Gallium nitride sintered body and method for producing same

By nitriding gallium metal under a nitrogen compound gas atmosphere to form a dense surface layer, the densification and re-oxidation problems of gallium nitride sintered bodies in hot pressing are solved, and a high-density gallium nitride sintered body with low oxygen content is prepared, which is suitable for applications such as sputtering targets.

CN118922395AActive Publication Date: 2024-11-08TOSOH CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202380029836.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-25
Filing Date
2023-03-17
Publication Date
2024-11-08
Estimated Expiration
2043-03-17

AI Technical Summary

Technical Problem

Gallium nitride sintered bodies prepared by existing hot pressing processes are difficult to densify and are prone to re-oxidation, leading to increased oxygen content and affecting their application performance.

Method used

By nitriding metallic gallium under specific conditions to form a dense surface layer, and then reacting it in a nitrogen-containing compound gas atmosphere, while controlling the reaction temperature and gas flow rate, a gallium nitride sintered body with high density and low oxygen content is prepared.

Benefits of technology

It achieves densification and re-oxidation suppression of gallium nitride sintered bodies, improves mechanical properties and oxygen content control, and is suitable for applications such as sputtering targets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922395A_ABST
    Figure CN118922395A_ABST
Patent Text Reader

Abstract

Provided are: a sintered body of high gallium nitride in which an increase in oxygen content due to re-oxidation after sintering is suppressed compared with conventional sintered bodies of gallium nitride obtained by hot pressing; a method for producing the sintered body; and at least one of the uses of the sintered body of high gallium nitride. A sintered body of gallium nitride has a surface layer having a higher density than the interior of the sintered body, and the atomic weight ratio of gallium to the sum of gallium and nitrogen is more than 0.5 and 0.60 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a sintered body of gallium nitride. Background Art

[0002] In order to stably form a gallium nitride film by sputtering, a sintered body of gallium nitride (GaN) is used as a sputtering target. Such a sintered body of gallium nitride is manufactured, for example, by hot isostatic pressing (hereinafter also referred to as "HIP") treatment. However, the HIP treatment not only has high manufacturing costs, but also makes it difficult to produce a large sintered body. On the other hand, hot pressing (hereinafter also referred to as "HP") treatment is known as a method for manufacturing a sintered body of gallium nitride that is cheaper than the HIP treatment. However, gallium nitride is difficult to densify in the HP treatment. In addition, the sintered body obtained by the HP treatment is prone to increase in oxygen content after sintering due to oxidation of residual metallic gallium and gallium nitride, that is, reoxidation of the sintered body.

[0003] Therefore, further densification and reduction of oxygen content in a sintered body of gallium nitride produced by HP treatment have been studied so far (for example, Patent Documents 1 to 3).

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2012-144424

[0007] Patent Document 2: Japanese Patent Application Publication No. 2017-024970

[0008] Patent Document 3: Japanese Patent Application Publication No. 2019-001681 Summary of the invention

[0009] Problem that the invention aims to solve

[0010] Patent Document 1 reduces the oxygen content of the sintered body by reducing gallium oxide by flowing ammonia gas through the sintered body obtained by HP treatment. However, since gallium oxide has a higher density than gallium nitride, it is difficult to further densify the gallium nitride sintered body while reducing gallium oxide.

[0011] Patent Documents 2 and 3 use gallium nitride powder with low oxygen concentration as a raw material of gallium nitride. When using this powder, a sintered body with low oxygen content can be obtained. However, Patent Documents 2 and 3 are improvements from the raw material aspect and do not solve the problem of HP treatment itself. In addition, they are not technologies for directly preventing the increase of oxygen content in the sintered body caused by reoxidation.

[0012] The present disclosure aims to provide at least one of a gallium nitride sintered body in which an increase in oxygen content due to reoxidation after sintering is suppressed compared with a conventional gallium nitride sintered body obtained by HP treatment, a method for producing the same, and a use thereof.

[0013] Solutions for solving problems

[0014] The present inventors have studied the prevention of reoxidation and densification of a sintered body of gallium nitride obtained by HP treatment after sintering, focusing on the metal gallium contained in the sintered body of gallium nitride. They have further found that by nitriding such metal gallium under specific conditions, the sintered body can be densified and reoxidation after sintering can be suppressed.

[0015] That is, the present invention is described in the claims, and the gist of the present disclosure is as follows.

[0016] [1] A sintered body of gallium nitride having a surface layer having a higher density than the interior of the sintered body, wherein the atomic weight ratio of gallium to the sum of gallium and nitrogen is greater than 0.5 and less than 0.60.

[0017] [2] The sintered body according to [1] above, wherein the oxygen content is 0.3 atm % or less.

