Triazole compound, synthesis method of triazole compound, coupling agent and application of triazole compound and coupling agent
By introducing specific linking groups into the triazole compound to connect two triazole rings, the problem of insufficient adhesion in the prior art is solved, and high adhesion to electrical and electronic materials is achieved, and suitable for miniaturization and thinning. and speed up demand.
Patent Information
- Application Number
- CN202380030621.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-29
- Filing Date
- 2023-03-24
- Publication Date
- 2024-11-08
AI Technical Summary
In the fields of electrical and electronic materials, existing triazole compounds are difficult to meet the requirements of miniaturization, thinning, precision and high-speed, and their adhesion is insufficient.
A novel triazole compound with two triazole rings was developed, connecting these triazole rings through specific linking groups, improving the interaction ability with metals, resin materials, etc., and using the coupling agent prepared by the compound To enhance adhesion between different materials.
The adhesion between metal and inorganic materials, metal and resin materials and inorganic materials and resin materials is significantly improved, and the compound is not easily decomposed by heat and alkali, and maintains stability.
Smart Images

Figure CN118922427A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a novel triazole compound, a synthesis method of the triazole compound, a coupling agent and uses thereof. Background Art
[0002] Conventionally, coupling agents have been used to combine materials with different properties, such as organic materials and inorganic materials, and have been used in the fields of electronic materials, coatings, primers, adhesives, etc. Therefore, coupling agents are indispensable chemical reagents in the development and production of composite materials.
[0003] For example, a coupling agent (silane coupling agent) using a compound composed of an organic substance and silicon is known. The silane coupling agent functions as a mediator for connecting an organic material and an inorganic material that are generally not compatible.
[0004] In addition, since triazole compounds have the function of preventing metals from rusting and the function of curing epoxy resins and polyurethane resins, various coupling agents using triazole compounds have been proposed.
[0005] As a triazole compound that can be used as a coupling agent, for example, Patent Document 1 proposes a triazole silane compound obtained by introducing an alkoxysilyl group into a specific triazole ring. In addition, Patent Document 2 proposes a triazole silane compound having two specific triazole rings and a disulfide bond (-SS-) and having -CO-NH-(CH2) introduced into the triazole ring. m -Si(OR)3 triazole silane compound.
[0006] Prior art literature
[0007] Patent Literature
[0008] [Patent Document 1] International Publication No. 2018 / 186476
[0009] [Patent Document 2] International Publication No. 2015 / 002158 Summary of the invention
[0010] Problems to be solved by the invention
[0011] In recent years, in the field of electrical and electronic materials, there is a demand for improved adhesion between materials in order to cope with miniaturization, thinning, precision, high-speed transmission, etc. Triazole compounds such as those disclosed in Patent Documents 1 and 2 can also exhibit excellent adhesion, but compounds that can exhibit higher adhesion are required.
[0012] The present invention is accomplished in view of the above-mentioned problems, and the problem is to provide a novel triazole compound and a synthesis method thereof, and a coupling agent.
[0013] Means for solving problems
[0014] The present inventors have conducted intensive studies to solve the above problems and have found that in a triazole compound having two triazole rings, the above problems can be solved by linking these triazole rings with a specific linking group, thereby completing the present invention.
[0015] That is, the present invention is as described in the following [1] to
[20] .
[0016] [1] A triazole compound represented by the following chemical formula (I).
[0017]
[0018] (In formula (I),
[0019] R1 and R2 are the same or different and represent a hydrogen atom, a linear or branched alkyl group having 1 to 6 carbon atoms, an aryl group, an aralkyl group, an amino group, a hydroxyl group, or an alkylthio group having 1 to 6 carbon atoms.
[0020] R3 and R4 are the same or different and represent a hydrogen atom or -(CH2) m -A group represented by -Si(OR)3, wherein R represents a methyl group or an ethyl group, and m represents an integer of 1 to 18, except when both R3 and R4 are hydrogen atoms.
[0021] X represents phenylene, -NH- or -(CH2) n -, wherein n represents an integer of 0 to 12.
[0022] [2] The method for synthesizing a triazole compound according to [1], wherein a triazole compound represented by the following chemical formula (II) is reacted with a compound represented by the following chemical formula (III).
[0023]
[0024] (In formula (II), R1, R2 and X are the same as above.)
[0025]
[0026] (In formula (III), R and m are the same as above. Hal represents a chlorine atom, a bromine atom or an iodine atom.)
[0027] [3] A coupling agent comprising a triazole compound represented by the following chemical formula (IV) as a component.
[0028]
[0029] (In formula (IV),
[0030] R1 and R2 are the same or different and represent a hydrogen atom, a linear or branched alkyl group having 1 to 6 carbon atoms, an aryl group, an aralkyl group, an amino group, a hydroxyl group, or an alkylthio group having 1 to 6 carbon atoms.
[0031] R5 and R6 are the same or different and represent a hydrogen atom or -(CH2) m -Si(OR) 3-p (OH) p Here, R represents a methyl group or an ethyl group, m represents an integer of 1 to 18, and p represents an integer of 0 to 3.
[0032] X represents phenylene, -NH- or -(CH2) n -, wherein n represents an integer of 0 to 12.
[0033] [4] A surface treatment liquid comprising a triazole compound represented by the following chemical formula (IV).
[0034]
[0035] (In formula (IV),
[0036] R1 and R2 are the same or different and represent a hydrogen atom, a linear or branched alkyl group having 1 to 6 carbon atoms, an aryl group, an aralkyl group, an amino group, a hydroxyl group, or an alkylthio group having 1 to 6 carbon atoms.
[0037] R5 and R6 are the same or different and represent a hydrogen atom or -(CH2) m -Si(OR) 3-p (OH) p Here, R represents a methyl group or an ethyl group, m represents an integer of 1 to 18, and p represents an integer of 0 to 3.
[0038] X represents phenylene, -NH- or -(CH2) n -, wherein n represents an integer of 0 to 12.
[0039] [5] The surface treatment liquid according to [4], wherein the surface treatment liquid is used to treat the surface of at least one selected from the group consisting of metals, inorganic materials, and resin materials.
[0040] [6] The surface treatment liquid according to [4], wherein the surface treatment liquid is used to bond two materials selected from the group consisting of metals, inorganic materials and resin materials.
[0041] [7] The surface treatment liquid described in [5] or [6], wherein the metal is at least one selected from the group consisting of copper, aluminum, titanium, nickel, tin, iron, silver, gold, and alloys thereof.
[0042] [8] A surface treatment method, comprising bringing the surface treatment liquid according to [4] into contact with the surface of at least one selected from the group consisting of metals, inorganic materials and resin materials.
[0043] [9] The surface treatment method according to [8], wherein the metal is at least one selected from the group consisting of copper, aluminum, titanium, nickel, tin, iron, silver, gold, and alloys thereof.
[0044]
[10] The surface treatment method described in [9], wherein the metal is copper or a copper alloy.
[0045]
[11] The surface treatment method described in
[10] , wherein an aqueous solution containing copper ions is brought into contact with the surface of the copper or copper alloy before the surface treatment liquid is brought into contact with the surface of the copper or copper alloy.
[0046]
[12] The surface treatment method described in
[10] or
[11] , wherein after the surface treatment liquid is brought into contact with the surface of the copper or copper alloy, an acidic aqueous solution or an alkaline aqueous solution is brought into contact with the surface of the copper or copper alloy.
[0047]
[13] A bonding method, wherein the surface treatment liquid described in [4] is brought into contact with at least one selected from the group consisting of metals, inorganic materials and resin materials, thereby forming a conversion film on the at least one, and bonding is performed through the conversion film.
[0048]
[14] A method for bonding metal to a resin material, wherein the surface treatment liquid described in [4] is brought into contact with at least one of the metal and the resin material to form a conversion film on the at least one, and the metal and the resin material are bonded to each other via the conversion film.
[0049]
[15] A printed wiring board obtained by bonding two materials selected from the group consisting of metals, inorganic materials and resin materials via a conversion film formed from the surface treatment liquid according to [4].
[0050]
[16] A semiconductor wafer obtained by bonding two materials selected from the group consisting of metals, inorganic materials and resin materials via a conversion film formed using the surface treatment solution according to [4].
