Perovskite solar cell with self-organizing monomolecular layer hole transport material
By using self-assembled single-layer hole transport materials in perovskite solar cells, the conjugated structure of halogen and carbazole derivatives is used to solve the hole transport layer efficiency and stability problems, and the perovskite solar cells are improved performance and stability, suitable for large-scale applications.
Patent Information
- Application Number
- CN202411039891.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-08
AI Technical Summary
The hole transport efficiency of the hole transport layer in the existing perovskite solar cells is low and the thermal stability is poor, especially under ultraviolet light irradiation, which leads to a decrease in device performance and stability, limiting the industrial application of materials.
Self-assembled single-layer hole transport material, using benzene ring or naphthalene or biphenyl with halogen as the linking group as the anchoring group, carbazole or carbazole derivative as the functional group, through conjugated structure and coupling Extreme moment regulation improves hole transmission efficiency and thermal stability.
It significantly improves the hole transport efficiency and thermal stability of the hole transport layer, enhances the performance and stability of perovskite solar cells, and is suitable for large-scale applications.
Smart Images

Figure BDA0004972114780000021 
Figure BDA0004972114780000031 
Figure BDA0004972114780000032
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of perovskite solar cells, and in particular to a perovskite solar cell with a self-organized monomolecular layer of hole transport material. Background Art
[0002] Perovskite solar cells are solar cells that use perovskite-type organic metal halide semiconductors as light-absorbing materials. They belong to the third generation of solar cells, also known as new concept solar cells. As a new generation of photovoltaic technology, perovskite solar cells (PSCs) have the advantages of simple preparation process, easy material adjustment, and low cost. The latest certified efficiency has reached 26.2% (National Renewable Energy Laboratory, NREL, 2023).
[0003] There are two main structural types of perovskite solar cells, one is the forward nip structure and the other is the reverse pin structure. Compared with the nip structure, the pin structure is more suitable for the production of large-area, stacked solar cells because it can use low-temperature processes and a wider variety of carrier extraction layers, and has a higher commercial prospect. However, the pin structure also faces a challenge, which is how to improve the interface quality and stability between the hole selective layer and the perovskite. At present, the hole transport materials (HTMs) commonly used for inverse devices are inorganic materials nickel oxide (NiO x ) and organic polymer materials, poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] (PTAA). Among them, there are energy level mismatch and defect states between nickel oxide and perovskite, resulting in voltage loss and interface degradation; PTAA is expensive, product batch instability and low film wettability, all of which limit the further improvement of device performance. Therefore, the development of high-performance, new hole transport materials for inverse devices is crucial to the performance of the device.
[0004] As hole transport materials, self-assembled monolayers (SAMs) have the characteristics of simple structure and flexible design, and can effectively adjust the interface energy level and reduce defect states based on molecular engineering. At the same time, this type of material also exhibits unique advantages such as low parasitic absorption, low material consumption, compatibility with stacked perovskite solar cells, and simplified large-area device manufacturing, and has become a popular choice for the preparation of high-efficiency perovskite solar cells.
[0005] At present, SAM materials often use organic molecules composed of anchoring groups (phosphate, carboxylic acid, boric acid, thiol, etc.) and aromatic groups (such as carbazole). Alkyl groups are used to connect the anchoring groups and aromatic groups. The insulating properties of the alkyl groups lead to poor stability of the entire molecule to ultraviolet light, resulting in low hole transfer efficiency. Under the irradiation of sunlight, ultraviolet rays will cause the molecules themselves to degrade, resulting in deep energy level defects in perovskites, which seriously reduce the performance and stability of the device. Especially for wide-bandgap perovskites suitable for the preparation of stacked cells, phase separation is prone to occur under ultraviolet light, resulting in large open-circuit voltage losses, thereby affecting the photoelectric properties of the material. Therefore, the development of new SAM materials with simple structure, low cost and excellent performance is a key issue that needs to be solved to promote the industrialization of PSCs. Summary of the invention
[0006] In order to overcome the shortcomings of the prior art, the present invention provides a perovskite solar cell with a self-organized monolayer hole transport material to solve the above-mentioned traditional technical problems. The hole transport layer is changed by self-assembling a monolayer hole transport material to improve the shortcomings of the hole transport layer, such as low hole transport efficiency and poor thermal stability. The perovskite solar cell has the characteristics of simple structure, high hole transport property, high thermal stability and suitability for large-scale applications.
[0007] The present invention is implemented by the following technical solutions:
[0008] A perovskite solar cell with a self-organized monomolecular layer of hole transport material, comprising from top to bottom a transparent conductive substrate, an electron transport layer, a perovskite light absorption layer, a hole transport layer and a metal electrode;
[0009] Wherein, the hole transport layer is made of a self-organized monolayer hole transport material; the self-organized monolayer hole transport material has the following structural formulas (I), (II), and (III):
[0010]
[0011] Wherein, in formula (I), R 11 is carbazole or a carbazole derivative, R 12 -R 13 is hydrogen, R 14 -R 15 is a halogen;
[0012] In formula (II), R 21 is carbazole or a carbazole derivative, R 22 -R 27 is hydrogen and / or halogen;
[0013] In formula (III), R 31 is carbazole or a carbazole derivative, R32 -R 39 is hydrogen and / or halogen.
[0014] The hole transport layer in the above-mentioned perovskite solar cell improves its performance through a self-organized monolayer hole transport material. The hole transport material uses a benzene ring or naphthalene or biphenyl with a halogen as a substituent as a connecting group, phosphoric acid as an anchoring group, and carbazole or a carbazole derivative as a functional group. The self-assembly and photoelectric properties of this type of material are regulated by the characteristics of the connecting group to change the entire molecular dipole moment, thereby enhancing the thermal stability of the self-organized monolayer.
