Flexible organic transistor array for ammonia gas detection and preparation method thereof
By adopting specific materials and structural designs in the organic transistor array, the responsiveness and sensitivity of ammonia detection are improved, and the problem of low responsiveness and sensitivity in the prior art is solved, achieving more stable and efficient ammonia detection.
Patent Information
- Application Number
- CN202410974693.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
AI Technical Summary
The existing organic transistor gas sensors have low responsiveness and sensitivity to ammonia, and are susceptible to chemical interactions and photoexcitation, resulting in insufficient stability and detection accuracy.
A flexible organic transistor array was designed, using polyethylene terephthalate or polyimide as the substrate, indium tin oxide as the gate, polyvinylpyrrolidone as the dielectric layer, 8-benzothiophene dimethyl The heterojunction composed of organic small molecular materials such as ylbenzothiophene and pentacene, the Au electrode is used as the source and drain, and the contact area is enhanced by the interdigital structure, and is prepared in combination with magnetron sputtering and vacuum thermal evaporation.
It improves the responsiveness and sensitivity to ammonia detection, enhances the stability and detection accuracy of the device, reduces the production cost, and is suitable for portable and wearable device applications.
Smart Images

Figure CN118921993A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of organic transistor sensor preparation, and in particular to a flexible organic transistor array for ammonia detection and a preparation method thereof. Background Art
[0002] As a detection device, gas sensors can convert the sensed gas information into electrical signal output according to certain rules, so as to meet the requirements of information transmission, processing, storage, display, recording and control. Gas sensors are widely used in industrial production detection and human daily life, especially for the detection of toxic gases such as sulfur dioxide, chlorine, carbon monoxide, ammonia, etc.
[0003] Using organic transistors as gas sensors is to utilize the ideal recognition ability of organic materials for target analysis gases, and to detect gas information through a series of changes in electrical parameters (carrier concentration, threshold voltage, current switching ratio, etc.). Organic transistors are light in weight, low in cost, have excellent gas-sensitive properties, and can work at room temperature to meet the low energy consumption requirements of sensors and realize portable real-time gas sensing; in addition, organic materials also have good mechanical flexibility and biocompatibility. Therefore, organic transistor gas sensors have received increasing attention in the field of wearable electronic products.
[0004] In fact, compared with organic transistor gas sensors, sensors with inorganic metal oxides as active materials are more stable. This is because the performance of organic materials is easily affected by chemical interactions, light excitation, dimensional deformation, etc. In addition, the non-covalent interaction between the surface of the organic semiconductor layer and the target analytical gas in contact is not strong, resulting in generally low sensitivity and responsiveness of organic transistor gas sensors. Therefore, it is urgent to synthesize organic sensitive materials with better performance or develop new device structures to promote the rapid development of this research field. Summary of the invention
[0005] The object of the present invention is to provide a flexible organic transistor array for ammonia detection and a preparation method thereof, which can improve the responsiveness and sensitivity of the transistor to ammonia detection.
[0006] Technical solution: In order to achieve the above-mentioned invention objectives, the flexible organic transistor array for ammonia detection of the present invention is used to detect ammonia, including a substrate, a gate, a dielectric layer, an organic small molecule semiconductor heterojunction, a source and a drain, wherein the gate covers one side of the substrate, and the dielectric layer covers the side of the gate facing away from the substrate; the organic small molecule semiconductor heterojunction includes an upper material and a lower material, the lower material covers the side of the dielectric layer facing away from the gate, the upper material covers the side of the lower material facing away from the dielectric layer, and the source and the drain cover a portion of the side of the upper material facing away from the lower material.
[0007] Furthermore, the substrate material is polyethylene terephthalate or polyimide, and the thickness of the polyethylene terephthalate or the polyimide is 0.05 to 0.175 mm.
[0008] Furthermore, the material of the gate is indium tin oxide, and the film thickness of the indium tin oxide is 200-300 nanometers.
[0009] Furthermore, the material of the dielectric layer is polyvinyl pyrrolidone, and the film thickness of the polyvinyl pyrrolidone is 600 to 900 nanometers. Polyvinyl pyrrolidone has good flexibility, low toxicity and biocompatibility; polyvinyl pyrrolidone has good interface contact with 8-benzothiophene dimethylbenzothiophene deposited by organic vapor deposition, which is conducive to low-temperature deposition of large-area high-quality organic materials on its surface, and improves the stability of transistor array for ammonia sensing.
[0010] Furthermore, the lower layer material is 8-benzothiophene dimethylbenzothiophene, and the thickness of the 8-benzothiophene dimethylbenzothiophene is 30 to 50 nanometers.
[0011] Furthermore, the upper layer material is any one of pentacene, 6,13-bis(triisopropylsilylethynyl)pentacene, 2,9-didecylnaphtho[2,3-B:2′,3′-F]thieno[3,2-B]thiophene and dinaphtho[2,3-B:2′,3′-F]thieno[3,2-B]thiophene, and the thickness of the upper layer material is 10 to 100 nanometers.
