Method for producing doped cathode active material

By using heat treatment technology of nickel-manganese granular oxide or hydroxide with uniformly dispersed lithium fluoride source and dopants, the problem of volume change and poor stability of cathode active materials during charging and discharging is solved, and low capacity is achieved Cathode active material with attenuation and high cycle stability.

CN118922383APending Publication Date: 2024-11-08BASF SE
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202380029796.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-25
Filing Date
2023-03-20
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing cathode active materials have large volume changes during charging and discharging, resulting in poor capacity attenuation and cycle stability, and unstable material quality, making it difficult to improve cycle stability under constant mass.

Method used

Using particulate oxides or hydroxides containing nickel and manganese as precursors, combined with a homogeneously dispersed lithium fluoride source and dopant, cathode active material formed by heat treatment is optimized through specific stoichiometric and particle size distribution. , improve the stability and circulation performance of the material.

Benefits of technology

Low capacity attenuation and high cycle stability are achieved, reproducible material performance at constant mass, improving the stability of cathode active material and cell cycle performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005056401170000141
    Figure BDA0005056401170000141
  • Figure BDA0005056401170000142
    Figure BDA0005056401170000142
Patent Text Reader

Abstract

A process for manufacturing a fluoride doped cathode active material wherein the process comprises the steps of: (a) providing a particulate oxide or (oxy) hydroxide or carbonate of TM wherein TM comprises nickel and manganese and wherein at least 50 mol-% of TM is manganese wherein the particulate oxide or (oxy) hydroxide has an average particle size (D50) in the range of 1 to 16 pm, (b) providing a lithium source containing 0.01 to 2.5 up by weight of a fluoride, the fluoride being homogeneously dispersed in the lithium source, (c) mixing the oxide or (oxy) hydroxide or carbonate of TM with the fluoride-containing lithium source, and optionally with an additional lithium source containing less fluoride, and optionally with one or more dopants based on at least one metal other than lithium, (d) heat treating the mixture obtained by step (c).
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a method for producing a fluoride-doped cathode active material, wherein the method comprises the following steps:

[0002] (a) providing a particulate oxide or (oxy)hydroxide of TM, wherein TM is a metal combination comprising nickel and manganese, wherein at least 50 mol-% of TM is manganese and wherein the particulate oxide or (oxy)hydroxide has an average particle size (D50) in the range of 1 to 16 μm,

[0003] (b) providing a lithium source containing 0.01% to 2.5% by weight of fluoride uniformly dispersed in the lithium source,

[0004] (c) mixing the oxide or (oxy)hydroxide of said TM with said fluoride-containing lithium source, and optionally with an additional lithium source containing less fluoride, and optionally with one or more dopants based on at least one metal other than lithium,

[0005] (d) subjecting the mixture obtained in step (c) to heat treatment.

[0006] Lithium-ion secondary batteries are modern devices for storing energy. Many applications have been and are being considered, from small devices such as mobile phones and laptops to automotive batteries and other batteries for electric vehicles. The various components of the battery, such as electrolytes, electrode materials, and separators, play a decisive role in the performance of the battery. Special attention has been paid to cathode materials. Several materials have been proposed, such as lithium iron phosphate, lithium cobalt oxide, and lithium nickel cobalt manganese oxide. Despite extensive research, the solutions found so far still leave room for improvement.

[0007] The cathode active material is usually manufactured by using a two-stage process. In the first stage, the compound is prepared by precipitating a sparingly soluble compound of one or more transition metals from a solution (e.g., a carbonate or hydroxide). The sparingly soluble salt is also referred to as a precursor in many cases. In the second stage, the precursor is mixed with a lithium compound (e.g., Li2CO3, LiOH, or Li2O) and calcined at high temperatures, e.g., at 600°C to 1100°C. In special formulations, dopants such as aluminum oxide, titanium oxide, zirconium oxide, or oxides or (oxy) hydrides of transition metals (e.g., Nb, Ta, W, Mo, etc.) may be added.

[0008] At present, a certain interest can be observed in so-called nickel-rich electrode active materials, for example electrode active materials containing at least 50 mol-% or even 75 mol-% or more Ni relative to the total metal content (metal means metal other than lithium). Some technical problems remain to be solved. Volumetric energy density, capacity decay, cycle stability are still areas of research and development. Some of these problems are attributed to the volume change of the cathode active material during charging and discharging. It has been suggested to reduce the volume change by incorporating fluorides, see for example US 5,773,168. The method disclosed is to mix a small amount of lithium fluoride with another lithium source (such as lithium carbonate) and then calcine it. However, the quality of such materials is often very uneven. In US2015 / 0064563, it has been suggested to incorporate fluorides by heat treating the cathode active material with a fluorinated polymer (such as polyvinylidene fluoride).

[0009] In US2013 / 0209840, a fluoride coating method is disclosed. The fluoride coating only affects the outer surface of the corresponding cathode active material. In N. Zhang et al., J. Electrochem. Soc. [Journal of the Electrochemical Society] 2020, 167, 080815, the authors reported experiments on fluoride doping by mixing the precursor with LiOH·H2O and LiF, followed by a two-step calcination.

[0010] However, it has been found that the above materials vary greatly between different samples.

[0011] Therefore, the object of the present invention is to provide a cathode active material having improved stability such as lower capacity fade and improved cycle stability at constant quality. Another object is to provide a method for making a cathode active material having improved stability such as lower capacity fade and improved cycle stability at constant and reproducible quality.

[0012] Accordingly, the method defined at the outset has been found, hereinafter also referred to as "the method of the invention" or as "the method according to the (present) invention". The method of the invention comprises a series of steps as defined at the outset, hereinafter also referred to as step (a), step (b), step (c), etc. The method of the invention will be described in more detail below.

[0013] Step (a) comprises providing a particulate oxide or (oxy)hydroxide or carbonate of TM, TM being a metal combination, wherein TM comprises nickel and manganese, wherein at least 50 mol-% of TM is manganese and wherein said particulate oxide or (oxy)hydroxide has an average particle size (D50) in the range of 1 to 16 μm, preferably 5 to 12 μm. Said particulate oxide or (oxy)hydroxide or carbonate of TM is also referred to as "precursor". Preferably, at least 95 mol-% of TM is selected from transition metals, such as nickel or manganese. At most 5 mol-%, preferably at most 1 mol-% of TM may be Mg or Al. Although strictly speaking the D50 value is a median value, it is often also referred to as the average particle size (D50).

