Perovskite cell preparation method and perovskite cell

By using perovskite precursor solution and self-assembled single-layer material in perovskite batteries, the perovskite layer with a laminated structure is solved, and the problem of low transmission efficiency in the prior art is achieved, and more efficient charge transport and Battery performance is improved.

CN118922042AActive Publication Date: 2024-11-08JINKO SOLAR CO LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411296537.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-08
Estimated Expiration
2044-09-14

AI Technical Summary

Technical Problem

The current perovskite batteries have poor transmission efficiency, mainly due to the poor coverage, high price and poor stability of hole transport layer materials such as PTAA.

Method used

The perovskite precursor solution, including a material with the molecular formula ABX3 and a self-assembled single-layer material, is coated on the conductive substrate and thermally annealed to form a first transport layer and P-type calcium stacked in sequence along the direction of the conductive substrate. Titanium and N-type perovskite layers use the movement of hydrophilic and hydrophobic groups of self-assembled single-layer materials to form an energy level gradient, enhancing charge transport capabilities and passivating surface and grain boundary defects.

Benefits of technology

It improves the power transmission efficiency of perovskite batteries, enhances the charge transport capacity, inhibits non-radiative recombination, forms a uniform perovskite layer, and improves the overall performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922042A_ABST
    Figure CN118922042A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a perovskite cell. The method comprises the steps that a perovskite precursor solution is prepared, solute of the perovskite precursor solution comprises a material with the molecular formula of ABX3 and a self-assembly monomolecular layer material, A is organic cations, B is metal cations, and X is halogen anions; coating the perovskite precursor solution on a conductive substrate to form a perovskite precursor layer; and performing thermal annealing treatment on the perovskite precursor layer to crystallize the perovskite precursor layer to form a first transmission layer, a P-type perovskite layer and an N-type perovskite layer which are sequentially stacked in the direction away from the conductive substrate. According to the preparation method of the perovskite battery, the power transmission efficiency of the prepared perovskite battery can be effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of new energy conversion and new energy battery components, and in particular to a method for preparing a perovskite battery and a perovskite battery. Background Art

[0002] Metal halide perovskite has become one of the most promising thin-film solar cell materials due to its excellent photoelectric properties such as excellent visible light absorption and long carrier diffusion length. The hole transport layer (HTL) in its structure mainly blocks electrons, enhances hole transport, and prevents quenching caused by direct contact between the perovskite active layer and the electrode.

[0003] However, the materials commonly used for hole transport layers are polymers, such as PTAA, which have disadvantages such as poor coverage, high price, and poor stability, resulting in poor power transmission efficiency of perovskite cells. Summary of the invention

[0004] Based on this, it is necessary to provide a method for preparing a perovskite battery to address the problem of power transmission efficiency of the perovskite battery.

[0005] A method for preparing a perovskite battery, comprising:

[0006] A perovskite precursor solution is prepared, wherein the solute of the perovskite precursor solution includes a material with a molecular formula of ABX3 and a self-assembled monolayer material, wherein A is an organic cation, B is a metal cation, and X is a halogen anion;

[0007] coating the perovskite precursor solution on a conductive substrate to form a perovskite precursor layer;

[0008] The perovskite precursor layer is subjected to thermal annealing to crystallize the perovskite precursor layer, thereby forming a first transmission layer, a P-type perovskite layer, and an N-type perovskite layer which are sequentially stacked in a direction away from the conductive substrate.

[0009] Optionally, the self-assembled monolayer material includes hydrophilic groups. During the thermal annealing treatment of the perovskite precursor layer, the hydrophilic groups move toward the conductive substrate, and part of the self-assembled monolayer material moves to the bottom of the perovskite precursor layer and crystallizes to form the first transport layer in contact with the conductive substrate.

[0010] Optionally, the hydrophilic group includes a phosphate group. During the crystallization of the perovskite material, the phosphate group moves toward the conductive substrate. The content of the phosphate group on the side of the perovskite precursor layer close to the conductive substrate is greater than the content of the phosphate group on the side away from the conductive substrate. The perovskite material crystallizes on the first transport layer to form the stacked P-type perovskite layer and the N-type perovskite layer.