[0012] Furthermore, the source and drain are Au electrodes, and the thickness of the Au electrodes is 70 nanometers.
[0013] Furthermore, the upper material, the source electrode and the drain electrode are all interdigitated structures. The upper material of the organic small molecule semiconductor heterojunction is interdigitated and patterned to increase the contact area between the organic material and the ammonia gas, thereby improving the performance of the organic heterojunction transistor.
[0014] A method for preparing a flexible organic transistor array for ammonia detection, the specific steps are as follows:
[0015] Step 1: providing a substrate, and depositing a transparent conductive film as a gate on the surface of the substrate by DC magnetron sputtering, sol-gel method or vacuum thermal evaporation;
[0016] Step 2: Mixing polyvinyl pyrrolidone particles, methylated poly (melamine-CO-formaldehyde) crosslinking agent and propylene glycol methyl ether acetate solution in a mass ratio of 2:1:6 to 2:1:14 in a magnetic stirrer to prepare a polyvinyl pyrrolidone solution;
[0017] Step 3: Spin-coating the polyvinyl pyrrolidone solution on the side of the gate facing away from the substrate, and then heating in an oven to form a dielectric layer;
[0018] Step 4: depositing an organic semiconductor heterojunction on a side of the dielectric layer facing away from the gate by an organic vacuum thermal evaporation process, wherein the organic small molecule semiconductor heterojunction comprises an upper layer material and a lower layer material, wherein the lower layer material covers a side of the dielectric layer facing away from the gate, and the upper layer material covers a side of the lower layer material facing away from the dielectric layer;
[0019] Step 5: Deposit a metal film on the side of the upper layer material facing away from the lower layer material by magnetron sputtering to form a source electrode and a drain electrode, thereby obtaining a flexible organic transistor array for ammonia detection.
[0020] Furthermore, before executing step 1, the substrate sheet is immersed in acetone solution, ethanol solution and deionized water in sequence, and then the substrate sheet is ultrasonically treated using an ultrasonic cleaner at room temperature, and then the substrate is blown dry using a nitrogen gun after the ultrasonic treatment.
[0021] Furthermore, the material of the substrate in step 1 is polyethylene terephthalate or polyimide, and the thickness of the polyethylene terephthalate or the polyimide is 0.05 to 0.175 mm.
[0022] Furthermore, the material of the gate in step 1 is indium tin oxide, and the film thickness of the indium tin oxide is 200-300 nanometers.
[0023] Furthermore, the material of the dielectric layer in step 3 is polyvinyl pyrrolidone, and the film thickness of the polyvinyl pyrrolidone is 600-900 nanometers.
[0024] Furthermore, the lower layer material in step 4 is 8-benzothiophene dimethylbenzothiophene, and the thickness of the 8-benzothiophene dimethylbenzothiophene is 30 to 50 nanometers.
[0025] Furthermore, the upper layer material in step 4 is any one of pentacene, 6,13-bis(triisopropylsilylethynyl)pentacene, 2,9-didecylnaphtho[2,3-B:2′,3′-F]thieno[3,2-B]thiophene and dinaphtho[2,3-B:2′,3′-F]thieno[3,2-B]thiophene, and the thickness of the upper layer material is 10 to 100 nanometers.
[0026] Furthermore, the source and drain in step 5 are Au electrodes, and the thickness of the Au electrodes is 70 nanometers.
[0027] An ammonia detection device comprises a flexible organic transistor array for ammonia detection.
[0028] Beneficial effects: The present invention utilizes an organic small molecule semiconductor heterojunction to sense ammonia. Compared with transistors based on a single layer of organic materials, for an organic small molecule semiconductor heterojunction with a stacked structure, the 8-benzothiophene dimethylbenzothiophene film can promote the growth of surface organic small molecule materials, and the organic small molecule materials located in the upper layer can enhance the hole carrier injection from the source and drain to the lower layer material 8-benzothiophene dimethylbenzothiophene, thereby improving the responsiveness and sensitivity of the array device to ammonia detection. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a schematic diagram of the structure of the flexible organic transistor array for ammonia detection of the present invention;
[0030] Figure 2 It is a time-current diagram of ammonia response of the flexible organic transistor array for ammonia detection of the present invention. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Unless otherwise defined, the technical terms or scientific terms used herein should be understood by people with general skills in the field to which the present invention belongs. "Including" and similar words used in this article mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, without excluding other elements or objects.
[0032] like Figure 1As shown, an embodiment of the present invention provides a flexible organic transistor array for ammonia detection, which is used to detect ammonia, including a substrate 1, a gate 2, a dielectric layer 3, an organic small molecule semiconductor heterojunction 4, a source 5 and a drain 6, wherein the gate 2 covers one side of the substrate 1, the dielectric layer 3 covers the side of the gate 2 facing away from the substrate 1, and the organic small molecule semiconductor heterojunction 4 includes an upper material 42 and a lower material 41, wherein the lower material 41 covers the side of the dielectric layer 3 facing away from the gate 2, and the upper material 42 covers the side of the lower material 41 facing away from the dielectric layer 3, and the source 5 and the drain 6 cover a part of the side of the upper material 42 facing away from the lower material 41. In this embodiment, the drain 6 and the source 5 cover the left and right sides of the upper material 42.