[0015] Furthermore, in formula (I), the halogen is one of fluorine (F), chlorine (Cl), bromine (Br), and iodine (I). Due to the conjugated structure of the benzene ring and the functional group, the disadvantage of low hole transport efficiency of the hole transport layer can be improved. At the same time, the benzene ring is easier to modify than the alkyl chain, and some halogen-containing electron-absorbing groups are modified on the benzene ring to increase the dipole moment of the molecule, thereby further enhancing the hole transport efficiency of the self-assembled monolayer. At the same time, the molecular thermal vibration of the benzene ring is much lower than that of the traditional alkyl linking group, which can greatly enhance the thermal stability of the self-assembled monolayer.
[0016] More preferably, the halogen is fluorine (F).
[0017] More preferably, in formula (II), R 22 -R 27 For hydrogen.
[0018] More preferably, in formula (III), R 32 -R 39 For hydrogen.
[0019] Furthermore, the structural formula of formula (I) includes but is not limited to any one of the compounds shown in formula (1) to formula (3):
[0020]
[0021] Furthermore, the structural formula of formula (II) includes but is not limited to any one of the compounds shown in formula (4) to formula (6):
[0022]
[0023] Furthermore, the structural formula of formula (III) includes but is not limited to any one of the compounds shown in formula (7) to formula (9):
[0024]
[0025] Furthermore, the preparation steps of the self-organized monolayer hole transport material are:
[0026] S1: Synthesis of intermediates
[0027] Under a nitrogen atmosphere, the first compound and the second compound are dissolved in N,N'-dimethylacetamide, followed by adding potassium carbonate and cuprous iodide, reacting at 160°C-200°C for 20h-26h, and cooling to room temperature after the reaction is completed; then, diluting with water, and then extracting with dichloromethane, drying the organic layer with anhydrous magnesium sulfate, filtering and spin-drying, and separating the crude product with silica gel column chromatography to obtain an intermediate;
[0028] The first compound is carbazole or a carbazole derivative; the second compound is
[0029] One of them, R 12 -R 13 is hydrogen, R 14 -R 15 is halogen, R 22 -R 27 is hydrogen and / or halogen, R 32 -R 39 is hydrogen and / or halogen;
[0030] S2: In a dried round-bottom flask, the intermediate is dissolved in dichloromethane. At room temperature, trimethylsilyl bromide is dropped into the well-stirred mixture. After 10 h to 16 h, the mixture is transferred to a round-bottom flask and concentrated under reduced pressure. A magnetic stirring bar and methanol are then added in sequence. The mixture is stirred at room temperature. The mixture is then filtered, rinsed with methanol, and the combined filtrate is concentrated under reduced pressure to obtain the product.
[0031] Further, in step S1, the molar ratio of the first compound to the second compound, potassium carbonate and cuprous iodide is 1:(1-1.1):(1.5-2):(1.5-2).
[0032] Further preferably, in step S1, the molar ratio of the first compound to the second compound, potassium carbonate and cuprous iodide is 3:3.1:6:6.
[0033] Further, in step S2, the molar ratio of the intermediate to trimethylsilyl bromide is 1:(3-4).
[0034] Further preferably, in step S2, the molar ratio of the intermediate to trimethylsilyl bromide is 1:4.
[0035] Furthermore, the transparent conductive substrate is fluorine-doped tin oxide (FTO) or indium-doped tin oxide (ITO); the perovskite light absorption layer is made of perovskite material; and the metal electrode is gold (Au) or silver (Ag).
[0036] Furthermore, the thickness of the transparent conductive substrate is 100-800 nm, the thickness of the electron transport layer is 10-50 nm, the thickness of the hole transport layer is 1-100 nm, and the thickness of the metal electrode is 100-240 nm.
[0037] Furthermore, the preparation steps of the perovskite solar cell are:
[0038] (1) Processing of transparent conductive substrates
[0039] A FTO / ITO transparent conductive material (thickness 600 nm) with an area of 2.5 cm×2.5 cm was ultrasonically cleaned for 30 min using a transparent glass cleaning agent, deionized water, acetone, and isopropanol in sequence, and then placed in an oven at 80°C for drying, cooled, and then treated with an ultraviolet ozone cleaning machine for 20 min to obtain a treated transparent conductive substrate;
[0040] (2) Preparation of hole transport layer
[0041] Take 100 μL of 3 mg / mL ethanol dispersion droplets of the above self-organized single-molecule hole transport material on the FTO substrate whose surface has been treated with UV ozone, spin coat it at 4000 r / min, 60 s to form a film, and then place it on a heating plate at 100°C and dry it for 10 min.
[0042] (3) Preparation of perovskite light absorbing layer
[0043] FAI (228.76 mg), PbI2 (613.13 mg), MABr (7.84 mg), PbBr2 (25.69 mg) and MACl (33 mg) were mixed in 1 mL of DMF / DMSO (volume ratio 8:1), stirred at 60 ° C for 2 hours for use. The perovskite precursor solution was spread on the hole transport layer prepared above, first spin-coated at 1000 rpm for 10 seconds, and then spin-coated at 4000 rpm for 30 seconds; when the spin-coating countdown was 15 seconds, 1 mL of ether anti-solvent was quickly added on the film sample, and heated at 150 ° C for 20 minutes after the spin coating was completed to form a high-quality perovskite layer.
[0044] (4) Preparation of electron transport layer and counter electrode
[0045] The sample was then transferred to a vacuum evaporator and 30 nm C 60 , 5nm BCP and 120nm silver / gold counter electrode layer.
