comprises the winding core according to the second aspect of the present invention and a non-aqueous electrolyte.
[0091] In one example, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer coated on one side or both sides of the positive electrode current collector.
[0092] Illustratively, the positive electrode current collector is a material having conductivity without causing adverse chemical changes in the secondary battery, including but not limited to aluminum, aluminum alloy, nickel, nickel alloy, titanium, and titanium alloy.
[0093] The positive electrode active material layer includes a positive electrode active material, a positive electrode conductor and a positive electrode binder. There is no particular limitation on the positive electrode active material, and any common positive electrode active material in the art can be used, for example, at least one of lithium cobalt oxide, lithium manganese oxide, lithium nickel oxide and lithium nickel cobalt manganese oxide lithium iron phosphate.
[0094] In one example, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer coated on one side or both sides of the negative electrode current collector.
[0095] Illustratively, the negative electrode current collector is a material having conductivity without causing adverse chemical changes in the secondary battery, and can be selected from copper, stainless steel, aluminum, nickel, titanium, carbon cloth, or a composite of the materials.
[0096] The negative electrode active material layer includes a negative electrode active material, a negative electrode conductive agent and a negative electrode binder. There is no particular limitation on the negative electrode active material, and any common negative electrode active material in the art can be used, for example, at least one of graphite, lithium titanate and silicon-based negative electrode.
[0097] In one example, the positive electrode conductive agent and the negative electrode conductive agent are independently selected from at least one of conductive graphite, ultrafine graphite, acetylene black, conductive carbon black SP, superconducting carbon black, carbon nanotubes and conductive carbon fibers.
[0098] In one example, the positive electrode binder and the negative electrode binder are independently selected from at least one of polyvinylidene fluoride, polytetrafluoroethylene, sodium carboxymethyl cellulose, styrene-butadiene rubber, polyurethane, polyvinyl alcohol, polyvinylidene fluoride and a copolymer of vinylidene fluoride and fluorinated olefin.
[0099] The non-aqueous electrolyte may be any commonly used electrolyte in the art and is not specifically limited herein.
[0100] In the present invention, when numbers are used to distinguish terms, such as "first ceramic layer", "second ceramic layer", etc., the numbers in this expression only serve to distinguish and do not indicate the order of precedence. Unless otherwise specified, the size of the numbers does not bring any limiting effect to the technical solution.
[0101] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0102] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.
[0103] The present invention is described in detail below in conjunction with specific embodiments, which are used to understand but not to limit the present invention.
[0104] In the following embodiments and comparative examples, when preparing the first ceramic layer, the second ceramic layer and the slurry, a solvent is used to dissolve other components, and the solvent can be selected from one or more of water, N-methyl-2-pyrrolidone, acetone, tetrahydrofuran, chloroform, dichloromethane, dimethylformamide and cyclohexane.
[0105] Since the membrane needs to be dried after coating the slurry, the solvent will evaporate after drying, so the mass of the final coating does not include the mass of the solvent.
[0106] The method for testing the compression ratio of the battery separator in the following examples and comparative examples is described as follows:
[0107] (1) Test and record the thickness of the diaphragm before compression;
[0108] (2) Compress the diaphragm at 1 MPa for 30 min at 80°C and record the thickness after compression;
[0109] (3) Calculate according to the formula: Compression ratio = (thickness before compression - thickness after compression) / thickness before compression * 100%.
[0110] Example 1
[0111] 1. Preparation of diaphragm
[0112] (1) Preparation of the first adhesive layer slurry
[0113] A first adhesive layer slurry is obtained by mixing a copolymer of vinylidene fluoride and hexafluoropropylene (a first polymer) and N-methyl-2-pyrrolidone (a solvent);
[0114] (2) Preparation of the second ceramic layer slurry
[0115] Aluminum oxide particles (second ceramic particles), a copolymer of vinylidene fluoride and hexafluoropropylene (second binder) and N-methyl-2-pyrrolidone (solvent) are mixed to obtain a second ceramic layer slurry. The second ceramic particles contain 60wt% and the second binder contains 40wt% based on the total mass of the second ceramic layer slurry.