[0033] Alternatively, if Figure 1 As shown, the material of the substrate 1 is polyimide with a thickness of 0.05 mm. The material of the gate 2 is indium tin oxide with a film thickness of 200 nanometers, the resistance of indium tin oxide is less than 10 ohms, and the visible light transmittance of indium tin oxide is greater than 90%. The material of the dielectric layer 3 is polyvinyl pyrrolidone with a film thickness of 700 nanometers. The lower layer material 41 of the organic small molecule semiconductor heterojunction 4 is 8-benzothiophene dimethylbenzothiophene (C8-BTBT) with a thickness of 30 nanometers; the upper layer material 42 of the organic small molecule semiconductor heterojunction 4 is pentacene with a thickness of 20 nanometers. The upper layer material 42, the source 5 and the drain 6 of the organic small molecule semiconductor heterojunction 4 all have a forked structure, the length of the forked structure is 1.5 mm, the width is 0.1 mm, and the distance between the fingers is 0.1 mm. The source electrode 5 and the drain electrode 6 are both Au electrodes with a thickness of 70 nanometers. This structure can be used to achieve high responsiveness of the organic transistor array to ammonia and improve the stability of the sensor.
[0034] As another implementation of this embodiment, a method for preparing a flexible organic transistor array for ammonia detection is used to prepare a flexible organic transistor array for ammonia detection, and the specific steps are as follows:
[0035] Step 1: Immerse the polyimide substrate in acetone solution, ethanol solution and deionized water in turn, and then use an ultrasonic cleaner to ultrasonically treat the substrate for 20 minutes at room temperature. This process aims to use the solvent's dissolving ability and the physical impact of ultrasound to effectively remove various impurities, pollutants and possible organic residues adsorbed on the substrate surface, ensuring good adhesion between the subsequent process layer and the substrate surface. After ultrasonic treatment, use a nitrogen gun to blow dry the substrate to avoid using air drying to cause water and oxygen contamination again, ensuring that the substrate surface is clean and dry, ready for subsequent processes.
[0036] Then, a transparent conductive film is deposited on the surface of the substrate as an indium tin oxide electrode by DC magnetron sputtering, sol-gel method or vacuum thermal evaporation; DC magnetron sputtering: In a vacuum environment, atoms or ions in indium tin oxide are bombarded out and deposited on the substrate through a magnetic field-assisted sputtering process to form a uniform, continuous and transparent conductive film.
[0037] Sol-gel method: Through chemical reactions such as hydrolysis and condensation of metal salts or metal oxide precursors in the solution, a sol is formed, which is then converted into a dense transparent conductive oxide film through drying and heat treatment.
[0038] Vacuum thermal evaporation: Under high vacuum conditions, conductive materials (such as aluminum, gold, silver, etc.) are heated and evaporated, condensed and deposited on the substrate to form a transparent conductive film. This method is suitable for preparing thinner metal films, and sometimes a transparent dielectric layer is combined to form a composite structure to improve transparency.
[0039] Step 2: Mix polyvinyl pyrrolidone particles, methylated poly (melamine-co-formaldehyde) crosslinker and propylene glycol methyl ether acetate solution in a mass ratio of 2:1:6 to 2:1:14 in a magnetic stirrer to prepare a polyvinyl pyrrolidone solution; the methylated poly (melamine-co-formaldehyde) crosslinker plays a role in enhancing the crosslinking degree and stability of the polyvinyl pyrrolidone film.
[0040] Step 3: Spin-coat the polyvinyl pyrrolidone solution on the side of the gate facing away from the substrate, and evenly disperse the solution through high-speed rotation to eventually form a uniform thin layer, and then heat the gate through an oven to form a dielectric layer on the side facing away from the substrate; the oven temperature, time and atmosphere need to be precisely controlled according to the characteristics of polyvinyl pyrrolidone and methylated poly (melamine-CO-formaldehyde) cross-linking agent to ensure the appropriate cross-linking degree and good electrical properties of the dielectric layer.
[0041] Step 4: 8-benzothiophene dimethyl benzothiophene (C8-BTBT) with a thickness of 30 nanometers is deposited on the side of the dielectric layer facing away from the gate by an organic vacuum thermal evaporation process, and then pentacene with a thickness of 20 nanometers is deposited on the side of the 8-benzothiophene dimethyl benzothiophene (C8-BTBT) facing away from the dielectric layer by an organic vacuum thermal evaporation process. The deposition rate of 8-benzothiophene dimethyl benzothiophene (C8-BTBT) is The substrate rotation speed is 5-20 r / min, the growth temperature is 130-170°C; the deposition rate of pentacene is The substrate rotation speed is 5 to 20 r / min, and the growth temperature is 170 to 250° C. The organic semiconductor material is heated and evaporated, and the deposition rate and thickness are precisely controlled to form a highly ordered and pure organic film.