[0014] In one embodiment of the present invention, the precursor comprises at least one of Mg, Al and Y, or at least one transition metal selected from Ti, Zr, Nb, Ta, Fe, Mo and W. In other embodiments, the precursor does not contain any metal other than nickel, cobalt and manganese, or even does not contain any metal other than nickel and manganese.

[0015] In one embodiment of the present invention, TM corresponds to the general formula (I)

[0016] (Ni a Co b Mn c ) 1-d M d (I)

[0017] in

[0018] a is in the range of 0.2 to 0.5, preferably 0.3 to 0.4,

[0019] b is 0 or in the range of 0.01 to 0.1, preferably 0.05 to 0.1, and more preferably 0, c is in the range of 0.5 to 0.8, preferably 0.6 to 0.7, and

[0020] d is in the range of 0 to 0.1, preferably 0.01 to 0.05.

[0021] M is at least one of Al, Mg, Ti, Mo, Nb, Ta, W and Zr, and

[0022] a+b+c=1.

[0023] The precursor is preferably obtained by coprecipitating nickel, cobalt and manganese in the form of hydroxides or carbonates from an aqueous solution containing nitrates, acetates or preferably sulfates of nickel and cobalt and / or manganese (the stoichiometric ratio of which corresponds to TM). The coprecipitation can be accomplished by adding alkali metal hydroxides or alkali metal carbonates (e.g. potassium hydroxide or sodium hydroxide, or potassium carbonate or sodium carbonate, respectively) in a continuous, semi-continuous or batch process. After the coprecipitation, the mother liquor is then removed (e.g. by filtration) and the water is then removed.

[0024] The precursor is in granular form. In one embodiment of the present invention, the average particle size (D50) of the precursor is in the range of 1 to 16 μm, preferably 5 to 12 μm, and more preferably 7 to 10 μm. The average particle size (D50) in the context of the present invention refers to the median of the volume-based particle size as can be determined, for example, by light scattering. In one embodiment, the precursor has a unimodal particle size distribution. In other embodiments, the particle distribution of the precursor can be bimodal, for example, having a maximum value in the range of 1 to 5 μm, and having another maximum value in the range of 7 to 16 μm.

[0025] The particle shape of the secondary particles of the precursor is preferably spherical, which are particles having a spherical shape. Spherical spheres should include not only those particles that are completely spherical, but also those particles in which at least 90% (number average) of representative samples have a maximum and minimum diameter that differ by no more than 10%.

[0026] In one embodiment of the present invention, the precursor comprises secondary particles, which are agglomerates of primary particles. Preferably, the precursor consists of spherical secondary particles, which are agglomerates of primary particles. Even more preferably, the precursor consists of spherical secondary particles, which are agglomerates of spherical primary particles or flakes.

[0027] In one embodiment of the present invention, the precursor may have a particle size distribution span in the range of 0.5 to 0.9, the span being defined as [(D90)-(D10)] divided by (D50), all of which are determined by laser analysis. In another embodiment of the present invention, the precursor may have a particle size distribution span in the range of 1.1 to 1.8.

[0028] In one embodiment of the present invention, the specific surface area (BET) of the precursor is determined by nitrogen adsorption method, for example according to DIN-ISO 9277:2003-05, at 2 to 10 m 2 / g, or even greater than 10 to 100 m 2 / g range.

[0029] Some metals are ubiquitous, such as sodium, calcium or zinc, and trace amounts of these metals are almost ubiquitous, but these trace amounts will not be considered in the description of the present invention. Trace amounts of metals in this context will mean an amount of 0.05 mol-% or less relative to the total metal content of the TM.

[0030] The precursor may contain sulfate, for example 0.1% to 0.5% sulfate by weight, as determined by ion chromatography. The precursor may contain carbonate, for example 0.1% to 2% carbonate by weight, each percentage being relative to the total weight of the precursor.

[0031] In step (b) a lithium source is provided, wherein the source contains 0.01% to 2.5% by weight of fluoride, uniformly dispersed in the lithium source. Preferably 0.05% to 0.5% by weight. The percentages are relative to the corresponding lithium source. The fluoride is preferably lithium fluoride, but may have counterions other than lithium and derived from impurities. Preferably, the majority of the fluoride is lithium fluoride. Even more preferably, the fluoride is lithium fluoride.

[0032] The lithium source is selected from lithium carbonate, lithium oxide (Li2O) and lithium hydroxide (LiOH), and includes lithium hydroxide hydrates such as but not limited to LiOH.H2O. Lithium oxide (Li2O) and lithium hydroxide (LiOH) are preferred.

[0033] In the lithium source, the fluoride is uniformly dispersed, preferably lithium fluoride. The term "uniformly dispersed" means that, for example, by X-ray diffraction, particle size distribution, optical microscopy and SEM / EDX (scanning electron microscopy / energy dispersive X-ray spectroscopy), no individual crystals or agglomerates of fluoride or even LiF may be detected. Particle size distribution and X-ray diffraction and SEM / EDX are preferred.

[0034] Preferably, the fluoride-containing lithium source is produced by recycling spent batteries, for example by a recovery process of lithium carbonate or lithium hydroxide from a lithium salt solution containing fluoride (e.g. derived from an electrolyte such as LiPF6 or from a decomposed fluoropolymer binder).

[0035] In one embodiment of the present invention, the recovery method comprises the following steps:

[0036] (i) producing black powder, sometimes referred to as black matter or active matter, from spent lithium-ion batteries by mechanical destruction of the batteries followed by thermal treatment,

[0037] (ii) treating the black powder with at least one of Ca(OH)2 or Mg(OH)2 in the presence of water or a polar solvent other than water at a temperature of at least 70°C, preferably 70°C to 120°C,

[0038] (iii) separating the solid from the liquid, preferably by filtration, optionally followed by washing the solid residue with a polar solvent such as water, thereby obtaining a solution of lithium hydroxide containing fluoride, and

[0039] (iv) optionally after purification of the solution, removing water from the solution of lithium hydroxide by one or more steps, for example by evaporation, to produce solid LiOH.

[0040] In another embodiment, steps (i) to (iii) are performed after step (v),

[0041] (v) adding CO2 or any water-soluble carbonate, such as Na2CO3, to precipitate Li2CO3,

[0042] (vi) separating the solid from the liquid by a solid-liquid separation method, such as filtration, optionally followed by washing the solid residue with a polar solvent such as water, thereby obtaining solid lithium carbonate containing fluoride.