[0051]
[17] An insulating composition comprising the coupling agent according to [3] and a resin material or an inorganic material.
[0052]
[18] An insulating material comprising the insulating composition according to
[17] .
[0053]
[19] A printed wiring board having an insulating layer obtained from the insulating composition according to
[17] .
[0054]
[20] A semiconductor wafer having an insulating layer obtained from the insulating composition according to
[17] .
[0055] Effects of the Invention
[0056] The triazole compound of the present invention is a compound combining two triazole rings, and thus can enhance the interaction with metals, resin materials, etc., and further, by utilizing a group selected from among phenylene, -NH- and -(CH2) n The linking group in the group consisting of the group represented by - binds two triazole rings and is therefore not easily decomposed by heat or alkali.
[0057] In addition, the coupling agent of the present invention uses a triazole compound obtained by connecting two triazole rings using the connecting group as a component, so it can improve the adhesion between materials with different properties. According to the surface treatment liquid containing the triazole compound, the adhesion between two materials with different materials, that is, metal and inorganic material, metal and resin material, and inorganic material and resin material can be improved. DETAILED DESCRIPTION
[0058] Hereinafter, the present invention will be described in detail. However, it should be noted that the present invention is not limited to the embodiments described below.
[0059] (Triazole compound)
[0060] The triazole compound of the present invention is represented by the following chemical formula (I) (hereinafter, sometimes referred to as triazole compound (I)).
[0061]
[0062] (In formula (I),
[0063] R1 and R2 are the same or different and represent a hydrogen atom, a linear or branched alkyl group having 1 to 6 carbon atoms, an aryl group, an aralkyl group, an amino group, a hydroxyl group, or an alkylthio group having 1 to 6 carbon atoms.
[0064] R3 and R4 are the same or different and represent a hydrogen atom or -(CH2) m -A group represented by -Si(OR)3, wherein R represents a methyl group or an ethyl group, and m represents an integer of 1 to 18, except when both R3 and R4 are hydrogen atoms.
[0065] X represents phenylene, -NH- or -(CH2) n -, wherein n represents an integer of 0 to 12.
[0066] In formula (I), R1 and R2 are hydrogen atoms, linear or branched alkyl groups having 1 to 6 carbon atoms, aryl groups, aralkyl groups, amino groups, hydroxyl groups, or alkylthio groups having 1 to 6 carbon atoms. R1 and R2 may be the same or different.
[0067] As the linear alkyl group having 1 to 6 carbon atoms, specifically, methyl, ethyl, n-propyl, n-butyl, n-pentyl, n-hexyl, etc. can be mentioned. As the branched alkyl group having 1 to 6 carbon atoms, it is a branched alkyl group having 3 to 6 carbon atoms, specifically, isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, sec-pentyl, tert-pentyl, isohexyl, sec-hexyl, tert-hexyl, etc. can be mentioned. As the aryl group, specifically, phenyl, o-tolyl, m-tolyl, p-tolyl, xylyl, trimethylphenyl, tetramethylphenyl, 1-naphthyl, 2-naphthyl, etc. can be mentioned. As the aralkyl group, specifically, benzyl, phenylethyl, phenylpropyl, methylbenzyl, etc. can be mentioned. Specific examples of the alkylthio group having 1 to 6 carbon atoms include methylthio, ethylthio, propylthio, isopropylthio, butylthio, isobutylthio, sec-butylthio, tert-butylthio, pentylthio, and hexylthio.
[0068] R1 and R2 are the same or different, and are more preferably a hydrogen atom, an amino group, or an alkylthio group having 1 to 6 carbon atoms.
[0069] R3 and R4 are hydrogen atoms or -(CH2) m -Si(OR)3 (R represents a methyl group or an ethyl group, and m represents an integer from 1 to 18). R3 and R4 may be the same or different, and R3 and R4 may not be hydrogen atoms at the same time.
[0070] For -(CH2) m In the group represented by -Si(OR)3, m is preferably an integer of 2 to 12, more preferably m is an integer of 3 to 10, and further preferably m is an integer of 3 to 8.
[0071] X represents phenylene, -NH- or -(CH2) n -(n is an integer of 0 to 12).
[0072] X is preferably -(CH2) n -, wherein n is more preferably an integer of 0 to 10, further preferably an integer of 0 to 8, and particularly preferably an integer of 0 to 6.
[0073] In the compound represented by the chemical formula (I) (triazole compound (I)), R3 and R4 are preferably bonded to the N atom at the 1-position or 2-position of the triazole ring.
[0074] Examples of the triazole compound (I) include triazole compounds represented by Chemical Formula (I-1) to Chemical Formula (I-8).
[0075]
[0076] (In formulas (I-1) to (I-8), R1, R2, m, R and X are the same as above.)
[0077] Specific examples of the triazole compound (I) in which R3 is hydrogen and R4 is bonded to the nitrogen at the 1-position of the triazole ring (compounds represented by formula (I-3)) include:
[0078] 1-(Trimethoxysilyl)methyl-3,3'-(1,4-phenylene)bis(1,2,4-triazole),
[0079] 1-[2-(Triethoxysilyl)ethyl]-3,3'-(1,2-phenylene)bis(5-methyl-1,2,4-triazole),
[0080] 1-[3-(Triethoxysilyl)propyl]-3,3'-(1,3-phenylene)bis(5-butyl-1,2,4-triazole),
[0081] 1-[3-(Triethoxysilyl)propyl]-3,3'-(1,4-phenylene)bis(5-amino-1,2,4-triazole),
[0082] 1-[6-(triethoxysilyl)hexyl]-3,3'-(1,4-phenylene)bis(5-ethylthio-1,2,4-triazole),
[0083] 1-[3-(Triethoxysilyl)propyl]-3,3'-iminobis(5-ethyl-1,2,4-triazole),
[0084] 1-[3-(Triethoxysilyl)propyl]-3,3'-iminobis(5-p-tolyl-1,2,4-triazole),
[0085] 1-[3-(Triethoxysilyl)propyl]-3,3'-iminobis(5-amino-1,2,4-triazole),
[0086] 1-[8-(Trimethoxysilyl)octyl]-3,3'-iminobis(5-isopropyl-1,2,4-triazole),
[0087] 1-[3-(Triethoxysilyl)propyl]-3,3'-bis(5-methyl-1,2,4-triazole),
[0088] 1-[3-(Triethoxysilyl)propyl]-3,3'-bis(5-pentyl-1,2,4-triazole),
[0089] 1-[3-(Triethoxysilyl)propyl]-3,3'-bis(5-amino-1,2,4-triazole),
[0090] 1-[10-(triethoxysilyl)decyl]-3,3'-bis(5-phenyl-1,2,4-triazole),
[0091] 1-[3-(Triethoxysilyl)propyl]-5-amino-5'-methyl-3,3'-bis-1,2,4-triazole,
[0092] 1-[3-(Triethoxysilyl)propyl]-3,3'-methylenebis(5-isobutyl-1,2,4-triazole),
[0093] 1-[3-(Triethoxysilyl)propyl]-3,3'-methylenebis(5-hydroxy-1,2,4-triazole),
[0094] 1-[3-(Triethoxysilyl)propyl]-3,3'-methylenebis(5-amino-1,2,4-triazole),
[0095] 1-[6-(Trimethoxysilyl)hexyl]-3,3'-methylenebis(5-amino-1,2,4-triazole),
[0096] 1-[3-(Triethoxysilyl)propyl]-3,3'-ethylenebis(5-ethyl-1,2,4-triazole),
[0097] 1-[3-(Triethoxysilyl)propyl]-3,3'-ethylenebis(5-amino-1,2,4-triazole),
[0098] 1-[12-(triethoxysilyl)dodecyl]-3,3'-ethylenebis(5-amino-1,2,4-triazole),
[0099] 1-[3-(Triethoxysilyl)propyl]-3,3'-tetramethylenebis(5-benzyl-1,2,4-triazole),
[0100] 1-[3-(Triethoxysilyl)propyl]-3,3'-tetramethylenebis(5-butylthio-1,2,4-triazole),
[0101] 1-[3-(Triethoxysilyl)propyl]-3,3'-tetramethylenebis(5-amino-1,2,4-triazole),
[0102] 1-[3-(Triethoxysilyl)propyl]-3,3'-pentamethylenebis(1,2,4-triazole),
[0103] 1-[3-(Triethoxysilyl)propyl]-3,3'-pentamethylenebis(5-amino-1,2,4-triazole),
[0104] 1-[4-(Triethoxysilyl)butyl]-3,3'-pentamethylenebis(5-amino-1,2,4-triazole),
[0105] 1-[3-(Triethoxysilyl)propyl]-3,3'-hexamethylenebis(5-amino-1,2,4-triazole),
[0106] 1-[3-(Triethoxysilyl)propyl]-3,3'-octamethylenebis(5-amino-1,2,4-triazole),
[0107] 1-[2-(Trimethoxysilyl)ethyl]-3,3'-nonamethylenebis(5-amino-1,2,4-triazole),
[0108] 1-[2-(Trimethoxysilyl)ethyl]-3,3'-decamethylenebis(5-amino-1,2,4-triazole),
[0109] 1-[3-(Triethoxysilyl)propyl]-3,3'-undecamethylenebis(5-amino-1,2,4-triazole),
[0110] 1-[3-(Triethoxysilyl)propyl]-3,3'-dodecamethylenebis(5-amino-1,2,4-triazole), and the like.