[0011] Optionally, the content of phosphate groups gradually decreases from the top surface of the N-type perovskite layer to the bottom surface of the P-type perovskite layer.

[0012] Optionally, the P-type perovskite layer includes a plurality of sub-P-type layers sequentially formed on the first transmission layer, and the content of holes in the plurality of sub-P-type layers increases layer by layer in a direction away from the conductive substrate;

[0013] The N-type perovskite layer includes a plurality of sub-N-type layers sequentially formed on the P-type perovskite layer, and the electron contents in the plurality of sub-N-type layers increase layer by layer in a direction away from the conductive substrate.

[0014] Optionally, the self-assembled monolayer material also includes a hydrophobic group. During the thermal annealing treatment of the perovskite precursor layer, the hydrophobic group moves away from the conductive substrate, and part of the self-assembled monolayer material moves to the top of the perovskite precursor layer and crystallizes on the top surface of the N-type perovskite layer to form a passivation layer.

[0015] Optionally, the preparation of the perovskite precursor solution comprises:

[0016] Providing iodine halide, inorganic metal halide, organic ammonium salt and the self-assembled monolayer material;

[0017] Dissolving the iodine halide, the inorganic metal halide, the organic ammonium salt and the self-assembled monolayer material in an organic solvent in a predetermined ratio to obtain the perovskite precursor solution;

[0018] Wherein, the self-assembled monolayer material includes one or more of 4PADCB, BCB-C4PA, BCBBr-C4PA, and DMACPA.

[0019] Optionally, the concentration of the self-assembled monolayer material in the perovskite precursor solution is 0.1 mg / mL to 10 mg / mL.

[0020] A perovskite battery, characterized in that it is produced by any one of the preparation methods of a perovskite battery.

[0021] A photovoltaic module, characterized by comprising a perovskite cell manufactured by any one of the methods for preparing a perovskite cell.

[0022] The preparation method of the perovskite battery provided in the above embodiment comprises preparing a perovskite precursor solution, wherein the solute of the perovskite precursor solution comprises a material with a molecular formula of ABX3 and a self-assembled monolayer material, wherein A is an organic cation, B is a metal cation, and X is a halogen anion; coating the perovskite precursor solution on a conductive substrate to form a perovskite precursor layer; thermally annealing the perovskite precursor layer to crystallize the perovskite precursor layer to form a first transport layer, a P-type perovskite layer, and an N-type perovskite layer stacked in sequence in a direction away from the conductive substrate. Since self-assembled monolayers (SAMs) have many advantages such as low material consumption, compatibility with flexible substrates, adjustable band gap, high transmittance and green environmental protection, the perovskite precursor solution obtained by combining the self-assembled monolayer material with the perovskite preparation solution, when preparing the perovskite layer, the SAMs molecules are dispersed from the precursor solution to the grain boundaries and the bottom of the film surface, forming a clear HTL and an energy level gradient. At the same time, a small amount of SAMs diffuses to the top surface of the perovskite film, passivating the defects on the surface and grain boundaries. The nuclear coordination complex between the deprotonated phosphate groups of the SAMs molecules and the polyiodide lead of the perovskite is responsible for both mechanical absorption and electronic charge transfer, resulting in p-type doping of the perovskite film. As a result, the morphology of the prepared perovskite layer is uniform, which not only enhances the charge transport capacity and inhibits non-radiative recombination, but also effectively improves the power transmission efficiency of the perovskite battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 A schematic diagram of a process for preparing a perovskite battery provided in one embodiment of the present application;

[0024] Figure 2 An exemplary diagram of preparing a perovskite layer for a perovskite battery provided in one embodiment of the present application;

[0025] Figure 3 A correlation distribution diagram of radiation wavelength and radiation intensity during current transmission in a perovskite layer after annealing provided in an embodiment of the present application;

[0026] Figure 4 A schematic diagram of the layering of a perovskite layer prepared according to an embodiment of the present application;

[0027] Figure 5 A distribution diagram of the correlation between time and electromagnetic wavelength during the current transmission process of the perovskite layer after annealing provided in one embodiment of the present application;

[0028] Figure 6 This is the structural formula of other materials in the self-assembled monolayer material provided in one embodiment of the present application. DETAILED DESCRIPTION

[0029] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific implementation disclosed below.