[0043] The lithium hydroxide produced according to the above recovery method generally contains 0.01% to 1.3% by weight of fluoride relative to the monohydrate of LiOH, preferably 0.05% to 0.5% by weight. Depending on the drying conditions, anhydrous LiOH is obtained instead of the monohydrate. In this case, the characteristic amounts of the above-mentioned impurities related to the monohydrate are respectively higher in concentration, about 1.75 times higher for 100% anhydrous LiOH (corresponding to the molar amount of the monohydrate divided by the molar amount of the anhydrate).

[0044] The lithium carbonate produced according to the above recovery method generally contains 0.01 to 1.5% by weight of fluoride, preferably 0.05 to 0.5% by weight.

[0045] Step (c) comprises mixing the oxide or (oxy)hydroxide of TM with the fluoride-containing lithium source, and optionally with an additional lithium source containing less fluoride, and optionally with one or more dopants based on at least one metal other than lithium. By carrying out step (c), a mixture is obtained. The expression "the fluoride-containing lithium source" is the lithium source provided in step (b). The expression "containing less fluoride" refers to a lithium source compared to the lithium source provided in step (b).

[0046] The combined amounts of precursors and total lithium source will correspond to the desired stoichiometry of the target cathode active material. Typically a stoichiometric amount or even a slight excess of lithium relative to the metal other than lithium is selected.

[0047] Step (c) may comprise mixing with an additional lithium source which contains less fluoride than the lithium source provided in step (b), for example 1 to 150 ppm, or even below detection levels.

[0048] The dopant is selected from oxides, hydroxides and oxyhydroxides of Mg, Ti, Zr, W, Nb, Ta and especially Al. Lithium titanate is a possible titanium source. Examples of dopants are MgO, Mg(OH)2, TiO2 (selected from rutile and anatase, preferably anatase), and basic titanium oxides such as TiO(OH)2, and Li4Ti5O 12 , ZrO2, Zr(OH)4, Li2ZrO3, Nb2O3, Ta2O5, Li2WO4, WO3, MoO3, Li2MoO4, Al(OH)3, Al2O3, Al2O3 hydrate and AlOOH. Preferred Al compounds are Al(OH)3, α-Al2O3, γ-Al2O3, Al2O3 hydrate and AlOOH, as well as TiO2 and Zr(OH)4. Even more preferred dopants are Al2O3 selected from α-Al2O3, γ-Al2O3, and most preferably γ-Al2O3.

[0049] In a preferred embodiment, one or more dopants are applied in an amount up to 2.5 mol %, preferably 0.1 to 1.5 mol %, relative to TM.

[0050] Examples of suitable equipment for carrying out step (c) are high shear mixers, drum mixers, ploughshare mixers and free fall mixers.

[0051] In one embodiment of the present invention, step (c) is carried out at a temperature ranging from ambient temperature to 200°C, preferably from 20°C to 50°C.

[0052] In one embodiment of the present invention, the duration of step (c) is 10 minutes to 2 hours. Depending on whether additional mixing is performed in step (d), sufficient mixing must be completed in step (c).

[0053] The mixing of the precursor, the lithium source from step (b) and - optionally - the further lithium source and / or one or more dopants can be carried out all in one step or in sub-steps, for example by first mixing the lithium source containing fluoride with the one or more dopants and adding this mixture to the precursor, or by first mixing the precursor with the lithium source containing fluoride and then adding the dopant and further lithium source, or by first mixing the dopant with the precursor and then adding the lithium source containing lithium fluoride and further lithium source. It is preferred to first mix the precursor with the two lithium sources and then add the dopant.

[0054] In one embodiment of the present invention, step (c) comprises two sub-steps:

[0055] (c1) mixing a fluoride-containing lithium source with a fluoride-free lithium source, and

[0056] (c2) mixing the mixture obtained from step (c1) with the oxide or (oxy)hydroxide or carbonate of said TM and - if applicable - with said one or more dopants.

[0057] In one embodiment of the present invention, the weight ratio of the fluoride-containing lithium source to the fluoride-free lithium source as provided in step (b) is in the range of 20:1 to 1:0, preferably 1:1 to 1:20.

[0058] Although an organic solvent, such as glycerol or ethylene glycol, or water may be added in step (c), it is preferred to carry out step (c) in a dry state without adding water or an organic solvent.

[0059] A mixture was obtained.

[0060] Step (d) comprises heat treating the mixture, for example at a temperature in the range of 850° C. to 1150° C., preferably 850° C. to 1000° C., more preferably 900° C. to 975° C. Heating from 1000° C. to 1150° C. is possible, and in such embodiments monolithic particles will be obtained.

[0061] In one embodiment of the present invention, the mixture from step (c) is heated to 850°C to 1000°C at a heating rate of 0.1 to 10°C / min.

[0062] In one embodiment of the invention, the temperature is ramped up before reaching the desired temperature of 850 to 1150° C., preferably 900 to 975° C. or 1000 to 1150° C. For example, the mixture from step (c) is first heated to a temperature of 350 to 550° C. and then kept constant for a period of 10 minutes to 4 hours, and then it is increased to 850 to 1000° C. or even 1150° C.

[0063] In embodiments where at least one solvent is used in step (c), the one or more solvents are removed in a portion of step (d), or separately and before starting step (d), for example by filtering, evaporating or distilling the one or more solvents. Evaporation and distillation are preferred.

[0064] In one embodiment of the invention, step (d) is carried out in a roller hearth kiln, a pusher kiln or a rotary kiln or a combination of at least two of the foregoing. The advantage of a rotary kiln is that the homogeneity of the material produced therein is very good. In roller hearth kilns and pusher kilns, different reaction conditions for the different steps can be easily set. In laboratory scale tests, box furnaces and tube furnaces as well as split tube furnaces are also feasible.

[0065] In one embodiment of the invention, step (d) is carried out in an oxygen-containing atmosphere, for example, in a nitrogen-air mixture, a noble gas-oxygen mixture, air, oxygen or oxygen-enriched air. In a preferred embodiment, the atmosphere in step (d) is selected from air, oxygen and oxygen-enriched air. Oxygen-enriched air can be, for example, a 50:50 mixture of air and oxygen by volume. Other options are a 1:2 mixture of air and oxygen by volume, a 1:3 mixture of air and oxygen by volume, a 2:1 mixture of air and oxygen by volume, and a 3:1 mixture of air and oxygen by volume.

[0066] In one embodiment of the invention, the stoichiometry of lithium in step (c) is in the range of 90 to 95 mol-% relative to the sum of TM and - if applicable - metal other than lithium from one or more dopants, and step (d) is followed by a further mixing step with a lithium source and a further heat treatment step.