[0111] As the triazole compound (I), R3 and R4 are the same or different from -(CH2) m Specific examples of the case where the group is represented by -Si(OR)3 and R3 and R4 are bonded to the nitrogen at the 1-position of the triazole ring (compound represented by formula (I-5)) include:
[0112] 3,3'-(1,4-phenylene)bis[1-(trimethoxysilyl)methyl-1,2,4-triazole],
[0113] 3,3'-(1,2-phenylene)bis{1-[2-(triethoxysilyl)ethyl]-5-methyl-1,2,4-triazole},
[0114] 3,3'-(1,3-phenylene)bis{1-[3-(triethoxysilyl)propyl]-5-butyl-1,2,4-triazole},
[0115] 3,3'-(1,4-phenylene)bis{1-[3-(triethoxysilyl)propyl]-5-amino-1,2,4-triazole},
[0116] 3,3'-(1,4-phenylene)bis{1-[6-(triethoxysilyl)hexyl]-5-ethylthio-1,2,4-triazole},
[0117] 3,3'-Iminobis{1-[3-(triethoxysilyl)propyl]-5-ethyl-1,2,4-triazole},
[0118] 3,3'-Iminobis{1-[3-(triethoxysilyl)propyl]-5-p-tolyl-1,2,4-triazole},
[0119] 3,3'-Iminobis{1-[3-(triethoxysilyl)propyl]-5-amino-1,2,4-triazole},
[0120] 3,3'-Iminobis{1-[8-(trimethoxysilyl)octyl]-5-isopropyl-1,2,4-triazole},
[0121] 3,3'-bis{1-[3-(triethoxysilyl)propyl]-5-pentyl-1,2,4-triazole},
[0122] 3,3'-bis{1-[3-(triethoxysilyl)propyl]-5-amino-1,2,4-triazole},
[0123] 3,3'-bis{1-[10-(triethoxysilyl)decyl]-5-phenyl-1,2,4-triazole},
[0124] 1,1'-bis[3-(triethoxysilyl)propyl]-5-amino-5'-methyl-3,3'-bis-1,2,4-triazole,
[0125] 3,3'-methylenebis{1-[3-(triethoxysilyl)propyl]-5-isobutyl-1,2,4-triazole},
[0126] 3,3'-methylenebis{1-[3-(triethoxysilyl)propyl]-5-hydroxy-1,2,4-triazole},
[0127] 3,3'-methylenebis{1-[3-(triethoxysilyl)propyl]-5-amino-1,2,4-triazole},
[0128] 3,3'-methylenebis{1-[6-(trimethoxysilyl)hexyl]-5-amino-1,2,4-triazole},
[0129] 3,3'-ethylenebis{1-[3-(triethoxysilyl)propyl]-5-ethyl-1,2,4-triazole},
[0130] 3,3'-ethylenebis{1-[3-(triethoxysilyl)propyl]-5-amino-1,2,4-triazole},
[0131] 3,3'-ethylenebis{1-[12-(triethoxysilyl)dodecyl]-5-amino-1,2,4-triazole},
[0132] 3,3'-Tetramethylenebis{1-[3-(triethoxysilyl)propyl]-5-benzyl-1,2,4-triazole},
[0133] 3,3'-Tetramethylenebis{1-[3-(triethoxysilyl)propyl]-5-butylthio-1,2,4-triazole},
[0134] 3,3'-Tetramethylenebis{1-[3-(triethoxysilyl)propyl]-5-amino-1,2,4-triazole},
[0135] 3,3'-pentamethylenebis{1-[3-(triethoxysilyl)propyl]-1,2,4-triazole},
[0136] 3,3'-pentamethylenebis{1-[3-(triethoxysilyl)propyl]-5-amino-1,2,4-triazole},
[0137] 3,3'-pentamethylenebis{1-[4-(triethoxysilyl)butyl]-5-amino-1,2,4-triazole},
[0138] 3,3'-hexamethylenebis{1-[3-(triethoxysilyl)propyl]-5-amino-1,2,4-triazole},
[0139] 3,3'-octamethylenebis{1-[3-(triethoxysilyl)propyl]-5-amino-1,2,4-triazole},
[0140] 3,3'-nonamethylenebis{1-[2-(trimethoxysilyl)ethyl]-5-amino-1,2,4-triazole},
[0141] 3,3'-decamethylenebis{1-[2-(trimethoxysilyl)ethyl]-5-amino-1,2,4-triazole},
[0142] 3,3'-undecamethylenebis{1-[3-(triethoxysilyl)propyl]-5-amino-1,2,4-triazole},
[0143] 3,3'-dodecamethylenebis{1-[3-(triethoxysilyl)propyl]-5-amino-1,2,4-triazole}, and the like.
[0144] The triazole compound (I) can be obtained by reacting a triazole compound represented by the chemical formula (II) (hereinafter, sometimes referred to as the triazole compound (II)) with a haloalkylsilane compound represented by the chemical formula (III) (hereinafter, sometimes referred to as the haloalkylsilane compound (III)).
[0145]
[0146] (In formula (II), R1, R2 and X are the same as above.)
[0147]
[0148] (In formula (III), R and m are the same as above. Hal represents a chlorine atom, a bromine atom or an iodine atom.)
[0149] In the formula (II), R1, R2 and X are the same as those shown in the formula (I), and preferred groups are also the same.
[0150] In the formula (III), R and m are the same as those shown in the formula (I), and preferred groups are also the same.
[0151] Hal in the formula (III) is a chlorine atom, a bromine atom or an iodine atom, and is preferably a chlorine atom or a bromine atom from the viewpoint of reactivity and availability of raw materials.