[0046] Compared with the prior art, the present invention has the following beneficial effects:
[0047] The hole transport layer in the perovskite solar cell of the present invention improves its performance through a self-organized monolayer hole transport material. The hole transport material uses a benzene ring or naphthalene or biphenyl with a halogen as a substituent as a connecting group, phosphoric acid as an anchoring group, and carbazole or a carbazole derivative as a functional group. The self-assembly and photoelectric properties of this type of material are regulated through the characteristics of the connecting group to change the entire molecular dipole moment, thereby enhancing the thermal stability of the self-organized monolayer. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 is the H NMR spectrum of compound SAM A-1;
[0049] Figure 2 is the H NMR spectrum of compound SAM A-2;
[0050] Figure 3 is the H NMR spectrum of compound SAM A-3;
[0051] Figure 4 is the H NMR spectrum of compound SAM B-1;
[0052] Figure 5 is the H NMR spectrum of compound SAM B-2;
[0053] Figure 6 is the H NMR spectrum of compound SAM B-3;
[0054] Figure 7 is the H NMR spectrum of compound SAM C-1;
[0055] Figure 8 is the H NMR spectrum of compound SAM C-2;
[0056] Fig. 9 is the H NMR spectrum of compound SAM C-3;
[0057] Fig.10 The IV curve of the solar cell prepared by using compound SAM A-1 as hole transport material;
[0058] Fig.11 The IV curve of the solar cell prepared by using compound SAM A-2 as hole transport material;
[0059] Fig.12 The IV curve of the solar cell prepared by using compound SAM A-3 as hole transport material;
[0060] Fig.13 The IV curve of the solar cell prepared by using compound SAM B-1 as hole transport material;
[0061] Fig.14 The IV curve of the solar cell prepared by using compound SAM B-2 as hole transport material;
[0062] Fig.15 The IV curve of the solar cell prepared by using compound SAM B-3 as hole transport material;
[0063] Fig.16 The IV curve of the solar cell prepared by using compound SAM C-1 as hole transport material;
[0064] Fig.17 The IV curve of the solar cell prepared by using compound SAM C-2 as hole transport material;
[0065] Fig.18 The IV curve of the solar cell prepared with compound SAM C-3 as hole transport material. DETAILED DESCRIPTION
[0066] The present invention is further described below in conjunction with specific implementation methods. It should be noted that, under the premise of no conflict, the various embodiments or technical features described below can be arbitrarily combined to form a new embodiment.
[0067] Example 1
[0068] The synthesis of the self-assembled monolayer hole transport material SAM A-1 is as follows:
[0069]
[0070] Step 1: Synthesis of intermediate 1
[0071] Under nitrogen atmosphere, raw material 1 (0.58 g, 3.0 mmol) and raw material 2 (1.01 g, 3.1 mmol) were dissolved in 25 mL N, N'-dimethylacetamide, followed by the addition of K2CO3 (0.83 g, 6.0 mmol) and cuprous iodide (0.06 g, 6.0 mmol). The reaction mixture was reacted at 180 ° C for 24 h. After the reaction was completed, it was cooled to room temperature. It was diluted with water and then extracted with dichloromethane. The organic layer was dried over anhydrous magnesium sulfate, filtered and dried. The crude product was separated by silica gel column chromatography to obtain a white solid (0.72 g, 62%).
[0072] After testing: 1H NMR (500MHz, CDCl3) δ=8.02–7.89(m,2H),7.75(d,J=7.5Hz,2H),7.30(dd,J=7.3,4.0Hz, 2H), 7.17 (dd, J=7.5, 1.3Hz, 2H), 4.22–3.97 (m, 4H), 2.50 (s, 6H), 1.20 (t, J=8.0Hz, 6H).
[0073] Step 2: Synthesis of compound SAM A-1
[0074] In a 50 mL oven-dried round-bottom flask, intermediate 1 (0.43 g, 1 mmol) was dissolved in 20 mL of dichloromethane. Trimethylsilyl bromide (0.612 g, 0.528 mL, 4 mmol) was added dropwise to the stirred mixture at room temperature. After 12 hours, the mixture was carefully transferred to a 100 mL round-bottom flask and concentrated under reduced pressure. A magnetic stirring bar and 20 mL of methanol were then added in sequence. The mixture was stirred at room temperature for 4 hours, the mixture was filtered, rinsed with methanol (3×5 mL), and the combined filtrate was concentrated under reduced pressure to obtain a solid as a crude product. Recrystallization from methanol / dichloromethane / ether gave a white solid (0.25 g, 65%).
[0075] After testing: Figure 1 As shown, 1 H NMR (500MHz, DMSO-d6) δ7.51(d,J=5.8Hz,2H),7.46(d,J=2.2Hz,2H),7.22(dd,J=8.5,2.2Hz,2H),6.74(d,J=8.5Hz,2H),1.47(s,6H)..ESI-MS(m / z):
[0076] [M+H] + calculated for C 20 H 17 NO3PF 388.08, found 388.08.
[0077] Example 2
[0078] The synthesis of the self-assembled monolayer hole transport material SAM A-2 is as follows:
[0079]
[0080] Step 1: Synthesis of intermediate 2
[0081] Under nitrogen atmosphere, raw material 3 (0.96 g, 3.0 mmol) and raw material 2 (1.01 g, 3.1 mmol) were dissolved in 25 mL N, N'-dimethylacetamide, followed by the addition of K2CO3 (0.83 g, 6.0 mmol) and cuprous iodide (0.06 g, 6.0 mmol). The reaction mixture was reacted at 180 ° C for 24 h. After the reaction was completed, it was cooled to room temperature. It was diluted with water and then extracted with dichloromethane. The organic layer was dried over anhydrous magnesium sulfate, filtered and dried. The crude product was separated by silica gel column chromatography to obtain a white solid (1.06 g, 66%).
[0082] After testing: 1 H NMR (500MHz, CDCl3) δ = 8.37 (s, 2H), 8.07 (d, J = 7.5Hz, 1H), 7.89 (d, J = 7.5Hz, 1H), 7.81–7.75 (m, 1H), 7.69–7.64 (m, 1H), 7.59 (dd, J=7.5, 1.9Hz, 4H), 7.44 (d, J=14.9Hz, 4H), 7.38–7.26 (m, 4H), 4.40–3.64 (m, 4H), 1.42–1.01 (m, 6H).
[0083] Step 2: Synthesis of compound SAM A-2
[0084] In a 50 mL oven-dried round-bottom flask, intermediate 2 (0.57 g, 1 mmol) was dissolved in 20 mL of dichloromethane. Trimethylsilyl bromide (0.612 g, 0.528 mL, 4 mmol) was added dropwise to the stirred mixture at room temperature. After 12 hours, the mixture was carefully transferred to a 100 mL round-bottom flask and concentrated under reduced pressure. A magnetic stirring bar and 20 ml of methanol were then added in sequence. The mixture was stirred at room temperature for 4 hours, the mixture was filtered, rinsed with methanol (3×5 mL), and the combined filtrate was concentrated under reduced pressure to obtain a solid as a crude product. Recrystallization from methanol / dichloromethane / ether gave a white solid (0.36 g, 70%).