[0018] [3] The sintered body according to [1] or [2], wherein the measured density is 3.80 g / cm 3 Above and 5.50g / cm 3 the following.

[0019] [4] The sintered body according to any one of [1] to [3] above, comprising metal gallium.

[0020] [5] A method for producing a sintered body according to any one of [1] to [4], comprising the following steps:

[0021] The nitrogen-containing compound gas is reacted with the bulk of gallium nitride at a reaction temperature of 1025° C. or less in an atmosphere where the nitrogen-containing compound gas flows at a flow rate of 0.5 L / min or more.

[0022] [6] The manufacturing method according to [5] above, wherein the block is a pre-sintered body of gallium nitride.

[0023] [7] The production method according to [6] above, wherein the pre-sintered body is a sintered body of gallium nitride obtained by hot pressing.

[0024] [8] The manufacturing method according to [5] above, wherein the bulk is a molded body of gallium nitride.

[0025] [9] The production method according to any one of [5] to [8] above, wherein the bulk contains metal gallium at least on the surface.

[0026]

[10] The production method according to any one of [5] to [9] above, wherein the nitrogen-containing compound gas is one or more gases selected from the group consisting of ammonia, hydrazine, and alkylamines.

[0027]

[11] A sputtering target comprising the sintered body according to any one of [1] to [4] above.

[0028] Effects of the Invention

[0029] According to the present disclosure, it is possible to provide a gallium nitride sintered body in which an increase in oxygen content due to reoxidation after sintering is suppressed compared to a conventional gallium nitride sintered body obtained by HP treatment, a method for producing the same, and at least any one of the uses thereof. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a SEM observation picture of the cross section of the sintered body of Example 4 (magnification: 500 times).

[0031] Figure 2 This is a SEM observation picture of the cross section of the sintered body of Comparative Example 1 (magnification: 500 times). DETAILED DESCRIPTION

[0032] Hereinafter, the sintered body of the present disclosure will be described with reference to an example of the embodiment.

[0033] The sintered body of the present embodiment is a gallium nitride sintered body having a surface layer having a higher density than the interior of the sintered body and in which the atomic weight ratio of gallium to the total of gallium and nitrogen exceeds 0.5 and is 0.60 or less.

[0034] The present embodiment relates to a sintered body of gallium nitride. The sintered body of gallium nitride (GaN) is a sintered body with gallium nitride as the main component (matrix, parent phase), a sintered body mainly composed of gallium nitride, a so-called gallium nitride sintered body, but may also contain components other than gallium nitride such as metallic gallium, preferably containing metallic gallium. For example, the sintered body of the present embodiment may include a sintered body containing metallic gallium and having gallium nitride as the main component.

[0035] The sintered body of the present embodiment may contain doping elements. As doping elements for forming an n-type semiconductor, one or more selected from the group consisting of silicon (Si), germanium (Ge), tin (Sn) and lead (Pb) can be cited. In addition, as doping elements for forming a p-type semiconductor, one or more selected from the group consisting of beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), vanadium (Ba), zinc (Zn) and cadmium (Cd) can be cited. In addition, as doping elements for forming an LED of any color, at least one of aluminum (Al) and indium (In) can be cited.

[0036] The sintered body of this embodiment has a surface layer having a higher density than the inner part of the sintered body. The surface layer is not easily oxidized and can significantly suppress reoxidation of the sintered body.

[0037] In this embodiment, the surface layer and the interior of the sintered body can be observed by scanning electron microscope (hereinafter also referred to as "SEM") observation of the cross section of the sintered body. Figure 1 As shown in the SEM observation of the cross section of the sintered body, in the direction from the surface toward the opposite surface ( Figure 1 The dense tissue structure changes to a sparse tissue structure in the direction of the arrow; hereinafter also referred to as the "thickness direction"), and it can be confirmed that there are areas where dense parts and sparse parts coexist ( Figure 1 The presence of a change region that can be observed in a SEM observation image with a magnification of 100 to 500 times is considered to be a surface layer of the sintered body. Figure 2 As shown in FIG. 1 , when the structure is uniform in the thickness direction and no variation region is confirmed, it is considered that there is no surface layer.