[0030] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present application belongs. In the description of the present application, it should be understood that the terms "first" and "second" are used for descriptive purposes only and are not to be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present application, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0031] The terms used herein in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application. It should be understood that when an element is considered to be "connected" to another element, it may be directly connected to the other element or there may be an intermediate element at the same time. On the contrary, when an element is referred to as being "directly" connected to another element, there is no intermediate element.

[0032] See also Figure 1 The present application provides a method for preparing a perovskite battery. The method comprises:

[0033] Step S101, preparing a perovskite precursor solution.

[0034] The solute of the perovskite precursor solution includes a material with a molecular formula of ABX3 and a self-assembled monolayer material, wherein A is an organic cation, B is a metal cation, and X is a halogen anion.

[0035] When preparing a perovskite precursor solution, the solution amount requirement value of the perovskite precursor solution is obtained, and based on the solution amount requirement value, the material configuration amount of the ABX3 material in the perovskite precursor solution corresponding to the solution amount requirement value is calculated through the preparation algorithm of the perovskite precursor solution. Based on the material configuration amount, a perovskite precursor solution of a traditional ABX3 material is prepared. Then, based on the solution capacity of the perovskite precursor solution of the traditional ABX3 material, according to the preset concentration value range of the self-assembled monolayer material in the perovskite precursor solution, the material configuration amount of the self-assembled monolayer material and the solution amount of the self-assembled monolayer material are determined. Based on the material configuration amount and the solution amount of the self-assembled monolayer material, a material solution of the self-assembled monolayer material is configured, and finally, the material solution of the self-assembled monolayer material is added to the perovskite precursor solution of the traditional ABX3 material, and mixed and stirred to complete the preparation process of the perovskite precursor solution. The concentration of the preset self-assembled monolayer material in the perovskite precursor solution may be in the range of 0.01-0.5 mg / ml.

[0036] Then, pour the material solution of the self-assembled monolayer material into the perovskite precursor solution of the traditional ABX3 material, and stir it clockwise at a constant speed for 3-5 minutes to complete the configuration step of the perovskite precursor solution. Among them, the ABX3 material includes one or more of CsI, FAI (CH5IN2), MAI (CH6IN), MABr (CH6BrN), MACl (CH6ClN), PbI2 and PbBr2; wherein the self-assembled monolayer material is used to divide the perovskite layer into sub-perovskite layers corresponding to different energy levels. And the concentration value ranges from 0.1 to 10 mg / mL.

[0037] Step S102 , coating a perovskite precursor solution on a conductive substrate to form a perovskite precursor layer.

[0038] The coating method of the conductive substrate is to coat it on the conductive substrate through a one-step spin coating process. The conductive substrate can be but not limited to a conductive glass ITO (Indium Tin Oxide) substrate or a fluorine-doped tin oxide FTO (Fluorine-doped Tin Oxide) substrate.

[0039] Step S103 , thermally annealing the perovskite precursor layer to crystallize the perovskite precursor layer to form a first transmission layer, a P-type perovskite layer, and an N-type perovskite layer stacked in sequence in a direction away from the conductive substrate.

[0040] The first transport layer is a compact HTL layer formed by depositing a self-assembled monolayer material on the surface of a conductive substrate after annealing. Figure 2, which is an example diagram of preparing a perovskite layer of a perovskite cell, wherein the conductive substrate is an ITO glass substrate.

[0041] In some embodiments, thermal annealing the perovskite precursor layer includes: thermal annealing at a temperature of 80° C. to 150° C. for 1 min to 60 min.