[0067] By implementing the method of the present invention, a cathode active material showing excellent stability, such as low capacity fade and high cycle stability, is produced.

[0068] Another aspect of the present invention is a cathode active material, also referred to hereinafter as the cathode active material of the present invention. The cathode active material of the present invention can be represented by the general formula Li 1+x TM 1-x O 2-y F y The cathode active material of the present invention is described as follows, and its average particle size (D50) is in the range of 1 to 16 μm, preferably 1 to 3 μm or 5 to 12 μm, and more preferably 7 to 10 μm. The TM in the cathode active material of the present invention comprises Ni and Mn, wherein at least 50 mol% of the TM is manganese, and wherein x is in the range of 0.05 to 0.4, preferably 0.2 to 0.35, and y is in the range of 0.0002 to 0.03, and F is uniformly distributed in this cathode active material. The embodiment in which the average diameter is 1 to 3 μm is preferably a so-called monolithic or single crystal particle.

[0069] F is uniformly distributed in the cathode active material of the present invention in the form of fluoride. This means that F is not accumulated on the outer surface of the secondary particles, but inside the secondary particles. Some fluoride may accumulate at the grain boundaries of the primary particles, but preferably there is no accumulation. In addition, there are few or even no secondary particles that do not contain fluoride.

[0070] The cathode active material of the present invention is in granular form. In one embodiment of the present invention, the average particle size (D50) of the cathode active material of the present invention is in the range of 1 to 16 μm, preferably 1 to 3 μm or 5 to 12 μm, and more preferably 7 to 10 μm. The average particle size (D50) in the context of the present invention refers to the median of the volume-based particle size as can be determined, for example, by light scattering. In one embodiment, the precursor has a unimodal particle size distribution. In other embodiments, the particle distribution of the precursor can be bimodal, for example, having a maximum value in the range of 1 to 5 μm, and having another maximum value in the range of 7 to 16 μm.

[0071] The particle shape of the secondary particles of the cathode active material of the present invention is preferably spherical, which are particles with a spherical shape. Spherical spheres should include not only those particles that are completely spherical, but also those particles in which at least 90% (number average) of the representative samples have a maximum and minimum diameter that differ by no more than 10%.

[0072] In one embodiment of the present invention, the cathode active material of the present invention is composed of secondary particles, which are agglomerates of primary particles. Preferably, the precursor is composed of spherical secondary particles, which are agglomerates of primary particles. Even more preferably, the precursor is composed of spherical secondary particles, which are agglomerates of spherical primary particles or flakes.

[0073] In one embodiment of the present invention, the cathode active material of the present invention has a particle size distribution span in the range of 0.5 to 0.9, which is defined as [(D90)-(D10)] divided by (D50), all of which are determined by laser analysis. In another embodiment of the present invention, the precursor may have a particle size distribution span in the range of 1.1 to 1.8.

[0074] In one embodiment of the present invention, the specific surface area (BET) of the cathode active material of the present invention is determined by nitrogen adsorption method, for example according to DIN-ISO 9277:2003-05, in the range of 0.1 to 1.5 m 2 / g, and preferably 0.2 to 1.0 m 2 / g range.

[0075] In one embodiment of the present invention, the TM in the cathode active material of the present invention is a metal combination according to the general formula (I):

[0076] (Ni a Co b Mn c ) 1-d M d (I)

[0077] in

[0078] a is in the range of 0.2 to 0.5, preferably 0.3 to 0.4,

[0079] b is 0 or in the range of 0.01 to 0.1, preferably 0.05 to 0.1, and more preferably 0, c is in the range of 0.5 to 0.8, preferably 0.6 to 0.7, and

[0080] d is in the range of 0 to 0.1, preferably 0.01 to 0.05.

[0082] M is at least one of Al, Mg, Ti, Mo, Nb, Ta, W and Zr, and

[0083] a+b+c=1.

[0084] A further aspect of the invention relates to an electrode comprising at least one particulate cathode active material according to the invention. They are particularly useful for lithium ion batteries. A lithium ion battery comprising at least one electrode according to the invention exhibits good cycling behavior / stability. An electrode comprising at least one particulate cathode active material according to the invention is also referred to hereinafter as a cathode according to the invention or a cathode according to the invention.

[0085] Specifically, the cathode of the present invention contains

[0086] (A) at least one particulate cathode active material of the present invention,

[0087] (B) carbon in an electrically conductive form,

[0088] (C) an adhesive material, also referred to as an adhesive or adhesive (C), and preferably,

[0089] (D) Current collector.

[0090] In a preferred embodiment, the cathode of the present invention comprises

[0091] (A) 80 to 98% by weight of the particulate cathode active material of the present invention,

[0092] (B) 1 to 17% by weight of carbon,

[0093] (C) 1 to 15% by weight of a binder,

[0094] Percentages are relative to the sum of (A), (B), and (C).

[0095] The cathodes according to the present invention may comprise additional components. They may include a current collector such as, but not limited to, aluminum foil. They may further comprise conductive carbon and a binder.

[0096] The cathode according to the present invention contains conductive modified carbon, also referred to as carbon (B) for short. Carbon (B) may be selected from soot, activated carbon, carbon nanotubes, graphene and graphite, and a combination of at least two of the foregoing.

[0097] Suitable binders (C) are preferably selected from organic (co)polymers. Suitable (co)polymers, i.e. homopolymers or copolymers, can be selected from (co)polymers obtainable, for example, by anionic, catalytic or free radical (co)polymerization, in particular from polyethylene, polyacrylonitrile, polybutadiene, polystyrene, and copolymers of at least two comonomers selected from ethylene, propylene, styrene, (meth)acrylonitrile and 1,3-butadiene. Polypropylene is also suitable. In addition, polyisoprene and polyacrylates are also suitable. Polyacrylonitrile is particularly preferred.

[0098] In the context of the present invention, polyacrylonitrile is understood to mean not only polyacrylonitrile homopolymers but also copolymers of acrylonitrile with 1,3-butadiene or styrene. Polyacrylonitrile homopolymers are preferred.

[0099] In the context of the present invention, polyethylene is understood to mean not only homopolyethylene but also copolymers of ethylene which comprise at least 50 mol % of copolymerized ethylene and up to 50 mol % of at least one further comonomer, for example α-olefins such as propylene, butene (1-butene), 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-pentene and also isobutene, vinylaromatic compounds such as styrene and also (meth)acrylic acid, vinyl acetate, vinyl propionate, C1-C12-hydroxyethyl esters of (meth)acrylic acid. 10 - Alkyl esters, especially methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, n-butyl acrylate, 2-ethylhexyl acrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, and also maleic acid, maleic anhydride and itaconic anhydride. The polyethylene may be HDPE or LDPE.