[0085] After testing: Figure 2 As shown, 1 H NMR (500MHz, DMSO-d6) δ = 8.59 (s, 2H), 7.80 (d, J = 8.0Hz, 4H), 7.76–7.70 (m, 2H), 7.57 (d, J = 8.5Hz, 2H), 7.54–7.46 (m, 6H), 7.38–7.30 (m, 2H).
[0086] ESI-MS(m / z):[M+H] + calculated for C 30 H21 F2NO3P 512.11, found 512.11.
[0087] Example 3
[0088] The synthesis of the self-assembled monolayer hole transport material SAM A-3 is as follows:
[0089]
[0090] Step 1: Synthesis of intermediate 3
[0091] Under nitrogen atmosphere, raw material 4 (1.08 g, 3.0 mmol) and raw material 2 (1.01 g, 3.1 mmol) were dissolved in 25 mL N, N'-dimethylacetamide, followed by the addition of K2CO3 (0.83 g, 6.0 mmol) and cuprous iodide (0.06 g, 6.0 mmol). The reaction mixture was reacted at 180 ° C for 24 h. After the reaction was completed, it was cooled to room temperature. It was diluted with water and then extracted with dichloromethane. The organic layer was dried over anhydrous magnesium sulfate, filtered and dried. The crude product was separated by silica gel column chromatography to obtain a white solid (0.92 g, 54%).
[0092] After testing: 1 H NMR (500MHz, CDCl3) δ = 7.46 (d, J = 1.9 Hz, 2H), 7.23 (dd, J = 7.5, 1.9 Hz, 2H), 6.85–6.78 (m,2H),6.75(d,J=7.5Hz,2H),4.30–3.90(m,4H),1.69(s,6H),1.21(t,J=8.0Hz,6H).
[0093] Step 2: Synthesis of compound SAM A-3
[0094] In a 50 mL oven-dried round-bottom flask, intermediate 3 (0.62 g, 1 mmol) was dissolved in 20 mL of dichloromethane. Trimethylsilyl bromide (0.612 g, 0.528 mL, 4 mmol) was added dropwise to the stirred mixture at room temperature. After 12 hours, the mixture was carefully transferred to a 100 mL round-bottom flask and concentrated under reduced pressure. A magnetic stirring bar and 20 mL of methanol were then added in sequence. The mixture was stirred at room temperature for 4 hours, the mixture was filtered, rinsed with methanol (3×5 mL), and the combined filtrate was concentrated under reduced pressure to obtain a solid as a crude product. Recrystallization from methanol / dichloromethane / ether gave a white solid (0.41 g, 67%).
[0095] After testing: Figure 3 As shown, 1H NMR (500MHz, DMSO-d6) δ7.83 (s, 2H), 7.51 (d, J = 5.8Hz, 2H), 7.32 (d, J = 8.2Hz, 2H), 7.16 (d, J = 9.4Hz, 2H), 2.45 (s, 6H). ESI-MS (m / z): [M+H] + calculated for C 21 H 27 NO3PBr2F2,557.92, found 557.92.
[0096] Example 4
[0097] The synthesis of the self-assembled monolayer hole transport material SAM B-1 is as follows:
[0098]
[0099] Step 1: Synthesis of intermediate 4
[0100] Under nitrogen atmosphere, raw material 1 (0.58 g, 3.0 mmol) and raw material 5 (1.07 g, 3.1 mmol) were dissolved in 25 mL N, N'-dimethylacetamide, followed by addition of K2CO3 (0.83 g, 6.0 mmol) and cuprous iodide (0.06 g, 6.0 mmol). The reaction mixture was reacted at 180 ° C for 24 h. After the reaction was completed, it was cooled to room temperature. It was diluted with water and then extracted with dichloromethane. The organic layer was dried over anhydrous magnesium sulfate, filtered and dried. The crude product was separated by silica gel column chromatography to obtain a white solid (0.93 g, 68%).
[0101] After testing: 1 H NMR (500MHz, CDCl3) δ = 8.50 (s, 1H), 8.35 (s, 1H), 8.12 (d, J = 7.5Hz, 1H), 8.09–8.02 (m, 2H), 7.99–7.97 (m, 1H), 7.94 (s,2H),7.81(d,J=7.5Hz,2H),7.17(dd,J=7.5,1.2Hz,2H),4.39–3.93(m,6H),2.50(s,6H),1.19(t,J=8.0Hz,6H).
[0102] Step 2: Synthesis of compound SAM B-1
[0103] In a 50 mL oven-dried round-bottom flask, intermediate 4 (0.46 g, 1 mmol) was dissolved in 20 mL of dichloromethane. Trimethylsilyl bromide (0.612 g, 0.528 mL, 4 mmol) was added dropwise to the stirred mixture at room temperature. After 12 hours, the mixture was carefully transferred to a 100 mL round-bottom flask and concentrated under reduced pressure. A magnetic stirring bar and 20 mL of methanol were then added in sequence. The mixture was stirred at room temperature for 4 hours, the mixture was filtered, rinsed with methanol (3×5 mL), and the combined filtrate was concentrated under reduced pressure to obtain a solid as a crude product. Recrystallization from methanol / dichloromethane / ether gave a white solid (0.29 g, 72%).
[0104] After testing: Figure 4 As shown, 1 H NMR (500MHz, DMSO-d6)δ=8.44(s,1H),8.22(s,1H),7.92–7.81(m,4H),7.72(d,J=8.7H z,2H),7.32(d,J=8.2Hz,2H),7.16(d,J=8.3Hz,2H),2.45(s,6H), ESI-MS(m / z):[M+H] + calculated for C 24 H 20 NO3P 401.12, found 401.12.