[0042] In some other embodiments, the thermal annealing treatment of the perovskite precursor layer includes: a first thermal annealing treatment at a temperature of 50° C. to 100° C. for 1 min to 60 min; and a second thermal annealing treatment at a temperature of 90° C. to 150° C. for 1 min to 60 min.

[0043] Among them, Figure 3 As shown, the distribution diagrams of the radiation wavelength and radiation intensity of the two perovskite layers measured during the current transmission process of the hole-free (left) perovskite layer doped with 4PADCB and the hole-containing (right) perovskite layer after annealing, among which the PL peak intensity of the hole-free perovskite layer doped with 4PADCB is improved, the non-radiative recombination of the interface is suppressed, and the defects are reduced.

[0044] Based on the above scheme, the self-assembled monolayer material is added to the perovskite precursor layer solution in a certain proportion, and then thermally annealed to prepare the perovskite layer, so that the morphology of the prepared perovskite layer is uniform, which not only enhances the charge transport capacity and inhibits non-radiative recombination, but also effectively improves the power transmission efficiency of the perovskite battery.

[0045] Optionally, the self-assembled monolayer material includes hydrophilic groups. During the thermal annealing process of the perovskite precursor layer, the hydrophilic groups move toward the conductive substrate, and part of the self-assembled monolayer material moves to the bottom of the perovskite precursor layer and crystallizes to form a first transmission layer in contact with the conductive substrate.

[0046] Among them, after the thermal annealing treatment, the N-type sub-perovskite layer is located above the P-type sub-perovskite layer to obtain a carrier concentration range of 10 15 ~10 18 Pieces / cm 3 The carrier concentration range of the material solution in the obtained P-type sub-perovskite layer is 10 10 ~10 8 Pieces / cm 3 .

[0047] Among them, Figure 4As shown, the perovskite layer obtained after preparation, the perovskite layer is, from top to bottom, a top surface passivation layer with a first concentration value, a first N-type sub-perovskite layer with a second concentration value, a second N-type sub-perovskite layer with a third concentration value, a first P-type sub-perovskite layer with a fourth concentration value, a second P-type sub-perovskite layer with a fifth concentration value, and a HTL layer formed by annealing the SAMS material precipitated on a conductive substrate. Among them, the layers of the perovskite layer are not clearly stratified by concentration, but are gradient, fuzzy stratification with gradually decreasing concentrations. Among them, the carrier concentration range corresponding to the first concentration value can be 10 20 Pieces / cm 3 The carrier concentration range corresponding to the second concentration value can be 10 18 Pieces / cm 3 The carrier concentration range corresponding to the third concentration value can be 10 15 Pieces / cm 3 The carrier concentration range corresponding to the fourth concentration value can be 10 10 Pieces / cm 3 , the carrier concentration range corresponding to the fifth concentration value can be 10 8 Pieces / cm 3 When constructing a perovskite cell corresponding to the perovskite layer, a transparent electrode layer and a buffer layer need to be added above the perovskite layer.

[0048] like Figure 5 As shown, the distribution diagram between time and electromagnetic wavelength during the current transmission process of the two perovskite layers measured after annealing, respectively, of the perovskite layer with holes (left) doped with 4PADCB and the perovskite layer without holes (right). Among them, the carrier lifetime of the sample of the perovskite layer without holes doped with 4PADCB decreases more slowly, indicating that the defects are suppressed, while the opposite is true for the sample with holes, indicating that the carrier transport capacity of the perovskite layer without holes doped with 4PADCB is enhanced.

[0049] Based on the above method, it can be ensured that after the thermal annealing treatment, layers with different concentration gradients are formed, and it can be ensured that the prepared P-type perovskite layer and N-type perovskite layer can have a specific concentration gradient. The concentration difference between two adjacent layers can be 10 2 Pieces / cm 3 .

[0050] Optionally, the hydrophilic group includes a phosphate group. During the crystallization of the perovskite material, the phosphate group moves toward the conductive substrate. The content of phosphate groups on the side of the perovskite precursor layer close to the conductive substrate is greater than the content of phosphate groups on the side away from the conductive substrate. The perovskite material crystallizes on the first transport layer to form stacked P-type perovskite layers and N-type perovskite layers.