[0038] In the sintered body of the present embodiment, the density of the surface layer is higher than that of the interior of the sintered body. By having such a surface layer, the mechanical properties of the sintered body become higher. The density of the surface layer and the interior of the sintered body can be confirmed by the SEM observation image of the cross section of the sintered body. That is, first, as the surface layer, an area of ​​0 to 1% in the thickness direction (hereinafter also referred to as the "surface area") is subjected to SEM observation, and as the interior of the sintered body, an area of ​​40 to 50% in the thickness direction (hereinafter also referred to as the "internal area") is subjected to SEM observation. Next, use conventional image analysis software (such as Image-Pro10, manufactured by Hakto Corporation) to perform image analysis on the surface area and the internal area, respectively, and detect pores and their areas. The pores can be detected from the SEM observation. Figure 2 As a result of image analysis, the area [μm] of the part excluding the pores is used to detect 2 ] Relative to the observation area of ​​SEM observation image [μm 2], the area density [%] of each area can be calculated by the following formula.

[0039] Area density [%] = {(area of ​​the portion excluding pores) / (observation area of ​​the SEM observation image)}×100

[0040] In the sintered body of the present embodiment, the area density of the surface layer may be higher than the area density of the interior of the sintered body. For example, the area density of the surface layer is preferably higher than the area density of the interior of the sintered body, and the area density difference (=(area density of the surface region)-(area density of the interior region)) is preferably 10% or more, 15% or more, or 20% or less, and may be exemplified as 30% or less or 25% or less. The upper and lower limits of the area density difference of the sintered body may be any combination of the above, and may be, for example, 10% or more and 30% or less, or 20% or more and 25% or less.

[0041] In addition, as for the density inside the sintered body, as the area density, less than 90%, less than 80%, less than 70%, less than 65%, less than 60%, or less than 58% can be cited, and 50% or more or 55% or more can be exemplified. The upper limit and lower limit of the area density inside the sintered body can be any combination of the above, for example, 50% or more and less than 90%, 50% or more and 65% or more, or 55% or more and 60% or less can be cited.

[0042] In the present embodiment, the thickness of the surface layer is arbitrary, for example, 10 μm or more, 20 μm or more, or 50 μm or more. In addition, 500 μm or less, 300 μm or less, 200 μm or less, 150 μm or less, 120 μm or less, 100 μm or less, or 80 μm or less. For example, 10 μm or more and 500 μm or less, 10 μm or more and 100 μm or less, or 20 μm or more and 80 μm or less can be mentioned. The thickness of the surface layer is the thickness measured as the length from the outermost surface to the change region in the SEM observation image of the cross section of the sintered body of the present embodiment. According to the SEM observation image, the thickness of 5 points is measured at equal intervals in a direction perpendicular to the thickness direction in 5 or more fields of view, preferably 10±2 fields of view, and the average value thereof can be obtained.

[0043] The bulk density of the sintered body of this embodiment is preferably 3.80 g / cm 3 Above and 5.50g / cm 3 The bulk density is preferably 3.80 g / cm 3 Above, 4.00g / cm 3 Above or 4.20g / cm 3By having such a bulk density, the sintered body of this embodiment can easily have sufficient strength when used as a sputtering target. The higher the bulk density, the more preferred it is. For example, 5.00 g / cm 3 Below, 4.80g / cm 3 Below or 4.70g / cm 3 The upper and lower limits of the bulk density of the sintered body may be any combination of the above, and an example thereof is 3.80 g / cm 3 Above and 5.00g / cm 3 Below, or 4.20g / cm 3 Above 4.70g / cm 3 the following.

[0044] In the present embodiment, the “density” refers to a bulk density measured by a method in accordance with JIS R1634, and the pretreatment may be performed by a vacuum method using distilled water.

[0045] In the sintered body of the present embodiment, the atomic weight ratio of gallium to the sum of gallium and nitrogen ([mol / mol]; hereinafter also referred to as "Ga / (Ga+N)") exceeds 0.5 and is less than or equal to 0.60. By setting Ga / (Ga+N) to this range, the dissolution of metallic gallium can be suppressed, and reoxidation can be suppressed. Since there is a tendency to be further less prone to reoxidation, Ga / (Ga+N) is preferably greater than or equal to 0.51, greater than or equal to 0.52, or greater than or equal to 0.53, and is preferably less than or equal to 0.58, less than or equal to 0.57, less than or equal to 0.56, less than or equal to 0.55, or greater than or equal to 0.54. The upper and lower limits of Ga / (Ga+N) of the sintered body may be any combination of the above, for example, greater than 0.5 and less than or equal to 0.58, greater than or equal to 0.51 and less than or equal to 0.56, greater than or equal to 0.52 and less than or equal to 0.55, or greater than or equal to 0.53 and less than or equal to 0.54.