[0105] Example 5
[0106] The synthesis of the self-assembled monolayer hole transport material SAM B-2 is as follows:
[0107]
[0108] Step 1: Synthesis of intermediate 5
[0109] Under nitrogen atmosphere, raw material 3 (0.96 g, 3.0 mmol) and raw material 5 (1.07 g, 3.1 mmol) were dissolved in 25 mL N, N'-dimethylacetamide, followed by the addition of K2CO3 (0.83 g, 6.0 mmol) and cuprous iodide (0.06 g, 6.0 mmol). The reaction mixture was reacted at 180 ° C for 24 h. After the reaction was completed, it was cooled to room temperature. It was diluted with water and then extracted with dichloromethane. The organic layer was dried over anhydrous magnesium sulfate, filtered and dried. The crude product was separated by silica gel column chromatography to obtain a white solid (0.99 g, 57%).
[0110] After testing: 1H NMR (500MHz, CDCl3) δ = 8.47 (s, 1H), 8.38 (d, J = 8.0Hz, 3H), 8.11 (dd, J = 7.4, 4.3Hz, 2H), 8.04 (dt, J = 14.6, 8.0Hz, 3H), 7.97 (d, J = 7.5Hz, 1H), 7.84–7. 74(m,1H),7.71–7.65(m,1H),7.59(dd,J=7.5,1.9Hz,4H),7.44(t,J=7.4H z,4H),7.38–7.28(m,2H),4.43–3.71(m,4H),1.19(td,J=8.0,3.8Hz,6H).
[0111] Step 2: Synthesis of compound SAM B-2
[0112] In a 50 mL oven-dried round-bottom flask, intermediate 5 (0.58 g, 1 mmol) was dissolved in 20 mL of dichloromethane. Trimethylsilyl bromide (0.612 g, 0.528 mL, 4 mmol) was added dropwise to the stirred mixture at room temperature. After 12 hours, the mixture was carefully transferred to a 100 mL round-bottom flask and concentrated under reduced pressure. A magnetic stirring bar and 20 ml of methanol were then added in sequence. The mixture was stirred at room temperature for 4 hours, the mixture was filtered, rinsed with methanol (3×5 mL), and the combined filtrate was concentrated under reduced pressure to obtain a solid as a crude product. Recrystallization from methanol / dichloromethane / ether gave a white solid (0.41 g, 79%).
[0113] After testing: Figure 5 As shown, 1 H NMR (500MHz, DMSO-d6) δ = 8.60–8.58 (m, 2H), 8.44 (s, 1H), 8.24–8.20 (m, 1H), 7.88–7.82 (m, 2H), 7.79 (d, J = 7.8Hz, 4H), 7.76–7. 71(m,3H),7.67(dd,J=8.8,2.0Hz,1H),7.57(d,J=8.4Hz,2H),7.49(t,J=7.7Hz,4H),7.33(t,J=7.3Hz,2H).ESI-MS(m / z):[M+H] + calculated for C 34 H 25 NO3P 526.16, found 526.16.
[0114] Example 6
[0115] The synthesis of the self-assembled monolayer hole transport material SAM B-3 is as follows:
[0116]
[0117] Step 1: Synthesis of intermediate 3
[0118] Under nitrogen atmosphere, raw material 3 (1.08 g, 3.0 mmol) and raw material 5 (1.07 g, 3.1 mmol) were dissolved in 25 mL N, N'-dimethylacetamide, followed by the addition of K2CO3 (0.83 g, 6.0 mmol) and cuprous iodide (0.06 g, 6.0 mmol). The reaction mixture was reacted at 180 ° C for 24 h. After the reaction was completed, it was cooled to room temperature. It was diluted with water and then extracted with dichloromethane. The organic layer was dried over anhydrous magnesium sulfate, filtered and dried. The crude product was separated by silica gel column chromatography to obtain a white solid (1.172 g, 62%).
[0119] After testing: 1 H NMR (500MHz, CDCl3) δ = 8.30 (s, 1H), 7.93 (d, J = 9.6Hz, 2H), 7.72 (d, J = 8.5Hz, 1H), 7.61 (d, J = 7.5Hz, 1H ), 7.53 (s, 1H), 7.47 (d, J = 1.9Hz, 2H), 7.21 (dd, J = 7.5, 1.9Hz, 2H), 6.86 (d, J = 7.5Hz, 2H), 1.70 (s, 6H).
[0120] Step 2: Synthesis of compound SAM B-3
[0121] In a 50 mL oven-dried round-bottom flask, intermediate 6 (0.63 g, 1 mmol) was dissolved in 20 mL of dichloromethane. Trimethylsilyl bromide (0.612 g, 0.528 mL, 4 mmol) was added dropwise to the stirred mixture at room temperature. After 12 hours, the mixture was carefully transferred to a 100 mL round-bottom flask and concentrated under reduced pressure. A magnetic stirring bar and 20 mL of methanol were then added in sequence. The mixture was stirred at room temperature for 4 hours, the mixture was filtered, rinsed with methanol (3×5 mL), and the combined filtrate was concentrated under reduced pressure to obtain a solid as a crude product. Recrystallization from methanol / dichloromethane / ether gave a white solid (0.48 g, 77%).
[0122] After testing: Figure 6 As shown, 1H NMR (500MHz, DMSO-d6) δ8.40(s,1H),8.18(s,1H),7.81(t,J=10.0Hz,2H),7.69(d,J=8.8Hz,1H),7.65–7. 61(m,1H),7.42(s,2H),7.20–7.15(m,2H),6.70(dd,J=8.6,1.8Hz,2H),1.44(s,6H).ESI-MS(m / z):[M+H] + calculated for C 25 H 21 NO3PBr2
[0123] 571.95, found 571.95.