[0100] In the context of the present invention, polypropylene is understood to mean not only homopolypropylene, but also copolymers of propylene, which contain at least 50 mol-% copolymerized polypropylene and up to 50 mol-% of at least one further comonomer, for example ethylene and α-olefins such as butene, 1-hexene, 1-octene, 1-decene, 1-dodecene and 1-pentene. The polypropylene is preferably isotactic or substantially isotactic.

[0101] In the context of the present invention, polystyrene is understood to mean not only homopolymers of styrene but also C1-C12 copolymers with acrylonitrile, 1,3-butadiene, (meth)acrylic acid, (meth)acrylic acid, and the like. 10- copolymers of alkyl esters, divinylbenzene, especially 1,3-divinylbenzene, 1,2-diphenylethylene and α-methylstyrene.

[0102] Another preferred binder (C) is polybutadiene.

[0103] Other suitable binders (C) are selected from polyethylene oxide (PEO), cellulose, carboxymethylcellulose, polyimide and polyvinyl alcohol.

[0104] In one embodiment of the present invention, the binder (C) is selected from a group consisting of binders having an average molecular weight M in the range of 50,000 to 1,000,000 g / mol, preferably to 500,000 g / mol. w Those (co)polymers.

[0105] The binder (C) may be a cross-linked or non-cross-linked (co)polymer.

[0106] In a particularly preferred embodiment of the present invention, binder (C) is selected from halogenated (co) polymers, especially fluorinated (co) polymers. Halogenated or fluorinated (co) polymers are understood to mean those (co) polymers comprising at least one (co) polymerized (co) monomer having at least one halogen atom or at least one fluorine atom per molecule, more preferably at least two halogen atoms or at least two fluorine atoms per molecule. Examples are polyvinyl chloride, polyvinylidene chloride, polytetrafluoroethylene, polyvinylidene fluoride (PVdF), tetrafluoroethylene-hexafluoropropylene copolymer, vinylidene fluoride-hexafluoropropylene copolymer (PVdF-HFP), vinylidene fluoride-tetrafluoroethylene copolymer, perfluoroalkyl vinyl ether copolymer, ethylene-tetrafluoroethylene copolymer, vinylidene fluoride-chlorotrifluoroethylene copolymer and ethylene-chlorofluoroethylene copolymer.

[0107] Suitable binders (C) are, in particular, polyvinyl alcohols and halogenated (co)polymers, for example polyvinyl chloride or polyvinylidene chloride, and in particular fluorinated (co)polymers, such as polyvinyl fluoride and in particular polyvinylidene fluoride and polytetrafluoroethylene.

[0108] The cathode of the present invention may contain 1% to 15% by weight of one or more binders relative to the cathode active material of the present invention. In other embodiments, the cathode of the present invention may contain 0.1% to less than 1% by weight of one or more binders.

[0109] Another aspect of the invention is a battery comprising at least one cathode comprising the cathode active material of the invention, carbon, and a binder, at least one anode, and at least one electrolyte.

[0110] The embodiments of the cathode of the present invention have been described above in detail.

[0111] The anode may contain at least one anode active material, such as carbon (graphite), TiO2, lithium titanium oxide, silicon or tin. The anode may additionally contain a current collector, such as a metal foil such as copper foil.

[0112] The electrolyte may include at least one non-aqueous solvent, at least one electrolyte salt, and optionally additives.

[0113] The nonaqueous solvent of the electrolyte may be liquid or solid at room temperature and is preferably selected from polymers, cyclic or acyclic ethers, cyclic or acyclic acetals, and cyclic or acyclic organic carbonates.

[0114] Examples of suitable polymers are in particular polyalkylene glycols, preferably poly-C1-C4-alkylene glycols, and in particular polyethylene glycol. Polyethylene glycol may account for up to 20 mol% of one or more C1-C4-alkylene glycols. Polyalkylene glycols are preferably polyalkylene glycols with two methyl or ethyl end caps.

[0115] The molecular weight M of suitable polyalkylene glycols and in particular suitable polyethylene glycols is w It may be at least 400 g / mol.

[0116] The molecular weight M of suitable polyalkylene glycols and in particular suitable polyethylene glycols is w It may be up to 5,000,000 g / mol, preferably up to 2,000,000 g / mol.

[0117] Examples of suitable acyclic ethers are, for example, diisopropyl ether, di-n-butyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, of which 1,2-dimethoxyethane is preferred.

[0118] Examples of suitable cyclic ethers are tetrahydrofuran and 1,4-dioxane.

[0119] Examples of suitable acyclic acetals are, for example, dimethoxymethane, diethoxymethane, 1,1-dimethoxyethane and 1,1-diethoxyethane.

[0120] Examples of suitable cyclic acetals are 1,3-dioxane and in particular 1,3-dioxolane.

[0121] Examples of suitable acyclic organic carbonates are dimethyl carbonate, ethyl methyl carbonate and diethyl carbonate.

[0122] Examples of suitable cyclic organic carbonates are compounds according to the general formula (II) and (III)

[0123]

[0124] Where R1 , R 2 and R 3 may be identical or different and are selected from hydrogen and C1-C4-alkyl, for example methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl and tert-butyl, wherein R 2 and R 3 Preferably not all are tert-butyl.

[0125] In a particularly preferred embodiment, R 1 is methyl and R 2 and R 3 Each is hydrogen, or R 1 , R 2 and R 3 Each is hydrogen.

[0126] Another preferred cyclic organic carbonate is vinylene carbonate, formula (IV).

[0127]

[0128] The solvent or solvents are preferably used in anhydrous state, ie with a water content in the range from 1 ppm to 0.1% by weight, which can be determined, for example, by Karl-Fischer titration.

[0129] The electrolyte (C) further comprises at least one electrolyte salt. Suitable electrolyte salts are in particular lithium salts. Examples of suitable lithium salts are LiPF6, LiBF4, LiClO4, LiAsF6, LiCF3SO3, LiC(C n F 2n+1 SO2)3, lithium imide such as LiN(C n F 2n+1 SO2)2, wherein n is an integer in the range of 1 to 20, LiN(SO2F)2, Li2SiF6, LiSbF6, LiAlCl4 and compounds having the general formula (C n F 2n+1 SO2) t Salts of YLi, wherein m is defined as follows:

[0130] When Y is selected from oxygen and sulfur, t=1,

[0131] When Y is selected from nitrogen and phosphorus, t=2, and

[0132] When Y is selected from carbon and silicon, t=3.