[0042] Step 5: Deposit a metal film on the side of pentacene facing away from 8-benzothiophene dimethylbenzothiophene (C8-BTBT) by magnetron sputtering to form a source and a drain, thereby obtaining a flexible organic transistor array for ammonia detection.
[0043] Another embodiment, optionally, as Figure 1 As shown, the material of substrate 1 is polyethylene terephthalate, with a thickness of 0.175 mm. The material of gate 2 is indium tin oxide, with a film thickness of 300 nanometers, the resistance of indium tin oxide is less than 10 ohms, and the visible light transmittance of indium tin oxide is greater than 90%. The material of dielectric layer 3 is polyvinyl pyrrolidone, with a film thickness of 700 nanometers. The lower layer material 41 of the organic small molecule semiconductor heterojunction 4 is 8-benzothiophene dimethylbenzothiophene (C8-BTBT), with a thickness of 30 nanometers; the upper layer material 42 of the organic small molecule semiconductor heterojunction 4 is 6,13-bis (triisopropylsilylethynyl) pentacene (Tips-Pentacene), with a thickness of 70 nanometers. The upper layer material 42, source 5 and drain 6 of the organic small molecule semiconductor heterojunction 4 all have a finger structure, the length of the finger structure is 1.5 mm, the width is 0.1 mm, and the distance between the fingers is 0.1 mm. The source electrode 5 and the drain electrode 6 are both Au electrodes with a thickness of 70 nanometers. This structure can be used to achieve high responsiveness of the organic transistor array to ammonia and improve the stability of the sensor.
[0044] As another implementation of this embodiment, a method for preparing a flexible organic transistor array for ammonia detection is used to prepare a flexible organic transistor array for ammonia detection, and the specific steps are as follows:
[0045] Step 1: Immerse the polyethylene terephthalate substrate in acetone solution, ethanol solution and deionized water in turn, and then use an ultrasonic cleaner to ultrasonically treat the substrate for 20 minutes at room temperature. This process aims to use the solvent's dissolving ability and the physical impact of ultrasound to effectively remove various impurities, pollutants and possible organic residues adsorbed on the substrate surface, ensuring good adhesion between the subsequent process layer and the substrate surface. After ultrasonic treatment, use a nitrogen gun to blow dry the substrate to avoid using air drying to cause moisture and oxygen contamination again, ensuring that the substrate surface is clean and dry, ready for subsequent processes.
[0046] Then, a transparent conductive film is deposited on the surface of the substrate as an indium tin oxide electrode by DC magnetron sputtering, sol-gel method or vacuum thermal evaporation; DC magnetron sputtering: In a vacuum environment, atoms or ions in indium tin oxide are bombarded out and deposited on the substrate through a magnetic field-assisted sputtering process to form a uniform, continuous and transparent conductive film.
[0047] Sol-gel method: Through chemical reactions such as hydrolysis and condensation of metal salts or metal oxide precursors in the solution, a sol is formed, which is then converted into a dense transparent conductive oxide film through drying and heat treatment.
[0048] Vacuum thermal evaporation: Under high vacuum conditions, conductive materials (such as aluminum, gold, silver, etc.) are heated and evaporated, condensed and deposited on the substrate to form a transparent conductive film. This method is suitable for preparing thinner metal films, and sometimes a transparent dielectric layer is combined to form a composite structure to improve transparency.
[0049] Step 2: Mix polyvinyl pyrrolidone particles, methylated poly (melamine-co-formaldehyde) crosslinker and propylene glycol methyl ether acetate solution in a mass ratio of 2:1:6 to 2:1:14 in a magnetic stirrer to prepare a polyvinyl pyrrolidone solution; the methylated poly (melamine-co-formaldehyde) crosslinker plays a role in enhancing the crosslinking degree and stability of the polyvinyl pyrrolidone film.
[0050] Step 3: Spin-coat the polyvinyl pyrrolidone solution on the side of the gate facing away from the substrate, and evenly disperse the solution through high-speed rotation to eventually form a uniform thin layer, and then heat the gate through an oven to form a dielectric layer on the side facing away from the substrate; the oven temperature, time and atmosphere need to be precisely controlled according to the characteristics of polyvinyl pyrrolidone and methylated poly (melamine-CO-formaldehyde) cross-linking agent to ensure the appropriate cross-linking degree and good electrical properties of the dielectric layer.