[0046] The oxygen content of the sintered body of the present embodiment is preferably 0.3 atm% or less, more preferably 0.2 atm% or less, and further preferably 0.1 atm% or less. The sintered body of the present embodiment is preferably oxygen-free (i.e., the oxygen content is 0 atm%), and examples thereof include an oxygen content of 0 atm% or more, more than 0 atm% or more than 0.01 atm%. If it is such an oxygen content, the film obtained by sputtering it tends to show characteristics that are more suitable for uses such as light-emitting diodes and power devices. The upper and lower limits of the oxygen content of the sintered body can be any combination of the above, for example, 0 atm% or more and 0.3 atm% or less. Examples include 0 atm% or more and 0.2 atm% or less, more than 0 atm% and 0.2 atm% or less, or 0.01 atm% or more and 0.1 atm% or less.

[0047] The composition of the sintered body of the present embodiment can be regarded as a composition represented by the following formula.

[0048] 100 = W Ga [Mass %] + W O [Mass %] + W N [Mass %] + W X [Mass %] (1)

[0049] (1)W Ga , W O , W N and W X are the mass proportions of gallium, oxygen, nitrogen and doping elements in the sintered body. O and W N W is a value measured by a thermal decomposition method using a conventional oxygen and nitrogen analyzer (e.g., LECO ON736, manufactured by Leco) to thermally decompose a gallium nitride sintered body. X is the value determined by glow discharge mass spectrometry. Ga According to W O , W N and W X The measured value of is the value obtained by formula (1).

[0050] The oxygen content is a value obtained from the following formula (2).

[0051] Oxygen content [atm%] =

[0052] (W O / M O ) / {(W Ga / M Ga )+(W N / M N )+(W O / M O )+(W X / M X )}(2)

[0053] (2) In the formula, M O The atomic weight of oxygen is 16.00 [g / mol], M Ga The amount of gallium in oxygen: 69.72 [g / mol], and M N The atomic weight of nitrogen is 14.01 [g / mol]. X It is the atomic weight of the doping element, for example, the atomic weight of silicon is 28.09 [g / mol], the atomic weight of magnesium is 24.31 [g / mol], the atomic weight of aluminum is 26.98 [g / mol], and the atomic weight of indium is 114.82 [g / mol].

[0054] Ga / (Ga+N) is a value obtained from the following formula (3).

[0055] Ga / (Ga+N)=(W Ga / M Ga ) / {(W Ga / M Ga )+(W N / M N )} (3)

[0056] The sintered body of the present embodiment can be used for known uses of sintered bodies of gallium nitride, but is particularly preferably used as a sintered body for a sputtering target.

[0057] Next, a method for producing a sintered body according to the present embodiment will be described.

[0058] The manufacturing method of the sintered body of the present embodiment is arbitrary as long as it is a manufacturing method having the above-mentioned characteristics. As a preferred manufacturing method, a manufacturing method having the following steps can be cited: in a nitrogen-containing compound gas circulation atmosphere of 0.5L / min or more, the nitrogen-containing compound gas is reacted with a bulk of gallium nitride at a reaction temperature of 1025°C or less. It has been studied to make a sintered body of gallium nitride react with a nitrogen-containing compound gas. However, in the present embodiment, it is found that the circulation rate of the nitrogen-containing compound gas affects the reaction state with the sintered body of gallium nitride, and further, by controlling the circulation rate of the nitrogen-containing compound gas, the reaction on the surface of the bulk can be promoted, and the sintered body of the present embodiment can be easily obtained. In the present embodiment, the bulk refers to an object that is not amorphous but has a certain shape, such as a powder or a liquid, and examples thereof include a sintered body and a molded body.

[0059] By allowing the nitrogen-containing compound gas to react with the bulk of gallium nitride in an atmosphere where the nitrogen-containing compound gas flows at a flow rate of more than 0.5 L / min (hereinafter also referred to as the "densification process"), the metallic gallium present on the surface of the sintered body of gallium nitride is effectively nitrided to form a dense gallium nitride layer (surface layer).

[0060] The bulk of gallium nitride (hereinafter also referred to as "bulk") provided for the densification process is essentially a bulk composed of gallium nitride, but preferably contains metallic gallium as a trace component, preferably is a bulk of gallium nitride containing metallic gallium, and further preferably is a bulk of gallium nitride containing metallic gallium at least on the surface.

[0061] The bulk is preferably a pre-sintered body of gallium nitride containing metallic gallium, and more preferably a pre-sintered body of gallium nitride containing metallic gallium at least on the surface. Such a sintered body may be a sintered body of gallium nitride obtained by any manufacturing method, but is preferably a sintered body of gallium nitride obtained by HIP treatment or HP treatment, and more preferably a sintered body of gallium nitride obtained by HP treatment. The sintered body of gallium nitride obtained by HP treatment is likely to contain metallic gallium on its surface.