[0133] Preferred electrolyte salts are selected from LiC(CF3SO2)3, LiN(CF3SO2)2, LiPF6, LiBF4, LiClO4, among which LiPF6 and LiN(CF3SO2)2 are particularly preferred.

[0134] In an embodiment of the invention, the battery according to the invention comprises one or more separators, by means of which the electrodes are mechanically separated. Suitable separators are polymer films, in particular porous polymer films, which are non-reactive to metallic lithium. Particularly suitable materials for separators are polyolefins, in particular film-forming porous polyethylene and film-forming porous polypropylene.

[0135] The membrane composed of polyolefin, in particular polyethylene or polypropylene, can have a porosity in the range of 35% to 45%. Suitable pore diameters are, for example, in the range of 30 to 500 nm.

[0136] In another embodiment of the present invention, the separator can be selected from a PET nonwoven material filled with inorganic particles. Such a separator can have a porosity in the range of 40% to 55%. Suitable pore sizes are, for example, in the range of 80 to 750 nm.

[0137] The battery according to the invention further comprises a housing, which may have any shape, for example a cubic or cylindrical disc or cylindrical can shape. In a variant, a metal foil configured as a pouch is used as housing.

[0138] The battery according to the present invention shows good cycling stability and low capacity fade.

[0139] The battery according to the invention may comprise two or more electrochemical cells combined with one another, which may be connected in series or in parallel, for example. Preferably they are connected in series. In the battery according to the invention, at least one of the electrochemical cells comprises at least one cathode according to the invention. Preferably, in the electrochemical cells according to the invention, the majority of the electrochemical cells comprise a cathode according to the invention. Even more preferably, in the battery according to the invention, all electrochemical cells comprise a cathode according to the invention.

[0140] The invention further provides for the use of a battery according to the invention in an apparatus, in particular in a mobile device. Examples of mobile devices are vehicles, such as cars, bicycles, aircraft or water vehicles (such as ships or vessels). Other examples of mobile devices are those that are moved manually, such as computers, in particular laptops, telephones or electric hand tools, such as in the construction industry, in particular drills, battery-powered screwdrivers or battery-powered staplers.

[0141] The present invention is further illustrated by the following working examples.

[0142] Description of the method

[0143] Li in aqueous solution was determined by optical emission spectroscopy using inductively coupled plasma (ICP-OES). Instrument: ICP-OES Agilent 5100SVDV; Wavelength: Li 670.783 nm; Internal standard: Sc 361.383 nm; Dilution factor: Li; Calibration: external.

[0144] Elemental analysis of fluorine and fluoride was performed according to the standardized methods: DIN EN 14582:2016-12 on sample preparation for determination of bulk fluorine content (waste sample); detection method is ion-selective electrode measurement. DIN 38405-D4-2:1985-07 (water samples; digestion of inorganic solids, followed by acid-loaded distillation and fluoride determination using an ion-selective electrode).

[0145] Starting Materials:

[0146] "Battery grade" LiOH.H2O, hereinafter also referred to as "LiOH bg", is commercially available from Livent and has a fluoride content of less than 5 ppm

[0147] LiF was commercially available from Sigma Aldrich.

[0148] I. Providing starting materials for calcination

[0149] I.1 Synthesis of precursors, step (a.1)

[0150] The stirred tank reactor was filled with deionized water and the temperature was adjusted to 45° C. Then, the pH value was adjusted to 11.3 by adding an aqueous sodium hydroxide solution.

[0151] The coprecipitation reaction was started by simultaneously feeding an aqueous solution of transition metal sulfate and an aqueous solution of sodium hydroxide at a flow rate ratio of 1.9, and the total flow rate resulted in an average residence time of 12 hours. The transition metal solution contained Ni and Mn in a molar ratio of 1:2, and the total concentration of transition metals was 1.65 mol / kg. The aqueous solution of sodium hydroxide was a 50 wt.% sodium hydroxide solution. The pH value was maintained at 11.3 by feeding an aqueous solution of sodium hydroxide alone. From the start of all feeds, the mother liquor was continuously removed. All feed streams were stopped after 29 hours. A mixed transition metal (TM) oxyhydroxide precursor was obtained by filtering the resulting suspension, washing with distilled water, drying in air at 120°C and sieving. The precursor TM-OH.1 was obtained, and the average particle size (D50) was 6 μm.

[0152] I.2 Synthesis of LiOH containing LiF, step (b.1)

[0153] According to the method described in Jia Li et al., Journal of Hazardous Materials 2016, 302, 97-104, about 1 t of mechanically treated battery waste is treated to obtain reduced material, the battery waste containing spent cathode active material (containing nickel, cobalt and manganese), organic carbon in the form of graphite and soot, and residual electrolyte, and other impurities (including fluorine compounds, phosphorus and calcium in particular). The atmosphere in the roasting system is air, the oxygen in which reacts with the carbon in the battery waste to form carbon monoxide, and the treatment temperature is 800°C.

[0154] After reaction and cooling to ambient temperature, the heat treated material was recovered from the furnace, mechanically treated to obtain granular material and analyzed by X-ray powder diffraction, elemental analysis and particle size distribution.

[0155] The Li content was 3.6 wt.-%, providing a reference for the following leaching procedure (see below). Fluorine (2.6 wt.-%) was mainly present as inorganic fluorides (2.3 wt.-%). The particle size was well below 1 mm; D50 was determined to be 17.36 μm.

[0156] The obtained XRD pattern was compared with the calculated reference pattern of Ni (which is the same as the pattern of one of the following: Co x Ni 1-x , x = 0 to 0.6, Co, Li2CO3 and LiAlO2), the following conclusions can be drawn: Ni is completely present in the form of a metallic phase, pure Ni or an alloy combined with Co. When in contact with permanent magnetic materials, the entire sample shows typical ferromagnetic behavior. As lithium salts, Li2CO3 and LiAlO2 can be clearly identified by their characteristic diffraction patterns.

[0157] Leaching of heat-treated black material with Ca(OH)2:

[0158] A PFA flask was charged with 30 g of the above heat treated battery waste material and 9 g of solid Ca(OH)2. The solids were mixed. Then, 200 g of water was added under stirring and the whole mixture was refluxed for 6 hours. After 6 hours, the solid content was filtered off and the filtrate sample was taken and analyzed for Li (c(Li)=0.49 wt.-%) and F (c(F)=0.015 wt.-%).