[0051] Optionally, the content of the phosphate groups gradually decreases from the top surface of the N-type perovskite layer to the bottom surface of the P-type perovskite layer.

[0052] Among them, the content of phosphate groups gradually decreases, so that the P-type perovskite layer can be isolated from the N-type perovskite layer, so as to ensure the constant structural position relationship between the P-type perovskite layer and the N-type perovskite layer, and the material stability in different perovskite layers, so that the energy level gradient difference of the perovskite layer is reduced, thereby being more matched, which can effectively improve the carrier transport capacity and reduce the defect density at the interface and inside the perovskite film, and inhibit the non-radiative recombination of interface carriers.

[0053] Optionally, the P-type perovskite layer includes a plurality of sub-P-type layers sequentially formed on the first transmission layer, and the content of holes in the plurality of sub-P-type layers increases layer by layer in a direction away from the conductive substrate; the N-type perovskite layer includes a plurality of sub-N-type layers sequentially formed on the P-type perovskite layer, and the content of electrons in the plurality of sub-N-type layers increases layer by layer in a direction away from the conductive substrate.

[0054] Specifically, the surface work function of the original perovskite deposited ITO or FTO moves upward, while the surface work function of the perovskite (SAMs) moves downward, and the perovskite (SAMs) energy band shows an upward bend, which allows hole extraction at the interface. Electrons accumulate around hydrogen protons from the doped SAMs, and electrons are transferred from the perovskite to the bottom of the perovskite (the deposited SAMs part), and the electron density (n) decreases. When the temperature remains unchanged, the electron-hole product (np) is a constant, which increases the hole density (p), resulting in the p-type characteristics of the perovskite film doped with SAMs, and the upper electron transport layer is N-type.

[0055] Based on the above scheme, it can be ensured that when annealing is performed to generate the perovskite layer, the structure setting method of first forming the N-type perovskite layer and then the P-type perovskite layer is arranged in order from high to low concentration, thereby improving the stability of the prepared perovskite layer.

[0056] Optionally, the self-assembled monolayer material also includes a hydrophobic group. During the thermal annealing process of the perovskite precursor layer, the hydrophobic group moves away from the conductive substrate, and part of the self-assembled monolayer material moves to the top of the perovskite precursor layer and crystallizes on the top surface of the N-type perovskite layer to form a passivation layer.

[0057] Optionally, preparing a perovskite precursor solution includes: providing iodine halide, inorganic metal halide, organic ammonium salt and self-assembled monolayer material; dissolving the iodine halide, inorganic metal halide, organic ammonium salt and self-assembled monolayer material in an organic solvent according to a predetermined ratio to obtain a perovskite precursor solution; wherein, in the perovskite precursor solution obtained by dissolving the self-assembled monolayer material, the predetermined ratio range of the self-assembled monolayer material is 0.01-0.5 mg / ml, Wherein, the self-assembled monolayer material includes one or more of 4PADCB ([4-(7H-dibenzocarbazole-7-yl)butyl]phosphonic acid), BCB-C4PA ([4-(7H-benzocarbazole-7-yl)butyl]phosphonic acid), BCBBr-C4PA ([4-(10-bromo-7H-benzocarbazole-7-yl)butyl]phosphonic acid), and DMACPA ([2,7-dibromo-9,9-dimethylacridine-10(9H)yl)butyl]phosphonic acid). Figure 6 As shown, it is the structural formula of other materials in the self-assembled monolayer material, wherein R is (C1~C4) alkyl or halogen; L is (C2~C12) alkyl.

[0058] Optionally, the concentration of the self-assembled monolayer material in the perovskite precursor solution is 0.1 mg / mL to 10 mg / mL.

[0059] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0060] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims.