[0051] Step 4: 8-benzothiophene dimethyl benzothiophene (C8-BTBT) with a thickness of 30 nanometers is deposited on the side of the dielectric layer facing away from the gate by an organic vacuum thermal evaporation process, and then 6,13-bis(triisopropylsilylethynyl) pentacene (Tips-Pentacene) with a thickness of 20 nanometers is deposited on the side of the 8-benzothiophene dimethyl benzothiophene (C8-BTBT) facing away from the dielectric layer by an organic vacuum thermal evaporation process. The deposition rate of 8-benzothiophene dimethyl benzothiophene (C8-BTBT) is The substrate rotation speed is 5-20 r / min, the growth temperature is 130-170°C; the deposition rate of 6,13-bis(triisopropylsilylethynyl)pentacene is The substrate rotation speed is 5 to 20 r / min, and the growth temperature is 170 to 250° C. The organic semiconductor material is heated and evaporated, and the deposition rate and thickness are precisely controlled to form a highly ordered and pure organic film.
[0052] Step 5: A metal film is deposited on the side of 6,13-bis(triisopropylsilylethynyl)pentacene (Tips-Pentacene) facing away from 8-benzothiophene dimethylbenzothiophene (C8-BTBT) by magnetron sputtering to form a source and a drain, thereby obtaining a flexible organic transistor array for ammonia detection.
[0053] The ammonia response time current diagram of the flexible organic transistor array for ammonia detection prepared in this embodiment is shown in FIG. Figure 2 As shown in the figure, the horizontal axis is the response time to ammonia detection, and the vertical axis is the percentage response, which is calculated by subtracting the detection current from the original current and then dividing it by the detection current.
[0054] Another embodiment, optionally, as Figure 1 As shown, the material of substrate 1 is polyimide with a thickness of 0.125 mm. The material of gate 2 is indium tin oxide with a film thickness of 200 nanometers, the resistance of indium tin oxide is less than 10 ohms, and the visible light transmittance of indium tin oxide is greater than 90%. The material of dielectric layer 3 is polyvinyl pyrrolidone with a film thickness of 700 nanometers. The lower layer material 41 of organic small molecule semiconductor heterojunction 4 is 8-benzothiophene dimethylbenzothiophene (C8-BTBT) with a thickness of 30 nanometers; the upper layer material 42 of organic small molecule semiconductor heterojunction 4 is 2,9-didecylnaphtho[2,3-B:2′,3′-F]thienyl[3,2-B]thiophene (C10-DNTT) with a thickness of 50 nanometers. The upper layer material 42, source 5 and drain 6 of organic small molecule semiconductor heterojunction 4 all have a forked structure, the length of the forked structure is 1.5 mm, the width is 0.1 mm, and the distance between the fingers is 0.1 mm. The source electrode 5 and the drain electrode 6 are both Au electrodes with a thickness of 70 nanometers. This structure can be used to achieve high responsiveness of the organic transistor array to ammonia and improve the stability of the sensor.
[0055] As another implementation of this embodiment, a method for preparing a flexible organic transistor array for ammonia detection is used to prepare a flexible organic transistor array for ammonia detection, and the specific steps are as follows:
[0056] Step 1: Immerse the polyethylene terephthalate substrate in acetone solution, ethanol solution and deionized water in turn, and then use an ultrasonic cleaner to ultrasonically treat the substrate for 20 minutes at room temperature. This process aims to use the solvent's dissolving ability and the physical impact of ultrasound to effectively remove various impurities, pollutants and possible organic residues adsorbed on the substrate surface, ensuring good adhesion between the subsequent process layer and the substrate surface. After ultrasonic treatment, use a nitrogen gun to blow dry the substrate to avoid using air drying to cause moisture and oxygen contamination again, ensuring that the substrate surface is clean and dry, ready for subsequent processes.
[0057] Then, a transparent conductive film is deposited on the surface of the substrate as an indium tin oxide electrode by DC magnetron sputtering, sol-gel method or vacuum thermal evaporation; DC magnetron sputtering: In a vacuum environment, atoms or ions in indium tin oxide are bombarded out and deposited on the substrate through a magnetic field-assisted sputtering process to form a uniform, continuous and transparent conductive film.
[0058] Sol-gel method: Through chemical reactions such as hydrolysis and condensation of metal salts or metal oxide precursors in the solution, a sol is formed, which is then converted into a dense transparent conductive oxide film through drying and heat treatment.
[0059] Vacuum thermal evaporation: Under high vacuum conditions, conductive materials (such as aluminum, gold, silver, etc.) are heated and evaporated, condensed and deposited on the substrate to form a transparent conductive film. This method is suitable for preparing thinner metal films, and sometimes a transparent dielectric layer is combined to form a composite structure to improve transparency.
[0060] Step 2: Mix polyvinyl pyrrolidone particles, methylated poly (melamine-co-formaldehyde) crosslinker and propylene glycol methyl ether acetate solution in a mass ratio of 2:1:6 to 2:1:14 in a magnetic stirrer to prepare a polyvinyl pyrrolidone solution; the methylated poly (melamine-co-formaldehyde) crosslinker plays a role in enhancing the crosslinking degree and stability of the polyvinyl pyrrolidone film.