[0116] (3) using any one of the coating processes such as gravure coating, dip coating, transfer coating and spray coating, double-sided coating is performed on the arc area of the diaphragm substrate using the first adhesive layer slurry, and double-sided coating is performed on the flat area of the diaphragm substrate using the second ceramic layer slurry, and drying;
[0117] Among them, the compression ratio of the arc area to the flat area is A=2.5;
[0118] The width L of the arc area is 7.85 mm, the thickness of the first adhesive layer is 4 μm, and the thickness of the second ceramic layer is 4 μm.
[0119] 2. Preparation of positive electrode
[0120] The positive electrode active material, positive electrode conductor and positive electrode binder are mixed in a certain proportion, and then N-methylpyrrolidone is added and stirred and dispersed to form a positive electrode slurry. In the positive electrode slurry, the solid components include 97.2wt% lithium cobalt oxide (LCO), 1.5wt% conductive carbon black and 1.3wt% polyvinylidene fluoride (PVDF). Then the positive electrode slurry is coated on the positive electrode collector once (double-sided coating) through a coating device, dried, cut and sliced to prepare a positive electrode sheet.
[0121] 3. Preparation of negative electrode sheet
[0122] The negative electrode active material, negative electrode conductive agent, negative electrode binder and thickener are mixed in a certain proportion, and deionized water is added and stirred to disperse to form a negative electrode slurry. In the negative electrode slurry, the solid components include 96.9% graphite, 0.5wt% conductive carbon black, 1.3wt% sodium carboxymethyl cellulose (CMC), and 1.3wt% styrene-butadiene rubber (SBR). Then the negative electrode slurry is coated on the negative electrode current collector (double-sided coating), dried, cut, and sliced to prepare the negative electrode sheet.
[0123] 4. Preparation of batteries
[0124] The positive electrode sheet prepared in step 2, the negative electrode sheet prepared in step 3 and the separator prepared in step 1 are prepared into a roll core (battery cell) with a total thickness of 5 mm. The battery cell is then made into a battery together with an aluminum-plastic film, and then the electrolyte injection, aging, formation, sorting and other processes are carried out. Finally, the electrochemical performance of the battery is tested.
[0125] Example 2
[0126] Refer to Example 1, the difference from Example 1 is:
[0127] 1. Preparation of diaphragm
[0128] (1) Preparation of the first adhesive layer slurry
[0129] The copolymer of vinylidene fluoride and trichloroethylene (first polymer) and dichloromethane (solvent) are mixed to obtain a first adhesive layer slurry;
[0130] (2) Preparation of the second adhesive layer slurry
[0131] Mixing polyvinylidene fluoride (second polymer) and dichloromethane (solvent) to obtain a second adhesive layer slurry;
[0132] (3) Preparation of second ceramic layer slurry
[0133] Mixing magnesium oxide particles (second ceramic particles), polyvinylidene fluoride (second binder) and dichloromethane (solvent) to obtain a second ceramic layer slurry, wherein the content of the second ceramic particles is 70wt% and the content of the second binder is 30wt% based on the total mass of the second ceramic layer slurry;
[0134] (4) using any one of the coating processes such as gravure coating, dip coating, transfer coating and spray coating, double-sided coating of the arc area of the diaphragm substrate with the first adhesive layer slurry, double-sided coating of the flat area of the diaphragm substrate with the second ceramic layer slurry, and then coating the second adhesive layer slurry on the surface of the second ceramic layer; drying;
[0135] Among them, the ratio of the compression ratio of the arc area to the flat area is A=2;
[0136] The width L of the arc area is 7.85 mm, the thickness of the first adhesive layer is 4 μm, and the total thickness of the second ceramic layer and the second adhesive layer is 4 μm (the thickness ratio of the second ceramic layer and the second adhesive layer is 3:1).