[0062] The bulk is preferably a molded body of gallium nitride containing metal gallium, and more preferably a molded body of gallium nitride containing metal gallium at least on the surface. The molded body of gallium nitride obtained by molding easily contains metal gallium on its surface.

[0063] In addition, Ga / (Ga+N) of the bulk can be more than 0.50 or more than 0.55. Ga / (Ga+N) of the bulk is less than 0.60 or less than 0.58. The upper and lower limits of Ga / (Ga+N) of the bulk can be any combination of the above, for example, more than 0.50 and less than 0.60, more than 0.50 and less than 0.58, or more than 0.55 and less than 0.58.

[0064] The bulk preferably contains metal gallium at least on the surface. By containing metal gallium on the surface, the metal gallium present on the surface is nitrided by the densification process, and the surface is easily densified. In this embodiment, the inclusion of metal gallium in the bulk can be confirmed by having an XRD peak of Ga (metal) in its surface XRD pattern.

[0065] The bulk preferably does not contain gallium oxide. In the present embodiment, "does not contain gallium oxide" means that there is no powder X-ray diffraction peak of gallium oxide in the powder X-ray diffraction pattern. The bulk may contain gallium oxide to the extent that no powder X-ray diffraction peak of gallium oxide can be confirmed in its powder X-ray diffraction pattern. No powder X-ray diffraction peak of gallium oxide can be confirmed means that the ratio of the peak intensity of the gallium oxide (002) plane to the peak intensity of the gallium nitride (002) plane is less than 1%.

[0066] The oxygen content of the bulk is preferably less than 0.3 atm%, less than 0.2 atm%, or less than 0.1 atm%. This makes it easy to suppress the formation of pores caused by the detachment of oxygen in the densification process and the increase in surface roughness caused by this. The oxygen content of the bulk is preferably low, but it can be exemplified as more than 0 atm% or more than 0 atm%. The upper and lower limits of the oxygen content of the bulk can be any combination of the above.

[0067] The bulk density of the block is preferably 3.50 g / cm 3 Above or 4.00g / cm 3 If the bulk density of the block is 3.50 g / cm3 The above-mentioned process can obtain a gallium nitride sintered body having practical mechanical strength through the densification step. The bulk density is preferably high, and an example thereof is 5.00 g / cm 3 Below or 4.80g / cm 3 The upper limit and lower limit of the bulk density of the block may be any combination of the above.

[0068] In the densification process, the nitrogen-containing compound gas is reacted with the bulk of gallium nitride at a reaction temperature of 1025°C or less in a nitrogen-containing compound gas circulation atmosphere of 0.5 L / min or more. In a nitrogen-containing circulation atmosphere of less than 0.5 L / min, the reaction between metallic gallium and the nitrogen-containing compound gas will not proceed sufficiently, and even if the reaction proceeds, gallium nitride will not be formed to the extent that the surface of the bulk is densified. The flow rate of the nitrogen-containing compound gas is 0.5 L / min or more, preferably 1.0 L / min or more or 2.0 L / min or more. The flow rate of the nitrogen-containing compound gas does not need to be increased more than necessary, and may be less than 10.0 L / min, less than 8.0 L / min, or less than 7.0 L / min. The flow rate of the nitrogen-containing compound gas may be any combination of the above, for example, 0.5 L / min to 10.0 L / min, 1.0 L / min to 8.0 L / min, 2.0 L / min to 7.0 L / min, or 2.0 L / min to 4.0 L / min.

[0069] In the present embodiment, the "nitrogen-containing compound gas" is a gas containing a compound containing a nitrogen atom in its structure, preferably a gas containing a nitrogen-containing compound that reacts with the bulk. Specific nitrogen-containing compound gases include one or more gases selected from the group consisting of ammonia, hydrazine, and alkylamines, and further include ammonia gas.

[0070] In the densification step, the nitrogen-containing compound gas is reacted with the block under a nitrogen-containing compound gas circulation atmosphere at a reaction temperature of 1025°C or less. The reaction can be carried out under conditions where the nitrogen-containing compound gas contacts the block and promotes nitridation of the block, and can be carried out using one or more selected from the group consisting of a sintering furnace, a tubular furnace, and an atmosphere furnace, preferably an atmosphere furnace. In addition, the reaction can be carried out under a nitrogen-containing compound gas circulation atmosphere, and further, it can be carried out under any of a pressurized atmosphere and an atmospheric pressure atmosphere. For simplicity, it is preferably carried out under an atmospheric pressure atmosphere.