[0152] Examples of the triazole compound (II) include:
[0153] 3,3'-(1,4-phenylene)bis(1,2,4-triazole),
[0154] 3,3'-(1,4-phenylene)bis(5-methyl-1,2,4-triazole),
[0155] 3,3'-(1,2-phenylene)bis(5-ethyl-1,2,4-triazole),
[0156] 3,3'-(1,4-phenylene)bis(5-isopropyl-1,2,4-triazole),
[0157] 3,3'-(1,3-phenylene)bis(5-butyl-1,2,4-triazole),
[0158] 3,3'-(1,4-phenylene)bis(5-phenyl-1,2,4-triazole),
[0159] 3,3'-(1,4-phenylene)bis(5-amino-1,2,4-triazole),
[0160] 3,3'-(1,4-phenylene)bis(5-hydroxy-1,2,4-triazole),
[0161] 3,3'-(1,4-phenylene)bis(5-ethylthio-1,2,4-triazole),
[0162] 5-amino-3,3'-(1,4-phenylene)bis(1,2,4-triazole),
[0163] 3,3'-Iminobis(1,2,4-triazole),
[0164] 3,3'-Iminobis(5-methyl-1,2,4-triazole),
[0165] 3,3'-Iminobis(5-hexyl-1,2,4-triazole),
[0166] 3,3'-Iminobis(5-phenyl-1,2,4-triazole),
[0167] 3,3'-Iminobis(5-benzyl-1,2,4-triazole),
[0168] 3,3'-Iminobis(5-amino-1,2,4-triazole),
[0169] 3,3'-Iminobis(5-hydroxy-1,2,4-triazole),
[0170] 3,3'-Iminobis(5-methylthio-1,2,4-triazole),
[0171] 5-amino-3,3'-iminobis(1,2,4-triazole),
[0172] 3,3'-Bis-1,2,4-triazole,
[0173] 3,3'-bis(5-methyl-1,2,4-triazole),
[0174] 3,3'-Bis(5-ethyl-1,2,4-triazole),
[0175] 3,3'-Bis(5-pentyl-1,2,4-triazole),
[0176] 3,3'-Bis(5-p-tolyl-1,2,4-triazole),
[0177] 3,3'-bis(5-benzyl-1,2,4-triazole),
[0178] 3,3'-bis(5-amino-1,2,4-triazole),
[0179] 3,3'-bis(5-hydroxy-1,2,4-triazole),
[0180] 3,3'-bis(5-hexylthio-1,2,4-triazole),
[0181] 5-amino-5'-methyl-3,3'-bis-1,2,4-triazole,
[0182] 3,3'-Methylenebis(1,2,4-triazole),
[0183] 3,3'-Methylenebis(5-methyl-1,2,4-triazole),
[0184] 3,3'-Methylenebis(5-isobutyl-1,2,4-triazole),
[0185] 3,3'-Methylenebis(5-phenyl-1,2,4-triazole),
[0186] 3,3'-Methylenebis(5-phenylethyl-1,2,4-triazole),
[0187] 3,3'-Methylenebis(5-amino-1,2,4-triazole),
[0188] 3,3'-Methylenebis(5-hydroxy-1,2,4-triazole),
[0189] 3,3'-Methylenebis(5-methylthio-1,2,4-triazole),
[0190] 5-amino-5'-ethyl-3,3'-methylenebis(1,2,4-triazole),
[0191] 3,3'-ethylenebis(1,2,4-triazole),
[0192] 3,3'-ethylenebis(5-propyl-1,2,4-triazole),
[0193] 3,3'-ethylenebis(5-hexyl-1,2,4-triazole),
[0194] 3,3'-ethylenebis(5-m-tolyl-1,2,4-triazole),
[0195] 3,3'-ethylenebis(5-amino-1,2,4-triazole),
[0196] 3,3'-ethylenebis(5-hydroxy-1,2,4-triazole),
[0197] 3,3'-ethylenebis(5-isopropylthio-1,2,4-triazole),
[0198] 5-amino-3,3'-ethylenebis(1,2,4-triazole),
[0199] 3,3'-trimethylenebis(1,2,4-triazole),
[0200] 5-methyl-3,3'-trimethylenebis(1,2,4-triazole),
[0201] 3,3'-trimethylenebis(5-butyl-1,2,4-triazole),
[0202] 3,3'-trimethylenebis(5-phenyl-1,2,4-triazole),
[0203] 3,3'-trimethylenebis(5-amino-1,2,4-triazole),
[0204] 3,3'-trimethylenebis(5-propylthio-1,2,4-triazole),
[0205] 5-amino-5'-benzyl-3,3'-trimethylenebis(1,2,4-triazole),
[0206] 3,3'-Tetramethylenebis(1,2,4-triazole),
[0207] 3,3'-Tetramethylenebis(5-ethyl-1,2,4-triazole),
[0208] 3,3'-Tetramethylenebis(5-hexyl-1,2,4-triazole),
[0209] 3,3'-Tetramethylenebis(5-benzyl-1,2,4-triazole),
[0210] 3,3'-Tetramethylenebis(5-amino-1,2,4-triazole),
[0211] 3,3'-Tetramethylenebis(5-hydroxy-1,2,4-triazole),
[0212] 3,3'-Tetramethylenebis(5-butylthio-1,2,4-triazole),
[0213] 5-amino-3,3'-tetramethylenebis(1,2,4-triazole),
[0214] 3,3'-pentamethylenebis(1,2,4-triazole),
[0215] 3,3'-pentamethylenebis(5-propyl-1,2,4-triazole),
[0216] 3,3'-pentamethylenebis(5-amino-1,2,4-triazole),
[0217] 3,3'-pentamethylenebis(5-hydroxy-1,2,4-triazole),
[0218] 3,3'-pentamethylenebis(5-pentylthio-1,2,4-triazole),
[0219] 5-amino-5'-phenyl-3,3'-pentamethylenebis(1,2,4-triazole),
[0220] 3,3'-hexamethylenebis(1,2,4-triazole),
[0221] 3,3'-hexamethylenebis(5-pentyl-1,2,4-triazole),
[0222] 3,3'-hexamethylenebis(5-amino-1,2,4-triazole),
[0223] 5-Hydroxy-3,3'-hexamethylenebis(1,2,4-triazole),
[0224] 5-phenyl-3,3'-hexamethylenebis(1,2,4-triazole),
[0225] 5-amino-5'-methylthio-3,3'-hexamethylenebis(1,2,4-triazole),
[0226] 3,3'-heptamethylenebis(1,2,4-triazole),
[0227] 3,3'-heptamethylenebis(5-tert-butyl-1,2,4-triazole),
[0228] 3,3'-heptamethylenebis(5-phenyl-1,2,4-triazole),
[0229] 3,3'-heptamethylenebis(5-amino-1,2,4-triazole),
[0230] 5-amino-5'-hydroxy-3,3'-heptamethylenebis(1,2,4-triazole),
[0231] 3,3'-octamethylenebis(1,2,4-triazole),
[0232] 3,3'-octamethylenebis(5-isobutyl-1,2,4-triazole),
[0233] 3,3'-octamethylenebis(5-amino-1,2,4-triazole),
[0234] 3,3'-octamethylenebis(5-hydroxy-1,2,4-triazole),
[0235] 5-propylthio-3,3'-octamethylenebis(1,2,4-triazole),
[0236] 3,3'-nonamethylenebis(1,2,4-triazole),
[0237] 3,3'-nonamethylenebis(5-isopentyl-1,2,4-triazole),
[0238] 5-phenyl-3,3'-nonamethylenebis(1,2,4-triazole),
[0239] 3,3'-nonamethylenebis(5-amino-1,2,4-triazole),
[0240] 3,3'-nonamethylenebis(5-methylthio-1,2,4-triazole),
[0241] 3,3'-decamethylenebis(1,2,4-triazole),
[0242] 3,3'-decamethylenebis(5-methyl-1,2,4-triazole),
[0243] 3,3'-decamethylenebis(5-amino-1,2,4-triazole),
[0244] 5-ethyl-3,3'-decamethylenebis(1,2,4-triazole),
[0245] 3,3'-undecamethylenebis(1,2,4-triazole),
[0246] 3,3'-undecamethylenebis(5-propyl-1,2,4-triazole),
[0247] 3,3'-undecamethylenebis(5-amino-1,2,4-triazole),
[0248] 3,3'-undecamethylenebis(5-methylthio-1,2,4-triazole),
[0249] 3,3'-dodecamethylenebis(1,2,4-triazole),
[0250] 3,3'-dodecamethylenebis(5-ethyl-1,2,4-triazole),
[0251] 3,3'-dodecamethylenebis(5-amino-1,2,4-triazole),
[0252] 3,3'-undecamethylenebis(5-hydroxy-1,2,4-triazole), etc.
[0253] These exemplified triazole compounds (II) can be synthesized according to the synthesis methods described in, for example, Chem. Eur. J., 18, 16742 (2012), J. Applied. Chem., 82, 276 (2009), and U.S. Patent No. 2,744,116.