[0137] Example 3
[0138] Refer to Example 1, the difference from Example 1 is:
[0139] 1. Preparation of diaphragm
[0140] (1) Preparation of the first adhesive layer slurry
[0141] The ethylene-vinyl acetate copolymer (first polymer) and acetone (solvent) are mixed to obtain a first adhesive layer slurry;
[0142] (2) Preparation of the first ceramic layer slurry
[0143] Mixing silica particles (first ceramic particles), ethylene-vinyl acetate copolymer (first binder) and acetone (solvent) to obtain a first ceramic layer slurry, wherein the content of the first ceramic particles is 60wt% and the content of the first binder is 40wt% based on the total mass of the first ceramic layer slurry;
[0144] (3) Preparation of the second adhesive layer slurry
[0145] Mixing polyacrylic acid (second polymer) and acetone to obtain a second adhesive layer slurry;
[0146] (4) Preparation of second ceramic layer slurry
[0147] Aluminum nitride particles (second ceramic particles), polyacrylic acid (second binder) and acetone (solvent) are mixed to obtain a second ceramic layer slurry, wherein the content of the second ceramic particles is 95wt% and the content of the second binder is 5wt% based on the total mass of the second ceramic layer slurry;
[0148] (5) using any one of the coating processes such as gravure coating, dip coating, transfer coating and spray coating, double-sided coating of the arc area of the diaphragm substrate with the first ceramic layer slurry, and then coating the first adhesive layer slurry on the surface of the first ceramic layer; double-sided coating of the flat area of the diaphragm substrate with the second ceramic layer slurry, and then coating the second adhesive layer slurry on the surface of the second ceramic layer; drying;
[0149] Among them, the compression ratio of the arc area to the flat area is A=2.2;
[0150] The arc width L is 7.85 mm, the thickness of the first ceramic layer and the first adhesive layer is 4 μm (the thickness ratio of the first ceramic layer and the first adhesive layer is 1:2), and the total thickness of the second ceramic layer and the second adhesive layer is 4 μm (the thickness ratio of the second ceramic layer and the second adhesive layer is 1:1).
[0151] Example 4
[0152] The process was carried out with reference to Example 1, except that the first polymer was replaced by polyacrylic acid, and the compression ratio of the arc area to the flat area was A=1.8.
[0153] Example 5
[0154] The method is carried out with reference to Example 1, but differs from Example 1 in that: based on the total mass of the second ceramic layer slurry, the content of the second ceramic particles is 70wt%, and the content of the second binder is 30wt%; wherein the compression ratio of the arc area to the flat area is A=3.
[0155] Example 6
[0156] The method is carried out with reference to Example 1, and the difference from Example 1 is that the width L of the arc area is 0.1 mm, including the inflection point of the bending area of the diaphragm.
[0157] Example 7
[0158] The method is carried out with reference to Example 1, except that the arc width L is 5 mm, including the inflection point of the bending area of the diaphragm.
[0159] Comparative Example 1
[0160] The method is carried out with reference to Example 1, except that: only the second adhesive layer is coated on the flat area, and the material and thickness of the second adhesive layer are the same as those of the first adhesive layer; and the compression ratio of the arc area to the flat area is A=1.
[0161] Comparative Example 2
[0162] The method is carried out with reference to Example 1, which differs from Example 1 in that: only the first ceramic layer is coated on the arc area, and the material and thickness of the first ceramic layer and the second ceramic layer are the same; and the compression ratio of the arc area to the flat area is A=1.
[0163] Comparative Example 3
[0164] The method is carried out with reference to Example 2, except that the first polymer is replaced by polyacrylic acid, the thickness ratio of the second ceramic layer to the second adhesive layer is 2:1, and the compression ratio of the arc area to the flat area is A=1.34.
[0165] Comparative Example 4
[0166] Refer to Example 1, which differs from Example 1 in that the second binder is polyacrylic acid, based on the total mass of the second ceramic layer slurry, the content of the second ceramic particles is 75wt%, and the content of the second binder is 25wt%, wherein the compression ratio of the arc area to the flat area is A=5.5.
[0167] Experimental example
[0168] (1) Battery cycle test at room temperature
[0169] The lithium-ion batteries of the above embodiments and comparative examples were placed in a 25°C environment, charged to 4.45V with a constant current and constant voltage of 3C, and charged to a cut-off current of 0.05C with a constant voltage of 4.45V; then left to stand for 15 minutes; and discharged to 3V with a current of 1C. The initial capacity was recorded as Q1, and the capacity after 600 cycles was recorded as Q2. The capacity retention rate of the battery after normal temperature cycling was calculated by the following formula: Capacity retention rate (%) = (Q2 / Q1)*100%.