[0071] The reaction temperature is below 1025°C. If the reaction temperature exceeds 1025°C, the nitridation of the surface of the sintered body proceeds rapidly in the atmosphere of the densification process in the present embodiment, thereby producing defects such as surface peeling. As a result, in addition to low density, it is also susceptible to reoxidation after sintering. The reaction temperature is preferably below 1020°C, more preferably below 1000°C, and further preferably below 990°C. The reaction temperature can be any temperature at which the reaction of the nitrogen-containing compound gas and the bulk is carried out. If it is above 900°C or above 950°C, the reaction is carried out efficiently. The upper and lower limits of the reaction temperature can be any combination of the above, for example, 900°C or above and 1020°C or below, 900°C or above and 1000°C or above and 950°C or below.

[0072] The temperature increase rate to the reaction temperature is arbitrary, and for example, it may be 100° C. / hour or more and 400° C. / hour or less.

[0073] The treatment time of the nitrogen-containing compound gas and the block at the reaction temperature (hereinafter also referred to as "holding time") can be arbitrarily set according to the amount and size of the block provided for the reaction and the performance of the reactor used in the reaction, and can be 0.5 hours or more, 1 hour or more, 10 hours or less, or 5 hours or less at the above reaction temperature. The upper limit and lower limit of the treatment time can be any combination of the above, for example, 0.5 hours or more and 10 hours or more, or 1 hour or more and 5 hours or less.

[0074] The production method of the present embodiment may include a step of processing the sintered body after the densification step (hereinafter also referred to as a “processing step”).

[0075] The processing step is a step of processing the sintered body of gallium nitride into a shape corresponding to the desired use. For example, when the sintered body of the present embodiment is used as a sputtering target, it can be processed by one or more processing methods selected from the group consisting of surface grinding, rotary grinding, and cylindrical grinding. In addition, in the processing step, the sintered body can also be joined to a backing plate.

[0076] Next, a sputtering target including a sintered body according to the present embodiment will be described.

[0077] A sputtering target including the sintered body of the present embodiment (hereinafter, also referred to as “the target of the present embodiment”) is a sputtering target in which the sintered body of the present embodiment is bonded to a support body via a bonding layer.

[0078] The shape of the target of the present embodiment is arbitrary, and at least any one of a flat plate shape and a cylindrical shape, and other shapes suitable for the application can be exemplified.

[0079] The target of the present embodiment joins (i.e., bonds) the sintered body of the present embodiment to a support body through a joining layer. The joining layer only needs to be composed of a solder containing one or more selected from the group of tin, indium and zinc. Since the electrical conductivity and thermal conductivity of the target are likely to be high, the joining layer is preferably composed of a solder containing indium. It should be noted that, in the case where the joining layer is a solder containing indium, the target of the present embodiment may have a layer (hereinafter also referred to as a "barrier layer") for improving wettability between the sintered body of gallium nitride and the joining layer. As a result, the indium wettability of the gallium nitride sintered body is improved, and as a result, the bonding between the sintered body of gallium nitride and the joining layer becomes more secure. The barrier layer only needs to be composed of a component with high wettability to indium, preferably at least one of nickel and chromium.

[0080] On the other hand, since the cost increases, the target of the present embodiment preferably does not have a layer containing tungsten (W), and particularly preferably does not have a layer containing tungsten as a barrier layer.

[0081] The support body in the target of the present embodiment is preferably one or more selected from the group consisting of copper, stainless steel and titanium. In addition, the shape of the support body can be any desired shape corresponding to the shape of the sintered body of the present embodiment, and at least one of a flat plate and a cylindrical shape, and other shapes suitable for the purpose can be exemplified.

[0082] Example

[0083] Hereinafter, the present disclosure will be described by way of examples, but the present disclosure is not limited to these examples.

[0084] (composition)

[0085] The oxygen [mass %] and nitrogen mass ratio [mass %] of the gallium nitride sintered body were measured by inert gas melting-infrared absorption method using an oxygen / nitrogen analyzer (device name: LECO ON736, manufactured by Leco). Based on the obtained oxygen and nitrogen mass ratios, the gallium mass ratio was calculated by the above formula (1), the oxygen content [atm %] was calculated by the above formula (2), and Ga / (Ga+N) was calculated by the above formula (3).

[0086] (Volume Density)

[0087] The bulk density of the gallium nitride sintered body was measured by a method in accordance with JIS R 1634. The pretreatment was performed by a vacuum method using distilled water.

[0088] (density)

[0089] As the density of the surface layer and the inside of the sintered body, the cross section of the sintered body was observed by SEM, and the area density of each was obtained from the obtained SEM observation figure. That is, the cross section observation was performed by embedding the sintered body with resin, cutting it and grinding it to a surface roughness Ra≤1.0μm, thereby exposing the cross section. The cross section was observed using SEM (device name: VE-9800, manufactured by KEYENCE). The conditions for SEM observation are as follows.