[0124] Example 7
[0125] The synthesis of the self-assembled monolayer hole transport material SAM C-1 is as follows:
[0126]
[0127] Step 1: Synthesis of intermediate 7
[0128] Under nitrogen atmosphere, raw material 1 (0.58 g, 3.0 mmol) and raw material 6 (1.14 g, 3.1 mmol) were dissolved in 25 mL N, N'-dimethylacetamide, followed by addition of K2CO3 (0.83 g, 6.0 mmol) and cuprous iodide (0.06 g, 6.0 mmol). The reaction mixture was reacted at 180 ° C for 24 h. After the reaction was completed, it was cooled to room temperature. Diluted with water and then extracted with dichloromethane. The organic layer was dried over anhydrous magnesium sulfate, filtered and dried. The crude product was separated by silica gel column chromatography to obtain a white solid (1.06 g, 73%).
[0129] After testing: 1 H NMR (500MHz, CDCl3) δ = 8.19 (d, J = 7.5Hz, 2H), 8.01 (dd, J = 13.4, 7.5Hz, 2H), 7.93 (d, J = 1.5Hz, 2H) ,7.84–7.69(m,6H),7.25–7.13(m,2H),4.07(p,J=8.1Hz,4H),2.50(s,6H),1.18(t,J=8.0Hz,6H).
[0130] Step 2: Synthesis of compound SAM C-1
[0131] In a 50 mL oven-dried round-bottom flask, intermediate 7 (0.48 g, 1 mmol) was dissolved in 20 mL of dichloromethane. Trimethylsilyl bromide (0.612 g, 0.528 mL, 4 mmol) was added dropwise to the stirred mixture at room temperature. After 12 hours, the mixture was carefully transferred to a 100 mL round-bottom flask and concentrated under reduced pressure. A magnetic stirring bar and 20 mL of methanol were then added in sequence. The mixture was stirred at room temperature for 4 hours, the mixture was filtered, rinsed with methanol (3×5 mL), and the combined filtrate was concentrated under reduced pressure to obtain a solid as a crude product. Recrystallization from methanol / dichloromethane / ether gave a white solid (0.29 g, 69%).
[0132] After testing: Figure 7 As shown, 1 H NMR (500MHz, DMSO-d6) δ=7.91–7.78(m,4H),7.64(q,J=8.4Hz,4H),7.48(d,J=8.3H z,2H),7.40–7.29(m,2H),7.17(d,J=8.3Hz,2H),2.45(s,6H).ESI-MS(m / z):[M+H] + calculated for C 26 H 23 NO3P 428.13, found 428.13.
[0133] Example 8
[0134] The synthesis of the self-assembled monolayer hole transport material SAM C-2 is as follows:
[0135]
[0136] Step 1: Synthesis of intermediate 8
[0137] Under nitrogen atmosphere, raw material 3 (0.96 g, 3.0 mmol) and raw material 6 (1.14 g, 3.1 mmol) were dissolved in 25 mL N, N'-dimethylacetamide, followed by the addition of K2CO3 (0.83 g, 6.0 mmol) and cuprous iodide (0.06 g, 6.0 mmol). The reaction mixture was reacted at 180 ° C for 24 h. After the reaction was completed, it was cooled to room temperature. It was diluted with water and then extracted with dichloromethane. The organic layer was dried over anhydrous magnesium sulfate, filtered and dried. The crude product was separated by silica gel column chromatography to obtain a white solid (1.11 g, 61%).
[0138] After testing: 1H NMR (500MHz, CDCl3) δ8.36(d,J=1.3Hz,2H),8.23(d,J=7.5Hz,2H),8.09(d,J=7.5Hz,1H),8.02–7.91(m,3H),7.85–7.74(m ,5H),7.71–7.63(m,1H),7.59(dd,J=7.5,1.9Hz,4H),7.44(t,J=7.4Hz,4H),7.36–7.29(m,2H),4.07(s,4H),1.21(s,6H).
[0139] Step 2: Synthesis of compound SAM C-2
[0140] In a 50 mL oven-dried round-bottom flask, intermediate 8 (0.61 g, 1 mmol) was dissolved in 20 mL of dichloromethane. Trimethylsilyl bromide (0.612 g, 0.528 mL, 4 mmol) was added dropwise to the stirred mixture at room temperature. After 12 hours, the mixture was carefully transferred to a 100 mL round-bottom flask and concentrated under reduced pressure. A magnetic stirring bar and 20 mL of methanol were then added in sequence. The mixture was stirred at room temperature for 4 hours, the mixture was filtered, rinsed with methanol (3×5 mL), and the combined filtrate was concentrated under reduced pressure to obtain a solid as a crude product. Recrystallization from methanol / dichloromethane / ether gave a white solid (0.40 g, 73%).
[0141] After testing: Figure 8 As shown, 1 H NMR (500MHz, DMSO-d6) δ = 8.58 (s, 2H), 7.86–7.77 (m, 6H), 7.75–7.70 (m, 2H), 7.67–7.5 5(m,6H),7.48(dt,J=8.2,4.4Hz,6H),7.33(td,J=7.3,2.8Hz,2H).ESI-MS(m / z):[M+H] + calculated for C 36 H 27 NO3P 552.17, found 552.17.
[0142] Example 9
[0143] The synthesis of the self-assembled monolayer hole transport material SAM C-3 is as follows:
[0144]
[0145] Step 1: Synthesis of intermediate 9
[0146] Under nitrogen atmosphere, raw material 4 (1.08 g, 3.0 mmol) and raw material 6 (1.14 g, 3.1 mmol) were dissolved in 25 mL N, N'-dimethylacetamide, followed by the addition of K2CO3 (0.83 g, 6.0 mmol) and cuprous iodide (0.06 g, 6.0 mmol). The reaction mixture was reacted at 180 ° C for 24 h. After the reaction was completed, it was cooled to room temperature. It was diluted with water and then extracted with dichloromethane. The organic layer was dried over anhydrous magnesium sulfate, filtered and dried. The crude product was separated by silica gel column chromatography to obtain a white solid (1.16 g, 59%).
[0147] After testing: 1 H NMR (500MHz, CDCl3) δ = 7.92 (dd, J = 13.3, 7.4Hz, 2H), 7.75 (dd, J = 7.5, 4.0Hz, 2H), 7.52 (s, 4H), 7.46 (d, J = 1 .9Hz,2H),7.34–7.18(m,2H),6.86(d,J=7.5Hz,2H),4.28–3.84(m,4H),1.69(s,6H),1.19(t,J=8.0Hz,6H).