[0254] Examples of the haloalkylsilane compound (III) include:
[0255] Chloromethyltrimethoxysilane,
[0256] Chloromethyltriethoxysilane,
[0257] 2-Chloroethyltrimethoxysilane,
[0258] 2-Chloroethyltriethoxysilane,
[0259] 3-Chloropropyltrimethoxysilane,
[0260] 3-Chloropropyltriethoxysilane,
[0261] 3-Bromopropyltrimethoxysilane,
[0262] 3-Bromopropyltriethoxysilane,
[0263] 3-iodopropyltrimethoxysilane,
[0264] 3-iodopropyltriethoxysilane,
[0265] 4-Bromobutyltrimethoxysilane,
[0266] 4-Bromobutyltriethoxysilane,
[0267] 5-Bromopentyltrimethoxysilane,
[0268] 5-Bromopentyltriethoxysilane,
[0269] 6-Bromohexyltrimethoxysilane,
[0270] 6-Bromohexyltriethoxysilane,
[0271] 8-Bromooctyltrimethoxysilane,
[0272] 8-Bromooctyltriethoxysilane,
[0273] 10-bromodecyltrimethoxysilane,
[0274] 10-bromodecyltriethoxysilane,
[0275] 12-bromododecyltrimethoxysilane, and
[0276] 12-Bromododecyltriethoxysilane, etc.
[0277] The triazole compound (I) of the present invention can be synthesized in a generally high yield by reacting the triazole compound (II) and the haloalkylsilane compound (III) in the presence of a dehydrohalogenating agent, in an appropriate amount of a reaction solvent, at an appropriate reaction temperature and reaction time. In the following reaction scheme (A), it is shown that R3 is a hydrogen atom and R4 is -(CH2) m Reaction scheme of triazole compound (I) containing a group represented by -Si(OR)3.
[0278]
[0279] (Wherein, R1, R2, X, R, Hal and m are the same as above.)
[0280] The reaction solvent is not particularly limited as long as it is inert to the triazole compound (II) and the haloalkylsilane compound (III), and examples thereof include:
[0281] Hydrocarbon solvents such as hexane, toluene, and xylene;
[0282] Diethyl ether, tetrahydrofuran, Ether solvents such as alkane and cyclopentyl methyl ether;
[0283] Ester solvents such as ethyl acetate and butyl acetate;
[0284] Alcohol solvents such as methanol and ethanol;
[0285] Amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone;
[0286] Ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone;
[0287] Acetonitrile, dimethyl sulfoxide, hexamethylphosphoramide, etc.
[0288] Examples of the dehydrohalogenating agent include:
[0289] Alkali metal alkoxides such as sodium methoxide, sodium ethoxide, potassium methoxide, potassium tert-butoxide;
[0290] Alkali metal carbonates such as sodium carbonate and potassium carbonate;
[0291] Organic bases such as triethylamine, diazabicycloundecene, sodium hydride, etc.
[0292] The reaction of the triazole compound (II) and the haloalkylsilane compound (III) is carried out in stoichiometric manner as shown in the reaction scheme (A). However, the amount of the haloalkylsilane compound (III) used (input amount) relative to the amount of the triazole compound (II) used (input amount) is determined by taking into account factors such as the reaction temperature and reaction time, the types of raw materials and reaction solvent used, the reaction scale, etc. It is preferred to use 0.8 to 1.2 equivalents of the haloalkylsilane compound (III) relative to each -NH of the triazole ring as the reaction site.
[0293] When the amount of the haloalkylsilane compound (III) added per reaction site (-NH) is more than 1.2 equivalents, the compound may polymerize and gel. When the amount of the haloalkylsilane compound (III) added per reaction site (-NH) is less than 0.8 equivalents, there is a risk that the purity of the product decreases or the separation operation of the product becomes complicated.
[0294] The dehydrohalogenating agent is used to neutralize the hydrogen halide by-produced by the reaction between the triazole compound (II) and the haloalkylsilane compound (III). Therefore, the amount used (input amount) may be equimolar or more relative to the amount of the haloalkylsilane compound (III).
[0295] The reaction temperature is not particularly limited as long as it is a temperature range at which -NH of the triazole ring of the triazole compound (II) reacts with the haloalkylsilane compound (III), but is preferably in the range of 0°C to 150°C, more preferably in the range of 5°C to 100°C.
[0296] The reaction time is appropriately determined depending on the set reaction temperature, and is preferably in the range of 30 minutes to 24 hours, and more preferably in the range of 1 hour to 8 hours.
[0297] (Coupling agent)
[0298] The coupling agent of the present invention contains a triazole compound represented by the following chemical formula (IV) (hereinafter, sometimes referred to as triazole compound (IV)) as a component.
[0299]
[0300] (In formula (IV),
[0301] R1 and R2 are the same or different and represent a hydrogen atom, a linear or branched alkyl group having 1 to 6 carbon atoms, an aryl group, an aralkyl group, an amino group, a hydroxyl group, or an alkylthio group having 1 to 6 carbon atoms.
[0302] R5 and R6 are the same or different and represent a hydrogen atom or -(CH2) m -Si(OR) 3-p (OH) p Here, R represents a methyl group or an ethyl group, m represents an integer of 1 to 18, and p represents an integer of 0 to 3.
[0303] X represents phenylene, -NH- or -(CH2) n -, wherein n represents an integer of 0 to 12.
[0304] In formula (IV), R1 and R2 are hydrogen atoms, linear or branched alkyl groups having 1 to 6 carbon atoms, aryl groups, aralkyl groups, amino groups, hydroxyl groups, or alkylthio groups having 1 to 6 carbon atoms. R1 and R2 may be the same or different.
[0305] As the linear alkyl group having 1 to 6 carbon atoms, specifically, methyl, ethyl, n-propyl, n-butyl, n-pentyl, n-hexyl, etc. can be mentioned. As the branched alkyl group having 1 to 6 carbon atoms, it is a branched alkyl group having 3 to 6 carbon atoms, specifically, isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, sec-pentyl, tert-pentyl, isohexyl, sec-hexyl, tert-hexyl, etc. can be mentioned. As the aryl group, specifically, phenyl, o-tolyl, m-tolyl, p-tolyl, xylyl, trimethylphenyl, tetramethylphenyl, 1-naphthyl, 2-naphthyl, etc. can be mentioned. As the aralkyl group, specifically, benzyl, phenylethyl, phenylpropyl, methylbenzyl, etc. can be mentioned. Specific examples of the alkylthio group having 1 to 6 carbon atoms include methylthio, ethylthio, propylthio, isopropylthio, butylthio, isobutylthio, sec-butylthio, tert-butylthio, pentylthio, and hexylthio.
[0306] R1 and R2 are the same or different, and are more preferably a hydrogen atom, an amino group, or an alkylthio group having 1 to 6 carbon atoms.
[0307] R5 and R6 are hydrogen atoms or -(CH2) m -Si(OR) 3-p (OH) p (R is a methyl group or an ethyl group, m is an integer from 1 to 18, and p is an integer from 0 to 3). R5 and R6 may be the same or different.
[0308] At least one of R5 and R6 is preferably -(CH2) m -Si(OR) 3-p (OH) p Represents the group.
[0309] In addition, for -(CH2) m -Si(OR) 3-p (OH) p In the group represented by , m is preferably an integer of 2 to 12, more preferably m is an integer of 3 to 10, and further preferably m is an integer of 3 to 8.
[0310] X represents phenylene, -NH- or -(CH2) n -(n is an integer of 0 to 12).
[0311] X is preferably -(CH2) n-, wherein n is more preferably an integer of 0 to 10, further preferably an integer of 0 to 8, and particularly preferably an integer of 0 to 6.
[0312] The compound represented by the chemical formula (IV) (triazole compound (IV)) includes the triazole compound (I), the hydrolyzate of the triazole compound (I) and the triazole compound (II). In the triazole compound (IV), R5 and / or R6 are -(CH2) m -Si(OR) 3-p (OH) p The compound in which p of the group represented by is an integer of 1 to 3 is a species generated by hydrolyzing the triazole compound (I) in which p is 0. These are all suitable as a component of the coupling agent. In addition, among the triazole compounds (IV), the compound in which p is an integer of 1 to 3 can be obtained by, for example, hydrolyzing the triazole compound (I) in which p is 0 and then removing the volatile components.
[0313] When the coupling agent of the present invention is used, the same surface treatment method as in the case of conventional coupling agents can be employed.