[0090] Accelerating voltage: 10 kV

[0091] Observation magnification: (surface area) 100 times, (internal area) 500 times

[0092] Observation field of view: 10 fields of view

[0093] In the SEM observation image of the cross section, the area of ​​0 to 1% in the thickness direction from the surface of the sintered body is regarded as the surface area, and the area of ​​40 to 50% in the thickness direction is regarded as the internal area, and the area density is calculated by image analysis of each SEM observation image. That is, the SEM observation image of the cross section is analyzed using image analysis software (software name: Image-Pro10, manufactured by Hakto Corporation). Figure 2 The pores are detected and their area [μm 2 After detection, the area [μm 2 ] relative to the observation area of ​​the SEM observation image [μm 2 ], and the area density [%] of the surface area and the internal area is calculated by the following formula.

[0094] Area density = {(area of ​​the region excluding the pores) / (observation area of ​​the SEM observation image)}×100

[0095] For one measurement sample, SEM observation images of cross sections in 10 fields of view were subjected to image analysis, and the average value thereof was taken as the area density of each measurement sample.

[0096] (Thickness of surface layer)

[0097] In the SEM observation figure of the cross section obtained by the same method as the area density of the surface layer, the region where the density changes in the surface layer is regarded as the variable region, and the region from the surface to the variable region is regarded as the surface layer, and its thickness is measured. 10 visual fields are carried out this measurement, and its average value is used as the thickness of the surface layer.

[0098] (Vickers hardness)

[0099] The Vickers hardness of the sintered body was measured by a method based on JIS Z 2244. Five points of measurement were performed on one measurement sample, and the average value was taken as the Vickers hardness.

[0100] (Determination of flexural strength)

[0101] The three-point bending strength of the sintered body was measured by a method in accordance with JIS R 1601. The measurement was performed twice, and the average value was taken as the bending strength.

[0102] Example 1

[0103] 50 g of gallium nitride powder (purity 4N; 99.99%) is filled into a cylindrical carbon container with a diameter of 53 mm. The carbon container is placed in a hot pressing device, and the temperature is raised to 1000°C at a heating rate of 200°C / hour, and hot pressing is performed for 2 hours at a processing temperature of 1070°C and a processing pressure of 40 MPa. After the hot pressing treatment, the gallium nitride sintered body is recovered after cooling to about 50°C in 5 hours. The gallium nitride sintered body is cut to form a circular plate-shaped gallium nitride sintered body with a diameter of 2 inches (=5.3 mm) and a thickness of 3.8 mm, which is used as a pre-sintered body. The volume density of the pre-sintered body is 4.47 g / cm 3 , the XRD peak of metal Ga was confirmed in the XRD pattern.

[0104] The obtained provisionally sintered body was placed in an atmosphere furnace (product name: MS-4272, manufactured by Motoyama Corporation) and heat-treated under the following conditions to obtain a sintered body of this example.

[0105] Heat treatment atmosphere: Ammonia flow atmosphere (ammonia flow rate: 2L / min)

[0106] Heating rate: 200℃ / hour

[0107] Keeping temperature: 980℃

[0108] Holding time: 1 hour

[0109] Cooling speed: 200℃ / hour

[0110] Example 2

[0111] The sintered body of this example was obtained by the same method as in Example 1 except that the flow rate of ammonia gas was changed to 4 L / min.

[0112] Example 3

[0113] The sintered body of this example was obtained by the same method as in Example 1 except that the flow rate of ammonia gas was changed to 6 L / min.

[0114] Example 4

[0115] A sintered body of this example was obtained in the same manner as in Example 1 except that the holding time at 980° C. was changed to 5 hours.

[0116] Example 5

[0117] A sintered body of this example was obtained in the same manner as in Example 1 except that the holding time at 980° C. was changed to 10 hours.

[0118] Example 6

[0119] Prepare 8g of mixed powder of metal gallium and gallium nitride with a Ga / (Ga+N) ratio of 0.59, and fill it into a rectangular mold of 10mm in length and 40mm in width. After filling, perform uniaxial stamping at a pressure of 100MPa to obtain a molded body. Perform cold isostatic pressing at a pressure of 300MPa to make a CIP-treated body. Arrange the CIP-treated body (compressed powder body) on an alumina setter plate, and sinter it in an atmosphere furnace under the following conditions to obtain a sintered body of this embodiment.

[0120] Heat treatment atmosphere: Ammonia flow atmosphere (ammonia flow rate 2L / min)

[0121] Heating rate: 200℃ / hour

[0122] Keeping temperature: 950℃

[0123] Holding time: 5 hours

[0124] Cooling speed: 200℃ / hour

[0125] Comparative Example 1

[0126] A sintered body of gallium nitride obtained by the same method as the pre-sintered body used in Example 1 was used as a sintered body of this comparative example.