[0159] Solid LiOH from leached LiOH filtrate

[0160] The filtrate obtained from the above experiment was then dried to produce solid LiOH as a monohydrate containing fluoride. Two different procedures were applied to adjust the fluoride content:

[0161] (A) Water is completely evaporated from 150 mL of a filtrate containing 0.49 wt.-% lithium and 0.015 wt.-% fluoride (40° C., 42 mbar). LiOH·LiF.1 is obtained. The XRD of LiOH·LiF.1 shows a small amount of Li2CO3 impurity. The latter is due to contact with air during most of the process steps. In addition to carbon-based impurities, elemental analysis shows fluoride as one of the main impurities (c(F)=0.5 wt.-%).

[0162] (B) Another 150 mL portion of the filtrate from another LiOH leaching experiment (containing 0.49 wt.-% lithium and 0.015 wt.-% fluoride) was concentrated 6-fold by evaporation (40° C., 42 mbar) (c(Li)=2.94 wt.-%), filtered and finally dried at 40° C. under a constant nitrogen flow for 24 h. XRD of LiOH·LiF.2 shows a small amount of Li2CO3 impurity. The latter is due to contact with air during most of the process steps. In addition to carbon-based impurities, elemental analysis shows fluoride as one of the main impurities (c(F)=0.25 wt.-%).

[0163] I.3 Synthesis of Li2CO3 containing fluoride, step (b.2)

[0164] CO2 was introduced into a LiOH solution containing 2.6 wt.-% lithium and 0.017 wt.-% fluoride for seven hours (ambient conditions, about 5 L / h). A white solid immediately emerged. After 7 hours, the solid was filtered off, dried and analyzed by XRD and by elemental analysis: Li2CO3·LiF.2 (Li=19.0 wt.-%, F=0.22 wt.-%). No separate LiF was detected.

[0165] II. Preparation of cathode active materials

[0166] II.1 Mixing step, step (c.1), and calcination, step (d.1)

[0167] “Battery grade” LiOH.H 2 O (hereinafter also referred to as “LiOH bg”, commercially available from Levent Corporation, having a fluoride content of less than 5 ppm) was used for mixing with LiOH.LiF.1.

[0168] Step (c.1): The precursor TM-OH.1 was mixed with a mixture of LiOH bg and LiOH·LiF.1 in a MICROTRON laboratory mixer from Kinematica at a molar ratio of Li / (Ni+Mn)=1.33:1 three times for one minute each time. The weight ratio of LiOH bg to LiOH·LiF.1 was 1:1. A mixture was obtained.

[0169] Step (d.1): The mixture from step (c.1) was heated to 950°C at a heating rate of 3°C / min and maintained for 6 h in a forced oxygen flow. After cooling to ambient temperature, the resulting powder was deagglomerated and sieved through a 32 μm sieve. CAM.1 was obtained. No fluoride agglomerates were detected.

[0170] Electrochemical testing was performed in a coin-type half-cell, showing excellent first cycle discharge capacity and cycling stability.

[0171] II.2 Production of cathode active material CAM.2

[0172] “Battery grade” Li 2 CO 3 (hereinafter also referred to as “Li 2 CO 3 bg”, commercially available from Levent Corporation, having a fluoride content of less than 5 ppm) was used for mixing with Li 2 CO 3 ·LiF. 2 .

[0173] Step (c.2): The precursor TM-OH.1 and Li2CO3·LiF.1 were mixed three times for one minute each time in a MICROTRON laboratory mixer from Cainmetall at a molar ratio of Li / (Ni+Mn)=1.33:1.

[0174] Step (d.2): The mixture from step (c.2) was heated to 950°C at a heating rate of 3°C / min and maintained for 6 h in a forced oxygen flow. After cooling to ambient temperature, the resulting powder was deagglomerated and sieved through a 32 μm sieve. CAM.2 was obtained. No fluoride agglomerates were detected.

[0175] D50=12 μm was determined using the laser diffraction technique in a Mastersizer 3000 instrument from Malvern Instruments. Li and transition metal contents were determined by ICP analysis. The residual moisture at 250° C. was determined to be less than 300 ppm.

[0176] II.3 Preparation of comparative cathode active material (C-CAM.3)

[0177] Compare step C-(b.3):

[0178] LiOH·H2O bg was mixed with LiF in a weight ratio of 99.66:0.34, corresponding to CAM.1. A premix was obtained. It can be seen from the crystals that LiF crystals are still present in the premix.

[0179] Step C-(c.3): The precursor TM-OH.1 and the premix from step C-(b.3) were mixed three times for one minute each at a molar ratio of Li / (Ni+Mn)=1.33:1 in a MICROTRON laboratory mixer from Cainmetall. A mixture was obtained.

[0180] Step C-(d.3): Step (d.1) was repeated, but using the mixture from step C-(c.3). After cooling to ambient temperature, the resulting powder was deagglomerated and sieved through a 32 μm sieve. C-CAM.3 was obtained. Several samples of C-CAM.3 showed different and inconsistent behavior compared to CAM.1 and CAM.2.

[0181] II.4 Preparation of comparative cathode active material (C-CAM.4)

[0182] Neither step (a) nor step (b) is performed.

[0183] Step C-(c.4): The precursor TM-OH.1 and LiOH·H2O bg were mixed three times in a MICROTRON laboratory mixer from Cainmetall at a molar ratio of Li / (Ni+Mn)=1.33:1 for one minute each time. A mixture was obtained.

[0184] Step C-(d.4): Repeat step (d.1), but use the mixture from step C-(c.4). After cooling to ambient temperature, the resulting powder is deagglomerated and sieved through a 32 μm sieve. C-CAM.4 is obtained.

[0185] III. Testing of cathode active materials

[0186] III.1 Cathode fabrication, general procedure

[0187] Positive electrode: PVDF binder ( 5130) was dissolved in NMP (Merck) to produce a 7.5 wt.% solution. For the preparation of the electrodes, the binder solution (3 wt.%) and carbon black (Super C65, 3 wt.-%) were suspended in NMP. After mixing using a planetary centrifugal mixer (ARE-250, Thinky Corp.; Japan), the CAM of the present invention (or comparative CAM) (94 wt.%) was added and the suspension was mixed again to obtain a lump-free slurry. The solid content of the slurry was adjusted to 61%. The slurry was coated on Al foil using a KTF-S roll-to-roll coater (Mathis AG). All electrodes were calendered before use. The thickness of the cathode material was 100 μm, corresponding to 6.5 mg / cm 2 Before cell assembly, all electrodes were dried at 105 °C for 7 h.