[0314] Examples of the surface treatment method include: (a) a method of spraying a treatment solution obtained by diluting an appropriate amount of a coupling agent with an organic solvent onto a substrate; (b) a method of spraying a treatment solution obtained by diluting the coupling agent with a water-organic solvent onto a substrate; (c) a method of spraying a treatment solution obtained by diluting the coupling agent with water onto a substrate; (d) a method of immersing a substrate in a treatment solution obtained by diluting the coupling agent with an organic solvent; (e) a method of immersing a substrate in a treatment solution obtained by diluting the coupling agent with a water-organic solvent; (f) a method of immersing a substrate in a treatment solution obtained by diluting the coupling agent with water, etc.
[0315] Examples of the organic solvent include:
[0316] Benzene, toluene, xylene, heptane, hexane, cyclohexane, n-octane and other hydrocarbon solvents;
[0317] Halogenated hydrocarbon solvents such as dichloromethane, dichloroethane, carbon tetrachloride, chloroform, chlorobenzene, dichlorobenzene, trichlorobenzene, etc.
[0318] Ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, etc.
[0319] Diethyl ether, tetrahydrofuran, Ether solvents such as alkane, ethylene glycol monomethyl ether (methyl cellosolve), ethylene glycol monoethyl ether (ethyl cellosolve), ethylene glycol monobutyl ether, and diethylene glycol monobutyl ether;
[0320] Methanol, ethanol, 1-propanol, 2-propanol, n-butanol, 2-butanol, tert-butanol, ethylene glycol, diethylene glycol, propylene glycol and other alcohol solvents, etc.
[0321] Examples of the substrate used in the present invention include granular, needle-shaped, fibrous, woven, plate-shaped, foil-shaped, and amorphous substrates made of metals, inorganic materials, and resin materials.
[0322] Examples of the metal include copper, aluminum, titanium, nickel, tin, iron, silver, gold, and alloys thereof. Plates, foils, plated films, and the like made of these metals may be used as the substrate.
[0323] As a specific example of the alloy, as a copper alloy, there is no particular limitation as long as it is an alloy containing copper, for example, alloys of Cu-Ag, Cu-Te, Cu-Mg, Cu-Sn, Cu-Si, Cu-Mn, Cu-Be-Co, Cu-Ti, Cu-Ni-Si, Cu-Zn-Ni, Cu-Cr, Cu-Zr, Cu-Fe, Cu-Al, Cu-Zn, Cu-Co and the like can be listed.
[0324] In addition, examples of other alloys include aluminum alloys (Al-Si alloys), nickel alloys (Ni-Cr alloys), iron alloys (Fe-Ni alloys, stainless steel, steel), and the like.
[0325] Among these metals, copper and copper alloys are preferred.
[0326] Examples of the inorganic material include silicon, ceramics, inorganic materials used as fillers, and glass.
[0327] Specifically, the following can be listed: silicon compounds such as silicon, silicon carbide, silicon dioxide, glass, diatomaceous earth, calcium silicate, talc, glass beads, sericite, activated clay, bentonite, aluminosilicate, and mica; oxides such as aluminum oxide, zinc oxide, iron oxide, magnesium oxide, tin oxide, and titanium oxide; hydroxides such as magnesium hydroxide, aluminum hydroxide, and basic magnesium carbonate; carbonates such as calcium carbonate, zinc carbonate, hydrotalcite, and magnesium carbonate; sulfates such as barium sulfate and gypsum; titanates such as barium titanate; nitrides such as aluminum nitride and silicon nitride; carbon fibers, etc.
[0328] Among these inorganic materials, silicon, ceramics (aluminum oxide, silicon carbide, aluminum nitride, silicon nitride, barium titanate, and the like), and glass are preferred.
[0329] Examples of the resin material include nylon, acrylic resin, epoxy resin, polyphenylene ether, Azole resin, polysiloxane resin, polyimide resin, bismaleimide resin, maleimide resin, cyanate resin, polyphenylene ether resin, polyphenylene ether resin, polybutadiene resin, olefin resin, fluorine-containing resin, polyetherimide resin, polyetheretherketone resin, liquid crystal resin, etc., can also be mixed or modified with each other and combined.
[0330] Among these resin materials, polyphenylene ether resin, polyphenylene ether resin, liquid crystal resin, acrylate resin, epoxy resin, olefin resin, polybenzoic acid resin, Azole resins, polysiloxane resins and polyimide resins.
[0331] By subjecting the substrate to a surface treatment using a treatment liquid containing the coupling agent of the present invention, the lipophilicity of the surface of the substrate is improved, thereby improving the affinity (adhesiveness, adhesion) for resins and the like.
[0332] In order to further exert the effect of this treatment, the surface-treated substrate may be further subjected to a heat treatment.
[0333] (Surface treatment liquid)
[0334] <Surface treatment liquid containing a triazole compound represented by the chemical formula (IV)>
[0335] The surface treatment liquid of the present invention contains the triazole compound represented by the chemical formula (IV) (triazole compound (IV)). In the triazole compound (IV), R5 and / or R6 are -(CH2) m -Si(OR) 3-p (OH) p The compound in which p of the group represented by is an integer of 1 to 3 is a species generated by hydrolysis of the compound in which p is 0 in a surface treatment liquid. These are all suitable as components of the surface treatment liquid. In addition, among the triazole compounds (IV), the compound in which p is an integer of 1 to 3 can be extracted from the surface treatment liquid containing the triazole compound (I) in which p is 0 and used, for example, by removing the volatile components.
[0336] In the practice of the present invention, as a raw material for preparing the surface treatment liquid, it is preferred to use a compound in which p is 0. In the case where p is 0, that is, at least one of R5 and R6 is -(CH2) m In the case of the group represented by -Si(OR)3, the same compounds as those of the above-mentioned triazole compound (I) may be used, and preferred compounds are also the same.
[0337] The surface treatment liquid of the present invention is prepared by mixing the triazole compound (IV) and water.
[0338] As water used for preparing the surface treatment liquid, pure water such as ion-exchanged water and distilled water is preferable.
[0339] In addition, in order to promote the dissolution (aqueous solution) of the triazole compound (IV), it is preferred to use a solubilizing agent in the surface treatment solution of the present invention. Examples of the solubilizing agent include acids, bases, and organic solvents. These solubilizing agents may be used alone or in combination of two or more.
[0340] It should be noted that, regarding the preparation method of the surface treatment liquid using a solubilizer and water, the solubilizer may be added after the triazole compound and water are mixed, the triazole compound may be mixed with a mixed solution of water and the solubilizer, or water may be added after the triazole compound and the solubilizer are mixed.
[0341] Examples of the acid include inorganic acids such as hydrochloric acid, sulfuric acid, nitric acid, and phosphoric acid; organic acids such as formic acid, acetic acid, propionic acid, butyric acid, 2-ethylbutyric acid, valeric acid, caproic acid, heptanoic acid, caprylic acid, nonanoic acid, capric acid, lauric acid, myristic acid, palmitic acid, heptadecanoic acid, oleic acid, stearic acid, glycolic acid, lactic acid, gluconic acid, glyceric acid, malonic acid, succinic acid, levulinic acid, benzoic acid, oxalic acid, tartaric acid, malic acid, benzenesulfonic acid, toluenesulfonic acid, methanesulfonic acid, 5-sulfosalicylic acid, 4-hydroxybenzenesulfonic acid, 3-methyl-4-hydroxybenzenesulfonic acid, 4-aminobenzenesulfonic acid, camphorsulfonic acid, benzenedisulfonic acid, benzenetrisulfonic acid, aminosulfonic acid, and amino acids. These acids may be used alone or in combination of two or more.
[0342] Examples of the base include alkali metal hydroxides such as sodium hydroxide and potassium hydroxide; amines such as ammonia, methylamine, dimethylamine, trimethylamine, ethylamine, diethylamine, triethylamine, propylamine, isopropylamine, butylamine, pentylamine, hexylamine, heptylamine, octylamine, nonylamine, allylamine, ethylenediamine, diethylenetriamine, triethylenetetramine, monoethanolamine, diethanolamine, triethanolamine, monopropanolamine, dipropanolamine, tripropanolamine, monoisopropanolamine, diisopropanolamine, triisopropanolamine, 2-amino-1-propanol, N,N-dimethylethanolamine, cyclohexylamine, aniline, pyrrolidine, piperidine, piperazine, and pyridine. These bases may be used alone or in combination.