[0127] Comparative Example 2

[0128] A sintered body of this comparative example was obtained in the same manner as in comparative example 1 except that the holding temperature was set to 1030°C.

[0129] Table 1 shows the production conditions of Examples and Comparative Examples, and Table 2 shows the evaluation results.

[0130] [Table 1]

[0131]

[0132] [Table 2]

[0133]

[0134] It can be confirmed from the above table that in the embodiment, the area density of the surface region is higher than the area density of the internal region, and the surface layer has a higher density than the inside of the sintered body. On the other hand, it can be confirmed that in Comparative Example 1 that has not undergone a densification process, the area density of the surface region and the internal region are equal, there is no surface layer, and the oxygen content becomes high. In addition, although Comparative Example 2 is a pre-sintered body treated the same as the embodiment, Ga / (Ga+N) is less than 0.5, and the oxygen content is high, and it can be confirmed that it is easy to be reoxidized. Therefore, it can be confirmed that the increase in the oxygen content of the sintered body of the embodiment is suppressed.

[0135] In addition, through densification treatment, Example 2 is 0.07g / cm 3 , Example 3 is 0.08g / cm 3 , Example 4 is 0.09g / cm 3 , and the bulk density increased. It can be confirmed that the bulk density of the sintered body tends to increase by the densification treatment of the examples.

[0136] Measurement example

[0137] The Vickers hardness and flexural strength of the sintered bodies of the examples and comparative examples were measured. The measurements were performed on each sintered body (hereinafter also referred to as "unprocessed sintered body") and a sintered body whose surface layer was removed by grinding (hereinafter also referred to as "processed sintered body"), respectively. It should be noted that Comparative Example 1 does not have a surface layer, so the flexural strength and the like were measured without the above-mentioned processing. The results are shown in the table below.

[0138] [Table 3]

[0139]

[0140] It can be confirmed from the above table that the sintered body of the embodiment has Vickers hardness and flexural strength due to the presence of the surface layer. In addition, for the sintered body of Comparative Example 2, the Vickers hardness and flexural strength of its unprocessed sintered body are higher than the Vickers hardness and flexural strength of the processed sintered body, but its rising range is small. It is thus believed that in the manufacture method of Comparative Example 2, the surface layer is not fully formed.

[0141] The entire contents of the specification, claims, drawings, and abstract of Japanese Patent Application No. 2022-049235 filed on March 25, 2022 are cited herein and incorporated as a disclosure of the specification of the present disclosure.

Claims

1. A sintered body of gallium nitride, comprising a surface layer having a higher density than the interior of the sintered body, wherein the atomic weight ratio of gallium to the sum of gallium and nitrogen is more than 0.5 and not more than 0.

60.

2. The sintered body according to claim 1, wherein the oxygen content is 0.3 atm % or less.

3. The sintered body according to claim 1 or 2, wherein the measured density is 3.80 g / cm 3 Above and 5.50g / cm 3 the following. The sintered body according to any one of claims 1 to 3, comprising metal gallium.

5. A method for producing a sintered body according to any one of claims 1 to 4, comprising the following steps: The nitrogen-containing compound gas is reacted with the bulk of gallium nitride at a reaction temperature of 1025° C. or less in an atmosphere where the nitrogen-containing compound gas flows at a flow rate of 0.5 L / min or more.

6. The manufacturing method according to claim 5, wherein: The block is a pre-sintered body of gallium nitride.

7. The manufacturing method according to claim 6, wherein: The pre-sintered body is a sintered body of gallium nitride obtained by hot pressing.

8. The manufacturing method according to claim 5, wherein: The block is a shaped body of gallium nitride.

9. The production method according to any one of claims 5 to 8, wherein The bulk comprises metallic gallium at least on the surface.

10. The production method according to any one of claims 5 to 9, wherein The nitrogen-containing compound gas is one or more gases selected from the group consisting of ammonia, hydrazine, and alkylamines. 11 . A sputtering target comprising the sintered body according to claim 1 .

Citation Information

Patent Citations

  • Gallium nitride sintered article of gallium nitride molded article and method for producing these articles

    CN103270000A

  • Gallium Nitride-Based Sintered Compact And Method For Manufacturing Same

    CN107429383A

  • Method for preparing GaN substrate material

    CN107587190A

  • Gallium nitride-based sintered body and method for manufacturing same

    CN112805263A

  • Gallium nitride-based sintered body and method for manufacturing same

    EP3865466A1