[0188] III.2 Electrolyte Preparation

[0189] A substrate electrolyte composition (EL substrate 1) was prepared containing 1 M LiPF6 in 3:7 by weight ethylene carbonate and ethyl methyl carbonate.

[0190] III.3 Fabrication of test cells

[0191] A coin-type half-cell (20 mm in diameter and 3.2 mm in thickness) comprising a cathode and lithium metal prepared as described under III.1 as a working electrode and a counter electrode, respectively, was assembled and packaged in an Ar-filled glove box. In addition, the cathode and anode and the separator were stacked in the order of cathode / / separator / / Li foil to produce a coin-type half-cell. Thereafter, 0.15 mL of the EL substrate 1 described above (II.2) was introduced into the coin-type half-cell.

[0192] IV. Battery Cell Performance Evaluation

[0193] Evaluation of Coin Cell Performance

[0194] The battery cell performance was evaluated using the produced button-type batteries.

[0195] The initial performance and rate performance were measured as follows: Coin half-cells according to III.3 were tested at 25°C in the voltage range between 4.3 V and 3.0 V. For the initial cycles, charging and discharging were performed in CC mode, i.e. a constant current (CC) of 0.1 C was applied until 4.3 V (during charging) or 3.0 V (during discharging) was reached, respectively. After the initial formation cycles, the rate characteristics were measured in CC mode with a constant discharge current of 3 C.

[0196] Cycling performance and resistance growth were tested as follows: After initial performance evaluation, the coin cell was cycled 100 times at 25° C. with a constant charge current of 0.5 C and a constant discharge current of 1 C. At the beginning of each discharge cycle, the resistance growth was measured by determining the voltage drop after 30 seconds.

[0197] The battery based on the cathode active material of the present invention is more excellent. In particular, CAM.1 and CAM.2 show higher cycle stability and lower resistance growth compared to C-CAM.3 and C-CAM.4. In particular, several samples of C-CAM.3 show completely different electrochemical behaviors. Without wishing to be bound by any theory, we assume that some samples of C-CAM.3 contain fluoride, while others do not.

Claims

1. A method for producing a fluoride-doped cathode active material, wherein the method comprises the following steps: (a) providing a particulate oxide or (oxy)hydroxide or carbonate of TM, wherein the TM comprises nickel and manganese and wherein at least 50 mol-% of the TM is manganese, wherein the particulate oxide or (oxy)hydroxide has an average particle size (D50) in the range of 1 to 16 μm, (b) providing a lithium source containing 0.01% to 2.5% by weight of fluoride uniformly dispersed in the lithium source, wherein the lithium source is selected from lithium hydroxide and lithium oxide and lithium carbonate, (c) mixing the oxide or (oxy)hydroxide or carbonate of said TM with said fluoride-containing lithium source, and optionally with an additional lithium source containing less fluoride, and optionally with one or more dopants based on at least one metal other than lithium, (d) subjecting the mixture obtained in step (c) to heat treatment.

2. The method according to claim 1, wherein: TM is a metal combination according to the general formula (I) (Ni a Co b Mr c ) 1-d M d (I) in a is in the range of 0.2 to 0.5, b is 0 or in the range of 0.01 to 0.1, c is in the range of 0.5 to 0.8, and d is in the range of 0 to 0.1, M is at least one of Al, Mg, Ti, Mo, Nb, Ta, W and Zr, and a+b+c=1.

3. The method according to claim 1 or 2, wherein: The lithium source is selected from lithium hydroxide and lithium oxide.

4. A method according to any one of the preceding claims, wherein: Step (d) is carried out at a temperature in the range of 850°C to 1150°C.

5. A method according to any one of the preceding claims, wherein: The weight ratio of the fluoride-containing lithium source to the fluoride-free lithium source is in the range of 1:1 to 1:

20.

6. A method according to any one of the preceding claims, wherein: The mixing step (c) is carried out in at least two sub-steps. (c1) mixing a fluoride-containing lithium source with a fluoride-free lithium source, and (c2) mixing the mixture obtained in step (c1) with an oxide or (oxy)hydroxide or carbonate of said TM and - if applicable - with one or more dopants.

7. A method according to any one of the preceding claims, wherein: The one or more dopants are selected from oxides and hydroxides of Al, Mg, and transition metals selected from Ti, Mo, Nb, Ta, W, and Zr.

8. A method according to any one of the preceding claims, wherein: The lithium source in which the fluoride is uniformly dispersed is obtained by a method of recycling waste batteries.

9. A method according to any one of the preceding claims, wherein: The fluoride is lithium fluoride.

10. A method according to any one of the preceding claims, wherein: The stoichiometry of lithium in step (c) is in the range from 90 to 95 mol-% relative to the sum of TM and - if applicable - the metal other than lithium from the one or more dopants, and step (d) is followed by another step of mixing with a lithium source and another step of heat treatment.

11. A method according to any one of the preceding claims, wherein: In the lithium source provided in step (b), individual crystals or agglomerates of fluoride may not be detected by particle size distribution and X-ray diffraction and SEM / EDX.

12. A method according to the general formula Li 1+x TM 1-x O 2-y F y A granular cathode active material having an average particle size (D50) in the range of 1 to 16 μm, wherein TM comprises nickel and manganese, and wherein at least 50 mol-% of TM is manganese, and wherein x is in the range of 0.05 to 0.4, and wherein y is in the range of 0.0002 to 0.03, and wherein F is uniformly distributed in such cathode active material and does not accumulate on the surface of the secondary particles of such cathode active material.

13. The particulate cathode active material according to claim 12, wherein TM is a metal combination according to the general formula (I) (Ni a Co b Mr c ) 1-d M d (I) in a is in the range of 0.2 to 0.5, b is 0 or in the range of 0.01 to 0.1, c is in the range of 0.5 to 0.8, and d is in the range of 0 to 0.1, M is at least one of Al, Mg, Ti, Mo, Nb, Ta, W and Zr, and a+b+c=1.

14. A cathode comprising (A) at least one particulate cathode active material according to claim 12 or 13, (B) carbon in an electrically conductive form, (C) Adhesive material.

15. A battery comprising (1) at least one cathode according to claim 14, (2) at least one anode, and (3) At least one electrolyte.

Citation Information

Patent Citations

  • Particles, process for production thereof and use thereof

    US20130209840A1

  • Method of manufacturing lithium nickel complex oxide, lithium nickel complex oxide manufactured thereby, and cathode active material including the same

    US20150064563A1

  • Nonaqueous electrolyte secondary battery and method for manufacturing the same

    US5773168A