[0343] Examples of the organic solvent include methanol, ethanol, 1-propanol, 2-propanol, butanol, tert-butanol, ethylene glycol, propylene glycol, 1,4-butanediol, glycerol, diethylene glycol, triethylene glycol, ethylene glycol monomethyl ether, ethylene glycol dimethyl ether, ethylene glycol monoethyl ether, ethylene glycol diethyl ether, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol dimethyl ether, diethylene glycol monoethyl ether, diethylene glycol diethyl ether, diethylene glycol monobutyl ether, triethylene glycol dimethyl ether, triethylene glycol diethyl ether, tetrahydrofurfuryl alcohol, furfuryl alcohol, acetone, tetrahydrofuran, dimethicone ... Alkane, acetonitrile, 2-pyrrolidone, formamide, dimethylformamide, dimethylacetamide, dimethyl sulfoxide, sulfolane, dimethyl carbonate, ethylene carbonate, N-methylpyrrolidone, γ-butyrolactone, 1,3-dimethyl-2-imidazolidinone, etc. These organic solvents may be used alone or in combination of two or more.
[0344] The content of the solubilizing agent in the surface treatment liquid is preferably 0.1% by weight to 99% by weight, more preferably 0.5% by weight to 99% by weight, and even more preferably 1% by weight to 99% by weight.
[0345] <Hydrolysis of triazole compounds>
[0346] The triazole compound (IV) of the present invention has a triazole ring in the molecule, so the triazole ring interacts with the surface of the substrate (metal, resin material, inorganic material) to form a chemical bond, thereby improving the adhesion between different materials.
[0347] The hydrolysis method of the triazole compound (IV) is shown in Scheme (B). In Scheme (B), at least one of R5 and R6 of the triazole compound (IV) is represented by -(CH2) m -Si(OR) 3-p (OH) p Indicates the situation of the group.
[0348] The scheme (B) shows the manner in which the alkoxysilyl group of the triazole compound (IV) is hydrolyzed, that is, the manner in which the trialkoxysilyl group is gradually converted into a dialkoxyhydroxysilyl group, a dihydroxyalkoxysilyl group, and a trihydroxysilyl group.
[0349]
[0350] Generally, it is known that a substance having an alkoxysilyl group in a molecule functions as a silane coupling agent.
[0351] For example, when the bonding of copper to a resin material is taken as an example, when the triazole compound used in the practice of the present invention has an alkoxysilyl group in the molecule, the triazole ring interacts with the resin and copper to form a chemical bond, and the alkoxysilyl group (-Si-OR) is hydrolyzed and converted into a hydroxysilyl group (-Si-OH), which chemically bonds to copper oxide dispersed on the surface of the copper.
[0352] Therefore, by bringing copper into contact with a surface treatment liquid, a conversion film derived from the triazole compound (IV) is formed on the surface of the copper by bonding with a triazole ring or a hydroxysilyl group, thereby forming a resin layer composed of a resin material on the surface of the conversion film. In this case, the adhesion between copper and the resin material can be improved compared to the case where the resin layer is directly formed on the surface of copper.
[0353] In the practice of the present invention, the concentration of the triazole compound (IV) in the surface treatment solution is converted into the concentration of the triazole compound in the form of a trialkoxy group, and is preferably 0.0001 mol / L to 1.0000 mol / L, more preferably 0.0010 mol / L to 0.5000 mol / L, and further preferably 0.0100 mol / L to 0.1000 mol / L.
[0354] The triazole silane compound (IV) having a hydroxysilyl group generated in the surface treatment liquid gradually reacts with each other and undergoes dehydration condensation, and the hydroxysilyl group forms a siloxane bond (Si-O-Si) (refer to scheme (B)), and is converted into a silane oligomer that is difficult to dissolve in water (a triazole silane compound having a group represented by chemical formula (e) in scheme (B)). It should be noted that X in the group represented by chemical formula (e) is an integer representing the number of repeating units.
[0355] When the amount of silane oligomers produced in the surface treatment liquid increases, insoluble components precipitate (the treatment liquid becomes turbid) and adhere to the treatment tank, the piping connected to the treatment tank, and sensors immersed in the treatment liquid for detecting the temperature and liquid level of the treatment liquid, which may hinder smooth surface treatment.
[0356] In order to avoid this situation, in the preparation of the surface treatment liquid, as a solubilizing agent for the silane oligomer that is poorly soluble in water, it is preferred that the surface treatment liquid contains the organic solvent. In addition, in the preparation of the surface treatment liquid, in order to promote the dissolution of the triazole compound, it is preferred to contain the solubilizing agent (acid, alkali, organic solvent). It should be noted that the organic solvent also has the function of being a solubilizing agent for the silane oligomer, so it is preferred that the surface treatment liquid of the present invention contains at least one selected from the group consisting of acid, alkali, and organic solvent as a solubilizing agent.
[0357] Similarly, in order to improve the stability of the surface treatment liquid and the uniformity of the conversion film, substances that generate halide ions such as chloride ions, bromide ions, and iodide ions, or metal ions such as copper ions, iron ions, and zinc ions may be used.
[0358] The halide ions show the effect of uniformly forming the flat part of the conversion film. As substances that generate halide ions, for example, lithium fluoride, sodium fluoride, potassium fluoride, magnesium fluoride, calcium fluoride, lithium chloride, sodium chloride, potassium chloride, magnesium chloride, calcium chloride, lithium bromide, sodium bromide, potassium bromide, magnesium bromide, calcium bromide, lithium iodide, sodium iodide, potassium iodide, magnesium iodide, calcium iodide, ammonium fluoride, ammonium chloride, ammonium bromide, ammonium iodide, cuprous chloride, cupric chloride, cuprous bromide, cupric bromide, etc. The halogen compound may be contained as an impurity of other components.
[0359] The content of halide ions in the surface treatment liquid is not particularly limited, and is, for example, preferably 0.10 mol / L or less (especially 0 mol / L to 0.10 mol / L), more preferably 0.050 mol / L or less (especially 0 mol / L to 0.050 mol / L), further preferably 0.020 mol / L or less (especially 0 mol / L to 0.020 mol / L), and particularly preferably 0.010 mol / L or less (especially 0 mol / L to 0.010 mol / L).
[0360] Copper ions form complexes with triazole compounds, which can improve the strength of the conversion coating or improve the adhesion strength between the metal and the resin. The valence of the copper ion can be 1 or 2. As substances that generate copper ions, for example, metallic copper, copper sulfate (and its hydrates (especially pentahydrates)), copper formate (and its hydrates (especially tetrahydrates)), copper nitrate, cuprous chloride, cupric chloride, copper acetate (and its hydrates (especially monohydrates)), copper hydroxide, copper oxide, copper sulfide, copper carbonate, cuprous bromide, cupric bromide, copper phosphate, and copper benzoate can be listed.
[0361] Furthermore, when the copper circuit is treated with the surface treatment liquid, the copper ions in the surface treatment liquid may include copper ions eluted from the metallic copper or copper oxide contained in the copper circuit.
[0362] The content of copper ions in the surface treatment solution is not particularly limited, and is, for example, preferably 1.00 mol / L or less (particularly 0 mol / L or more and 1.00 mol / L or less), more preferably 0.50 mol / L or less (particularly 0 mol / L or more and 0.50 mol / L or less), further preferably 0.10 mol / L or less (particularly 0 mol / L or more and 0.10 mol / L or less), and particularly preferably 0.010 mol / L or less (particularly 0 mol / L or more and 0.010 mol / L or less).
[0363] In addition, a known coupling agent may be used in combination within the range that does not impair the effects of the present invention. Examples of known coupling agents include silane coupling agents (silane coupling agents) having a mercapto group (mercapto group), a vinyl group, an epoxy group, a (meth)acryloyl group, an amino group, a chloropropyl group, and the like.