[0061] Step 3: Spin-coat the polyvinyl pyrrolidone solution on the side of the gate facing away from the substrate, and evenly disperse the solution through high-speed rotation to eventually form a uniform thin layer, and then heat the gate through an oven to form a dielectric layer on the side facing away from the substrate; the oven temperature, time and atmosphere need to be precisely controlled according to the characteristics of polyvinyl pyrrolidone and methylated poly (melamine-CO-formaldehyde) cross-linking agent to ensure the appropriate cross-linking degree and good electrical properties of the dielectric layer.
[0062] Step 4: 8-benzothiophene dimethylbenzothiophene (C8-BTBT) (C8-BTBT) with a thickness of 30 nanometers is deposited on the side of the dielectric layer facing away from the gate by an organic vacuum thermal evaporation process, and then 2,9-didecylnaphtho[2,3-B:2′,3′-F]thieno[3,2-B]thiophene (C10-DNTT) with a thickness of 50 nanometers is deposited on the side of 8-benzothiophene dimethylbenzothiophene (C8-BTBT) (C8-BTBT) facing away from the dielectric layer by an organic vacuum thermal evaporation process. The deposition rate of 8-benzothiophene dimethylbenzothiophene (C8-BTBT) (C8-BTBT) is The substrate rotation speed is 5-20 r / min, the growth temperature is 130-170°C; the deposition rate of 2,9-didecylnaphtho[2,3-B:2′,3′-F]thieno[3,2-B]thiophene (C10-DNTT) is The substrate rotation speed is 5 to 20 r / min, and the growth temperature is 170 to 250° C. The organic semiconductor material is heated and evaporated, and the deposition rate and thickness are precisely controlled to form a highly ordered and pure organic film.
[0063] Step 5: A metal film is deposited on the side of 2,9-didecylnaphtho[2,3-B:2′,3′-F]thieno[3,2-B]thiophene (C10-DNTT) facing away from 8-benzothiophenedimethylbenzothiophene (C8-BTBT) (C8-BTBT) by magnetron sputtering to form a source and a drain, thereby obtaining a flexible organic transistor array for ammonia detection.
[0064] Another embodiment, optionally, as Figure 1 As shown, the material of the substrate 1 is polyethylene terephthalate, with a thickness of 0.175 mm. The material of the gate 2 is indium tin oxide, with a film thickness of 200 nanometers, the resistance of indium tin oxide is less than 10 ohms, and the visible light transmittance of indium tin oxide is greater than 90%. The material of the dielectric layer 3 is polyvinyl pyrrolidone, with a film thickness of 700 nanometers. The lower layer material 41 of the organic small molecule semiconductor heterojunction 4 is 8-benzothiophene dimethylbenzothiophene (C8-BTBT), with a thickness of 50 nanometers; the upper layer material 42 of the organic small molecule semiconductor heterojunction 4 is dinaphtho[2,3-B:2′,3′-F]thieno[3,2-B]thiophene (DNTT), with a thickness of 80 nanometers. The upper layer material 42, source electrode 5 and drain electrode 6 of the organic small molecule semiconductor heterojunction 4 all have a forked structure, the length of the forked structure is 1.5 mm, the width is 0.1 mm, and the distance between the fingers is 0.1 mm. The source electrode 5 and the drain electrode 6 are both Au electrodes with a thickness of 70 nanometers. This structure can be used to achieve high responsiveness of the organic transistor array to ammonia and improve the stability of the sensor.
[0065] As another implementation of this embodiment, a method for preparing a flexible organic transistor array for ammonia detection is used to prepare a flexible organic transistor array for ammonia detection, and the specific steps are as follows:
[0066] Step 1: Immerse the polyethylene terephthalate substrate in acetone solution, ethanol solution and deionized water in turn, and then use an ultrasonic cleaner to ultrasonically treat the substrate for 20 minutes at room temperature. This process aims to use the solvent's dissolving ability and the physical impact of ultrasound to effectively remove various impurities, pollutants and possible organic residues adsorbed on the substrate surface, ensuring good adhesion between the subsequent process layer and the substrate surface. After ultrasonic treatment, use a nitrogen gun to blow dry the substrate to avoid using air drying to cause moisture and oxygen contamination again, ensuring that the substrate surface is clean and dry, ready for subsequent processes.
[0067] Then, a transparent conductive film is deposited on the surface of the substrate as an indium tin oxide electrode by DC magnetron sputtering, sol-gel method or vacuum thermal evaporation; DC magnetron sputtering: In a vacuum environment, atoms or ions in indium tin oxide are bombarded out and deposited on the substrate through a magnetic field-assisted sputtering process to form a uniform, continuous and transparent conductive film.
[0068] Sol-gel method: Through chemical reactions such as hydrolysis and condensation of metal salts or metal oxide precursors in the solution, a sol is formed, which is then converted into a dense transparent conductive oxide film through drying and heat treatment.