Claims

1. A method for preparing a perovskite battery, It is characterized in that include: Prepare a perovskite precursor solution, wherein the solute of the perovskite precursor solution includes a molecular formula of ABX 3 A material and a self-assembled monolayer material, wherein A is an organic cation, B is a metal cation, and X is a halogen anion; coating the perovskite precursor solution on a conductive substrate to form a perovskite precursor layer; The perovskite precursor layer is subjected to thermal annealing to crystallize the perovskite precursor layer, thereby forming a first transmission layer, a P-type perovskite layer, and an N-type perovskite layer which are sequentially stacked in a direction away from the conductive substrate.

2. The method for preparing a perovskite battery according to claim 1, It is characterized in that The self-assembled monolayer material includes a hydrophilic group. During the thermal annealing treatment of the perovskite precursor layer, the hydrophilic group moves toward the conductive substrate, and part of the self-assembled monolayer material moves to the bottom of the perovskite precursor layer and crystallizes to form the first transport layer in contact with the conductive substrate.

3. The method for preparing a perovskite battery according to claim 2, It is characterized in that The hydrophilic group includes a phosphate group. During the crystallization of the perovskite material, the phosphate group moves toward the conductive substrate. The content of the phosphate group on the side of the perovskite precursor layer close to the conductive substrate is greater than the content of the phosphate group on the side away from the conductive substrate. The perovskite material crystallizes on the first transport layer to form the stacked P-type perovskite layer and the N-type perovskite layer.

4. The method for preparing a perovskite battery according to claim 3, It is characterized in that The content of the phosphate group gradually decreases from the top surface of the N-type perovskite layer to the bottom surface of the P-type perovskite layer.

5. The method for preparing a perovskite battery according to claim 4, It is characterized in that The P-type perovskite layer includes a plurality of sub-P-type layers sequentially formed on the first transmission layer, and the content of holes in the plurality of sub-P-type layers increases layer by layer in a direction away from the conductive substrate; The N-type perovskite layer includes a plurality of sub-N-type layers sequentially formed on the P-type perovskite layer, and the electron contents in the plurality of sub-N-type layers increase layer by layer in a direction away from the conductive substrate.

6. The method for preparing a perovskite battery according to claim 2, It is characterized in that The self-assembled monolayer material also includes a hydrophobic group. During the thermal annealing treatment of the perovskite precursor layer, the hydrophobic group moves away from the conductive substrate, and part of the self-assembled monolayer material moves to the top of the perovskite precursor layer and crystallizes on the top surface of the N-type perovskite layer to form a passivation layer.

7. A method for preparing a perovskite battery according to any one of claims 1 to 6, It is characterized in that The preparation of the perovskite precursor solution comprises: Providing iodine halide, inorganic metal halide, organic ammonium salt and the self-assembled monolayer material; Dissolving the iodine halide, the inorganic metal halide, the organic ammonium salt and the self-assembled monolayer material in an organic solvent in a predetermined ratio to obtain the perovskite precursor solution; Wherein, the self-assembled monolayer material includes one or more of 4PADCB, BCB-C4PA, BCBBr-C4PA, and DMACPA.

8. The method for preparing a perovskite battery according to claim 7, It is characterized in that The concentration of the self-assembled monolayer material in the perovskite precursor solution is 0.1 mg / mL to 10 mg / mL.

9. A perovskite battery, It is characterized in that The perovskite cell is prepared according to the preparation method of any one of claims 1 to 8.

10. A photovoltaic module, It is characterized in that A perovskite battery produced by the method for producing a perovskite battery as described in any one of claims 1 to 8.

Citation Information

Patent Citations

  • P-i-n perovskite battery hole transport layer based on self-assembly engineering

    CN110600612A

  • Perovskite thin film based on phosphate group small molecules, preparation method of perovskite thin film and application of perovskite thin film to photovoltaic cell

    CN116056531A

  • Perovskite cell with modified hole transport layer and preparation method thereof

    CN117979786A

  • Perovskite precursor solution, perovskite thin film preparation method and solar cell

    CN117998953A

  • Perovskite solar cell, preparation method thereof and photovoltaic module

    CN118102736A