[0170] (2) Battery expansion rate test
[0171] The initial thickness of the electrode sheet was measured as M1, and the thickness after 600 cycles was measured as M2. The expansion rate of the battery after normal temperature cycling was calculated by the following formula: battery expansion rate (%) = [(M2-M1) / M1]*100%.
[0172] (3) Battery lithium deposition detection
[0173] The battery that has been cycled for 600 weeks is disassembled to observe whether lithium deposition occurs.
[0174] Table 1
[0175]
[0176]
[0177] According to the results in Table 1, compared with the comparative example, the degree of lithium deposition in the arc area of the embodiment of the present invention is significantly reduced, and the larger the ratio of the compression ratio of the arc area to the flat area, that is, the higher the compression ratio of the arc area, the less likely the arc area is to deposit lithium, which means that increasing the compression ratio of the arc area diaphragm can effectively solve the problem of lithium deposition in the arc black spots caused by the pore blocking of the arc area diaphragm rubber layer.
[0178] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A winding core, characterized in that: The winding core is a winding structure formed by sequentially stacking a first diaphragm, a first pole piece, a second diaphragm and a second pole piece; The first diaphragm and the second diaphragm include a substrate, and the substrate is divided into an arc area and a flat area; At least one surface of the arc area is provided with a first glue layer and / or a first ceramic layer, and at least one surface of the flat area is provided with a second glue layer and / or a second ceramic layer; The compression ratio of the arc area is greater than the compression ratio of the flat area.
2. The winding core according to claim 1, wherein: The compression ratio of the arc area to the flat area is A, and A satisfies: 1.5≤A≤5; Preferably, A satisfies: 1.8≤A≤3.
3. The winding core according to claim 1, wherein: The compression ratio of the arc zone is 10-35%, preferably 20-30%; And / or, the compression ratio of the flat zone is 2-30%, preferably 5-15%.
4. The winding core according to claim 1, wherein: The thickness of the first adhesive layer and the second adhesive layer are independently 0.5 μm-20 μm; and / or the thickness of the first ceramic layer and the second ceramic layer are independently 0.5 μm-20 μm; Preferably, the thickness of the first adhesive layer and the second adhesive layer are different; Preferably, the total thickness of the first adhesive layer and the first ceramic layer is the same as the total thickness of the second adhesive layer and the second ceramic layer.
5. The winding core according to claim 1, wherein: The first adhesive layer includes a first polymer, and the second adhesive layer includes a second polymer; Preferably, the first polymer and the second polymer are each independently selected from at least one of homopolymers or copolymers of olefin-based monomers, halogen-substituted olefin-based monomers and acrylic monomers.
6. The winding core according to claim 1, wherein: The first ceramic layer includes first ceramic particles and a first binder, and the second ceramic layer includes second ceramic particles and a second binder; Preferably, the first ceramic particles and the second ceramic particles are each independently selected from at least one of metal oxides, inorganic metal salts, metal nitrides and inorganic ceramic solid electrolytes.
7. The winding core according to claim 1, wherein: Along the direction in which the winding core is stretched, the width of the arc area is not greater than the bent portion of the winding structure, and the width of the flat area is not less than the unbent portion of the winding structure.
8. The winding core according to claim 7, wherein: The arc area is a part of the bending area of the diaphragm and includes the inflection point of the bending, and the flat area is the entire unbent area and partial bending area of the diaphragm and does not include the inflection point of the bending; the inflection point of the bending is the intersection of the center line of the winding core and the bending area.
9. The winding core according to claim 7, wherein: The arc area is the entire curved area of the diaphragm, and the flat area is the entire uncurved area of the diaphragm; And / or, the width L of the arc area is Wherein, d is the thickness of the winding core.
10. A battery, characterized in that: The battery comprises the winding core according to any one of claims 1 to 9.
Citation Information
Patent Citations
Lithium battery
CN112563583A
Winding type battery core and battery
CN113471630A
Bare battery cell and lithium battery
CN216773319U
Battery cell structure for inhibiting fracture of cyclic expansion positive plate
CN216903069U
Nonaqueous electrolyte secondary battery
JP2006244834A
Cited By
Battery
CN119208518A