[0069] Vacuum thermal evaporation: Under high vacuum conditions, conductive materials (such as aluminum, gold, silver, etc.) are heated and evaporated, condensed and deposited on the substrate to form a transparent conductive film. This method is suitable for preparing thinner metal films, and sometimes a transparent dielectric layer is combined to form a composite structure to improve transparency.
[0070] Step 2: Mix polyvinyl pyrrolidone particles, methylated poly (melamine-co-formaldehyde) crosslinker and propylene glycol methyl ether acetate solution in a mass ratio of 2:1:6 to 2:1:14 in a magnetic stirrer to prepare a polyvinyl pyrrolidone solution; the methylated poly (melamine-co-formaldehyde) crosslinker plays a role in enhancing the crosslinking degree and stability of the polyvinyl pyrrolidone film.
[0071] Step 3: Spin-coat the polyvinyl pyrrolidone solution on the side of the gate facing away from the substrate, and evenly disperse the solution through high-speed rotation to eventually form a uniform thin layer, and then heat the gate through an oven to form a dielectric layer on the side facing away from the substrate; the oven temperature, time and atmosphere need to be precisely controlled according to the characteristics of polyvinyl pyrrolidone and methylated poly (melamine-CO-formaldehyde) cross-linking agent to ensure the appropriate cross-linking degree and good electrical properties of the dielectric layer.
[0072] Step 4: 8-benzothiophene dimethylbenzothiophene (C8-BTBT) with a thickness of 30 nanometers is deposited on the side of the dielectric layer facing away from the gate by an organic vacuum thermal evaporation process, and then dinaphtho[2,3-B:2′,3′-F]thieno[3,2-B]thiophene (DNTT) with a thickness of 80 nanometers is deposited on the side of 8-benzothiophene dimethylbenzothiophene (C8-BTBT) facing away from the dielectric layer by an organic vacuum thermal evaporation process. The deposition rate of 8-benzothiophene dimethylbenzothiophene (C8-BTBT) is The substrate rotation speed is 5-20 r / min, the growth temperature is 130-170°C; the deposition rate of dinaphtho[2,3-B:2′,3′-F]thieno[3,2-B]thiophene (DNTT) is The substrate rotation speed is 5 to 20 r / min, and the growth temperature is 170 to 250° C. The organic semiconductor material is heated and evaporated, and the deposition rate and thickness are precisely controlled to form a highly ordered and pure organic film.
[0073] Step 5: A metal film is deposited on the side of dinaphtho[2,3-B:2′,3′-F]thieno[3,2-B]thiophene (DNTT) facing away from 8-benzothiophene dimethylbenzothiophene (C8-BTBT) by magnetron sputtering to form a source and a drain, thereby obtaining a flexible organic transistor array for ammonia detection.
[0074] As another implementation of this embodiment, an ammonia detection device includes a flexible organic transistor array for ammonia detection. Preferably, the ammonia detection device can be fixed or portable, and the portable device can be a wearable device or a handheld device. The wearable device is one of a smart watch, a smart bracelet, smart glasses, smart headphones, smart clothing, a pedometer and smart shoes; the handheld device is one of a smart phone, a smart tablet computer, a handheld game console, an e-book, an RFID handheld terminal and a camera.
[0075] In the above embodiments, the flexible organic transistor array for ammonia detection described in the present invention contains different bio-friendly materials and is suitable for portable sensors, human skin devices, bionic electronic devices and other fields. At the same time, no high-temperature treatment occurs during the preparation of the device, the preparation cost is low, and it is suitable for large-scale mass production.
[0076] Although the embodiments of the present invention are described in detail above, it is obvious to those skilled in the art that various modifications and variations can be made to these embodiments. However, it should be understood that such modifications and variations are within the scope and spirit of the present invention as described in the claims. Moreover, the present invention described herein may have other embodiments and may be implemented or realized in a variety of ways.
[0077] Although the embodiments of the present invention are described in detail above, it is obvious to those skilled in the art that various modifications and variations can be made to these embodiments. However, it should be understood that such modifications and variations are within the scope and spirit of the present invention as described in the claims. Moreover, the present invention described herein may have other embodiments and may be implemented or realized in a variety of ways.
Claims
1. A flexible organic transistor array for ammonia detection, used to detect ammonia, It is characterized in that It includes a substrate, a gate, a dielectric layer, an organic small molecule semiconductor heterojunction, a source electrode and a drain electrode, wherein the gate covers one side of the substrate, and the dielectric layer covers the side of the gate facing away from the substrate; the organic small molecule semiconductor heterojunction includes an upper layer material and a lower layer material, wherein the lower layer material covers the side of the dielectric layer facing away from the gate, the upper layer material covers the side of the lower layer material facing away from the dielectric layer, and the source electrode and the drain electrode cover a part of the side of the upper layer material facing away from the lower layer material.
2. The flexible organic transistor array for ammonia detection according to claim 1, It is characterized in that The material of the substrate is polyethylene terephthalate or polyimide, and the thickness of the polyethylene terephthalate or the polyimide is 0.05-0.175 mm.