[0148] Step 2: Synthesis of compound SAM C-3
[0149] In a 50 mL oven-dried round-bottom flask, intermediate 9 (0.65 g, 1 mmol) was dissolved in 20 mL of dichloromethane. Trimethylsilyl bromide (0.612 g, 0.528 mL, 4 mmol) was added dropwise to the stirred mixture at room temperature. After 12 hours, the mixture was carefully transferred to a 100 mL round-bottom flask and concentrated under reduced pressure. A magnetic stirring bar and 20 mL of methanol were then added in sequence. The mixture was stirred at room temperature for 4 hours, the mixture was filtered, rinsed with methanol (3×5 mL), and the combined filtrate was concentrated under reduced pressure to obtain a solid as a crude product. Recrystallization from methanol / dichloromethane / ether gave a white solid (0.46 g, 77%).
[0150] After testing: Fig. 9 As shown, 1 H NMR (500MHz, DMSO-d6) δ = 7.82 (dd, J = 8.5, 1.9Hz, 2H), 7.73–7.59 (m, 4H), 7.56–7.42 (m, 4 H),7.22(dd,J=8.5,2.0Hz,2H),6.74(d,J=8.5Hz,2H),1.47(s,6H).ESI-MS(m / z):[M+H] + calculated for C 27 H 23NO3PBr2 597.97, found 597.97.
[0151] Performance Testing
[0152] 1. Preparation of perovskite solar cells
[0153] (1) Processing of transparent FTO conductive substrate
[0154] The FTO transparent conductive material (thickness of 600 nm) with an area of 2.5 cm×2.5 cm was ultrasonically cleaned with a transparent glass cleaning agent, deionized water, acetone, and isopropanol for 30 minutes, then placed in an oven for drying at 80°C, cooled, and then treated with an ultraviolet ozone cleaning machine for 20 minutes to obtain a treated transparent conductive substrate.
[0155] (2) Preparation of hole transport layer
[0156] Take 100 μL of 3 mg / mL ethanol dispersion droplets of the above self-organized single-molecule hole transport material on the FTO substrate whose surface has been treated with UV ozone, spin coat it at 4000 r / min, 60 s to form a film, and then place it on a heating plate at 100°C and dry it for 10 minutes.
[0157] (3) Preparation of perovskite light absorbing layer
[0158] FAI (228.76 mg), PbI2 (613.13 mg), MABr (7.84 mg), PbBr2 (25.69 mg) and MACl (33 mg) were mixed in 1 mL of DMF / DMSO (volume ratio 8:1), stirred at 60 ° C for 2 hours for use. The perovskite precursor solution was spread on the hole transport layer prepared above, first spin-coated at 1000 rpm for 10 seconds, and then spin-coated at 4000 rpm for 30 seconds; when the spin-coating countdown was 15 seconds, 1 mL of ether anti-solvent was quickly added on the film sample, and heated at 150 ° C for 20 minutes after the spin coating was completed to form a high-quality perovskite layer.
[0159] (4) Preparation of electron transport layer and counter electrode
[0160] The sample was then transferred to a vacuum evaporator and 30 nm C 60 , 5nm BCP and 120nm silver counter electrode layer.
[0161] 2. The self-organized monolayer hole transport materials obtained in Examples 1 to 9 were applied to the performance test of perovskite solar cells, and the perovskite solar cells were prepared using the above preparation steps. The specific test results are as follows.
[0162] (1) Example 1 Self-assembled monolayer hole transport material SAM A-1
[0163] Test light source: SS-X50, data acquisition using Keithley 2400 digital source meter.
[0164] Test results see Fig.10 The open circuit voltage (Voc) of the perovskite solar cell is 1.16 V and the short circuit current density (Jsc) is 25.8 mA cm -2 , the fill factor (FF) is 0.790 and the photoelectric conversion efficiency is 22.9%.
[0165] (2) Example 2 Self-assembled monolayer hole transport material SAM A-2
[0166] Test light source: AM SS-X50, data acquisition using Keithley 2400 digital source meter.
[0167] Test results see Fig.11 The open circuit voltage (Voc) of the perovskite solar cell is 1.15 V and the short circuit current density (Jsc) is 25.8 mA cm -2 , the fill factor (FF) is 0.780 and the photoelectric conversion efficiency is 22.2%.
[0168] (3) Example 3 Self-assembled monolayer hole transport material SAM A-3
[0169] Test light source: SS-X50, data acquisition using Keithley 2400 digital source meter.
[0170] Test results see Fig.12 The open circuit voltage (Voc) of the perovskite solar cell is 1.17 V and the short circuit current density (Jsc) is 25.9 mA cm -2 , the fill factor (FF) is 0.797 and the photoelectric conversion efficiency is 23.4%.
[0171] (4) Example 4 Self-assembled monolayer hole transport material SAM B-1
[0172] Test light source: SS-X50, data acquisition using Keithley 2400 digital source meter.
[0173] Test results see Fig.13 The open circuit voltage (Voc) of the perovskite solar cell is 1.18 V and the short circuit current density (Jsc) is 23.4 mA cm -2 , the fill factor (FF) is 0.700 and the photoelectric conversion efficiency is 19.3%.
[0174] (5) Example 5 Self-assembled monolayer hole transport material SAM B-2
[0175] Test light source: AM SS-X50, data acquisition using Keithley 2400 digital source meter.
[0176] Test results see Fig.14 The open circuit voltage (Voc) of the perovskite solar cell is 1.19 V and the short circuit current density (Jsc) is 23.9 mA cm -2 , the fill factor (FF) is 0.770 and the photoelectric conversion efficiency is 21.8%.
[0177] (6) Example 6 Self-assembled monolayer hole transport material SAM B-3
[0178] Test light source: SS-X50, data acquisition using Keithley 2400 digital source meter.
[0179] Test results see Fig.15 The open circuit voltage (Voc) of the perovskite solar cell is 1.18 V and the short circuit current density (Jsc) is 23.3 mA cm -2 , the fill factor (FF) is 0.681 and the photoelectric conversion efficiency is 18.7%.
[0180] (7) Example 7 Self-assembled monolayer hole transport material SAM C-1
[0181] Test light source: SS-X50, data acquisition using Keithley 2400 digital source meter.
[0182] Test results see Fig.16 The open circuit voltage (Voc) of the perovskite solar cell is 1.18 V and the short circuit current density (Jsc) is 24.1 mA cm -2 , the fill factor (FF) is 0.695 and the photoelectric conversion efficiency is 19.7%.
[0183] (8) Example 8 Self-assembled monolayer hole transport material SAM C-2
[0184] Test light source: AM SS-X50, data acquisition using Keithley 2400 digital source meter.
[0185] Test results see Fig.17 The open circuit voltage (Voc) of the perovskite solar cell is 1.16 V and the short circuit current density (Jsc) is 25.0 mA cm -2 , the fill factor (FF) is 0.806 and the photoelectric conversion efficiency is 23.3%.
[0186] (9) Example 9 Self-assembled monolayer hole transport material SAM C-3
[0187] Test light source: SS-X50, data acquisition using Keithley 2400 digital source meter.
[0188] Test results see Fig.18 The open circuit voltage (Voc) of the perovskite solar cell is 1.16 V and the short circuit current density (Jsc) is 25.6 mA cm -2 , the fill factor (FF) is 0.791 and the photoelectric conversion efficiency is 23.6%.
[0189] The above-mentioned embodiments are only preferred embodiments of the present invention and cannot be used to limit the scope of protection of the present invention. Any non-substantial changes and substitutions made by technicians in this field on the basis of the present invention shall fall within the scope of protection required by the present invention.
Claims
1. A perovskite solar cell with a self-organized monolayer hole transport material, comprising from top to bottom a transparent conductive substrate, an electron transport layer, a perovskite light absorption layer, a hole transport layer and a metal electrode, characterized in that: The hole transport layer is made of a self-organized monolayer hole transport material; the self-organized monolayer hole transport material has the following structural formulas (I), (II), and (III): Wherein, in formula (I), R 11 is carbazole or a carbazole derivative, R 12 -R 13 is hydrogen, R 14 -R 15 is a halogen; In formula (II), R 21 is carbazole or a carbazole derivative, R 22 -R 27 is hydrogen and / or halogen; In formula (III), R 31 is carbazole or a carbazole derivative, R 32 -R 39 is hydrogen and / or halogen.
2. The perovskite solar cell with a self-organized monolayer hole transport material according to claim 1, characterized in that: In formula (I), halogen is one of fluorine, chlorine, bromine and iodine; in formula (II), R 22 -R 27 is hydrogen; in formula (III), R 32 -R 39 For hydrogen.
3. The perovskite solar cell with a self-organized monolayer hole transport material according to claim 1, characterized in that: The structural formula of formula (I) includes any one of the compounds shown in formula (1) to formula (3):
4. The perovskite solar cell with a self-organized monolayer hole transport material according to claim 1, characterized in that: The structural formula of formula (II) includes any one of the compounds shown in formula (4) to formula (6):
5. The perovskite solar cell with a self-organized monolayer hole transport material according to claim 1, characterized in that: The structural formula of formula (III) includes any one of the compounds shown in formula (7) to formula (9):
6. The perovskite solar cell with a self-organized monolayer hole transport material according to claim 1, characterized in that: The preparation steps of the self-organized monolayer hole transport material are as follows: S1: Synthesis of intermediates Under a nitrogen atmosphere, the first compound and the second compound are dissolved in N,N'-dimethylacetamide, followed by adding potassium carbonate and cuprous iodide, reacting at 160°C-200°C for 20h-26h, and cooling to room temperature after the reaction is completed; then, diluting with water, and then extracting with dichloromethane, drying the organic layer with anhydrous magnesium sulfate, filtering and spin-drying, and separating the crude product with silica gel column chromatography to obtain an intermediate; The first compound is carbazole or a carbazole derivative; the second compound is One of them, R 12 -R 13 is hydrogen, R 14 -R 15 is halogen, R 22 -R 27 is hydrogen and / or halogen, R 32 -R 39 is hydrogen and / or halogen; S2: In a dried round-bottom flask, the intermediate is dissolved in dichloromethane. At room temperature, trimethylsilyl bromide is dropped into the well-stirred mixture. After 10 h to 16 h, the mixture is transferred to a round-bottom flask and concentrated under reduced pressure. A magnetic stirring bar and methanol are then added in sequence. The mixture is stirred at room temperature. The mixture is then filtered, rinsed with methanol, and the combined filtrate is concentrated under reduced pressure to obtain the product.
7. The perovskite solar cell with a self-organized monolayer hole transport material according to claim 6, characterized in that: In step S1, the molar ratio of the first compound to the second compound, potassium carbonate and cuprous iodide is 1:(1-1.1):(1.5-2):(1.5-2).
8. The perovskite solar cell with a self-organized monolayer hole transport material according to claim 7, characterized in that: In step S1, the molar ratio of the first compound to the second compound, potassium carbonate and cuprous iodide is 3:3.1:6:
6.
9. The perovskite solar cell with a self-organized monolayer hole transport material according to claim 6, characterized in that: In step S2, the molar ratio of the intermediate to trimethylsilyl bromide is 1:(3-4).
10. The perovskite solar cell with a self-organized monolayer hole transport material according to claim 1, characterized in that: The transparent conductive substrate is fluorine-doped tin oxide or indium-doped tin oxide; the perovskite light absorption layer is made of perovskite material; and the metal electrode is gold or silver.
Citation Information
Cited By
Perovskite solar cell module self-assembled monomolecular hole transport material and preparation method thereof
CN119504856A
Carbazole derivative modified by sulfur-containing functional group as well as preparation method and application of carbazole derivative
CN119823181A
Self-assembled monomolecular layer hole transport material based on polycarbazole derivative and preparation method and application thereof
CN121405741A
A self-assembled monolayer hole transport material based on polycarbazole derivatives, its preparation method and application