3. The flexible organic transistor array for ammonia detection according to claim 1, It is characterized in that The material of the gate is indium tin oxide, and the film thickness of the indium tin oxide is 200-300 nanometers.
4. The flexible organic transistor array for ammonia detection according to claim 1, It is characterized in that The material of the dielectric layer is polyvinyl pyrrolidone, and the film thickness of the polyvinyl pyrrolidone is 600-900 nanometers.
5. The flexible organic transistor array for ammonia detection according to claim 1, It is characterized in that The lower layer material is 8-benzothiophene dimethylbenzothiophene, and the thickness of the 8-benzothiophene dimethylbenzothiophene is 30 to 50 nanometers.
6. The flexible organic transistor array for ammonia detection according to claim 5, It is characterized in that The upper layer material is any one of pentacene, 6,13-bis(triisopropylsilylethynyl)pentacene, 2,9-didecylnaphtho[2,3-B:2′,3′-F]thieno[3,2-B]thiophene and dinaphtho[2,3-B:2′,3′-F]thieno[3,2-B]thiophene, and the thickness of the upper layer material is 10 to 100 nanometers.
7. The flexible organic transistor array for ammonia detection according to claim 1, It is characterized in that The source and drain are Au electrodes, and the thickness of the Au electrodes is 70 nanometers.
8. The flexible organic transistor array for ammonia detection according to claim 6 or 7, It is characterized in that The upper layer material, the source electrode and the drain electrode are all interdigitated structures.
9. A method for preparing a flexible organic transistor array for ammonia detection, It is characterized in that The specific steps are as follows: Step 1: providing a substrate, and depositing a transparent conductive film as a gate on the surface of the substrate by DC magnetron sputtering, sol-gel method or vacuum thermal evaporation; Step 2: Mixing polyvinyl pyrrolidone particles, methylated poly (melamine-CO-formaldehyde) crosslinking agent and propylene glycol methyl ether acetate solution in a mass ratio of 2:1:6 to 2:1:14 in a magnetic stirrer to prepare a polyvinyl pyrrolidone solution; Step 3: Spin-coating the polyvinyl pyrrolidone solution on the side of the gate facing away from the substrate, and then heating in an oven to form a dielectric layer; Step 4: depositing an organic semiconductor heterojunction on a side of the dielectric layer facing away from the gate by an organic vacuum thermal evaporation process, wherein the organic small molecule semiconductor heterojunction comprises an upper layer material and a lower layer material, wherein the lower layer material covers a side of the dielectric layer facing away from the gate, and the upper layer material covers a side of the lower layer material facing away from the dielectric layer; Step 5: Deposit a metal film on the side of the upper layer material facing away from the lower layer material by magnetron sputtering to form a source electrode and a drain electrode, thereby obtaining a flexible organic transistor array for ammonia detection.
10. The method for preparing the flexible organic transistor array for ammonia detection according to claim 9, It is characterized in that Before executing step 1, the substrate sheet is immersed in acetone solution, ethanol solution and deionized water in turn, and then the substrate sheet is ultrasonically treated using an ultrasonic cleaner at room temperature, and then the substrate is blown dry using a nitrogen gun after the ultrasonic treatment.
11. The method for preparing the flexible organic transistor array for ammonia detection according to claim 10, It is characterized in that The material of the substrate in step 1 is polyethylene terephthalate or polyimide, and the thickness of the polyethylene terephthalate or the polyimide is 0.05 to 0.175 mm.
12. The method for preparing the flexible organic transistor array for ammonia detection according to claim 9, It is characterized in that The material of the gate in step 1 is indium tin oxide, and the film thickness of the indium tin oxide is 200-300 nanometers.
13. The method for preparing the flexible organic transistor array for ammonia detection according to claim 9, It is characterized in that The material of the dielectric layer in step 3 is polyvinyl pyrrolidone, and the film thickness of the polyvinyl pyrrolidone is 600-900 nanometers.
14. The method for preparing a flexible organic transistor array for ammonia detection according to claim 9, It is characterized in that The lower layer material in step 4 is 8-benzothiophene dimethylbenzothiophene, and the thickness of the 8-benzothiophene dimethylbenzothiophene is 30 to 50 nanometers.
15. The method for preparing a flexible organic transistor array for ammonia detection according to claim 9, It is characterized in that The upper layer material in step 4 is any one of pentacene, 6,13-bis(triisopropylsilylethynyl)pentacene, 2,9-didecylnaphtho[2,3-B:2′,3′-F]thieno[3,2-B]thiophene and dinaphtho[2,3-B:2′,3′-F]thieno[3,2-B]thiophene, and the thickness of the upper layer material is 10 to 100 nanometers.
16. The method for preparing a flexible organic transistor array for ammonia detection according to claim 9, It is characterized in that The source and drain in step 5 are Au electrodes, and the thickness of the Au electrodes is 70 nanometers.