[0364] Examples of such silane coupling agents include:
[0365] 3-Mercaptopropyltrimethoxysilane,
[0366] Mercaptosilane compounds such as 3-mercaptopropylmethyldimethoxysilane,
[0367] Vinyltrichlorosilane,
[0368] Vinyltrimethoxysilane,
[0369] Vinyl silane compounds such as vinyltriethoxysilane,
[0370] Styrylsilane compounds such as p-styryltrimethoxysilane,
[0371] 2-(3,4-Epoxycyclohexyl)ethyltrimethoxysilane,
[0372] 3-Glycidoxypropyltrimethoxysilane,
[0373] 3-Glycidoxypropylmethyldiethoxysilane,
[0374] Epoxysilane compounds such as 3-glycidoxypropyltriethoxysilane,
[0375] Acryloyloxysilane compounds such as 3-acryloyloxypropyltrimethoxysilane,
[0376] 3-methacryloxypropylmethyldimethoxysilane,
[0377] 3-Methacryloyloxypropyltrimethoxysilane,
[0378] 3-methacryloxypropylmethyldiethoxysilane,
[0379] Methacryloxysilane compounds such as 3-methacryloxypropyltriethoxysilane,
[0380] N-2-(Aminoethyl)-3-aminopropylmethyldimethoxysilane,
[0381] N-2-(Aminoethyl)-3-aminopropyltrimethoxysilane,
[0382] N-2-(Aminoethyl)-3-aminopropyltriethoxysilane,
[0383] 3-Aminopropyltrimethoxysilane,
[0384] 3-Aminopropyltriethoxysilane,
[0385] 3-Triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine,
[0386] N-phenyl-3-aminopropyltrimethoxysilane,
[0387] Aminosilane compounds such as N-(vinylbenzyl)-2-aminoethyl-3-aminopropyltrimethoxysilane,
[0388] Urea silane compounds such as 3-ureidopropyltriethoxysilane,
[0389] Chloropropylsilane compounds such as 3-chloropropyltrimethoxysilane,
[0390] Sulfide silane compounds such as bis(triethoxysilylpropyl)tetrasulfide, and
[0391] Isocyanatosilane compounds such as 3-isocyanatopropyltriethoxysilane, etc.
[0392] In addition, aluminum-based coupling agents, titanium-based coupling agents, zirconium-based coupling agents, and the like can also be cited.
[0393] (Handling method)
[0394] There is no particular limitation on the method for bringing the surface treatment liquid of the present invention into contact with the surface of the substrate, and similarly to the case of the coupling agent, spraying, dipping, coating, and the like may be employed.
[0395] The time for contacting the surface treatment liquid with the substrate (treatment time) is preferably set to 1 second to 10 minutes, and more preferably set to 5 seconds to 3 minutes. When the treatment time is less than 1 second, the thickness of the conversion film formed on the substrate surface becomes thinner, and it is difficult to obtain sufficient adhesion between materials of different materials. On the other hand, even if the treatment time is more than 10 minutes, there is no significant difference in the thickness of the conversion film. Therefore, from the perspective of productivity, it is preferably treated within 10 minutes.
[0396] The temperature of the surface treatment liquid when the surface treatment liquid is brought into contact with the substrate surface is preferably set to 5° C. to 50° C., and can be appropriately set in relation to the above-mentioned treatment time.
[0397] After the substrate is brought into contact with the surface treatment liquid of the present invention, it may be washed with water and then dried, or it may be dried without washing with water.
[0398] The drying is preferably performed at a temperature of room temperature to 150°C.
[0399] It should be noted that the water used for water washing is preferably pure water such as ion-exchanged water and distilled water. The method and time of water washing are not particularly limited, and the washing can be carried out by spraying, immersion, etc. for an appropriate time.
[0400] The thickness of the conversion film is preferably 0.5 nm to 1,000 nm, more preferably 1 nm to 200 nm, and even more preferably 1 nm to 100 nm. When the thickness is 0.5 nm or more, the adhesion between materials is sufficiently improved, and when the thickness is 1,000 nm or less, the chemical resistance of the conversion film can be maintained.
[0401] In the present invention, the dried conversion film may be treated with plasma, laser, ion beam, ozone, heating, humidification, etc. to modify the surface of the conversion film. Alternatively, plasma, laser, ion beam, pumice brush, etc. mechanical grinding, drilling, etc. processing methods may be used to clean the metal surface for the purpose of removing resin and ion residues.
[0402] Before the surface treatment liquid of the present invention is brought into contact with the surface of copper or copper alloy (hereinafter, both are sometimes referred to as copper), the surface of the copper may be subjected to at least one pretreatment selected from pickling treatment, alkali treatment, roughening treatment, heat resistance treatment, rust prevention treatment or conversion treatment.
[0403] The pickling treatment is performed to remove the grease components attached to the surface of the copper and to remove the oxide film on the surface of the copper. In the pickling treatment, solutions such as hydrochloric acid solutions, sulfuric acid solutions, nitric acid solutions, sulfuric acid-hydrogen peroxide solutions, organic acid solutions, inorganic acid-organic solvent solutions, and organic acid-organic solvent solutions can be used.
[0404] The alkali treatment is performed to remove the grease components attached to the surface of copper and to remove the residues of the previous process (for example, dry film resist for copper circuit formation, etc.). In the alkali treatment, a solution containing an alkali metal hydroxide such as sodium hydroxide and potassium hydroxide; an amine such as ammonia, ethanolamine, monopropanolamine, tetramethylammonium hydroxide; an aqueous solution of sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, ammonium carbonate, ammonium bicarbonate, sodium acetate, potassium acetate, sodium phosphate, disodium hydrogen phosphate, potassium phosphate, dipotassium hydrogen phosphate, etc., an organic solvent solution, etc. can be used.
[0405] The roughening treatment is performed to improve the adhesion between copper and resin due to the anchoring effect, and a concave-convex shape is given to the surface of copper to improve the adhesion between copper and resin materials. The roughening treatment can be performed by micro-etching, electroplating, electroless plating, oxidation (black oxide, brown oxide), redox method, brush grinding, jet scrubbing, etc.
[0406] In the micro-etching method, various etchants such as organic acid-divalent copper ion, sulfuric acid-hydrogen peroxide, persulfate, cupric chloride, and ferric chloride can be used. In the electroplating method, fine copper particles are precipitated on the surface of copper to form unevenness on the surface of copper.
[0407] In the heat-resistant treatment, at least one coating selected from nickel, nickel-phosphorus, zinc, zinc-nickel, copper-zinc, copper-nickel, copper-nickel-cobalt or nickel-cobalt is formed on the surface of copper. The coating can be formed by a known method using electroplating, but is not limited to electroplating, and there is no problem in using means such as evaporation.
[0408] The rust prevention treatment is performed to prevent oxidation corrosion on the copper surface, and a method of forming a plating film composed of zinc or zinc alloy or a plating film of electrolytic chromate on the copper surface can be adopted. In addition, a treatment solution containing an organic compound type rust inhibitor such as a benzotriazole type rust inhibitor can also be brought into contact with the copper surface.
[0409] In the conversion treatment, a method of forming a passive film of tin or a method of forming a passive film of copper oxide can be used.
[0410] It is also possible to contact an aqueous solution containing copper ions with the surface of the copper before and / or after the surface treatment solution of the present invention is contacted with the surface of the copper. The aqueous solution containing copper ions has the function of improving the film-forming property of the conversion film formed on the surface of the copper and making the thickness of the conversion film formed on the surface of the copper uniform. The valence of the copper ion is not particularly limited, and is a monovalent or divalent copper ion.
[0411] The copper ion source of the aqueous solution containing copper ions is not particularly limited as long as it is a copper salt soluble in water, and examples thereof include copper salts such as copper sulfate, copper nitrate, copper chloride, copper formate, and copper acetate. In order to make the copper salt soluble in water, ammonia, hydrochloric acid, etc. may be added.
[0412] Before and / or after the surface treatment solution of the present invention is brought into contact with the surface of copper, an acidic aqueous solution or an alkaline aqueous solution may be brought into contact with the surface of the copper. The acidic aqueous solution or the alkaline aqueous solution also has the function of making the thickness of the conversion film formed on the surface of copper uniform, similarly to the aqueous solution containing copper ions.
[0413] There are no particular restrictions on the acidic aqueous solution and the alkaline aqueous solution. Examples of the acidic aqueous solution include aqueous solutions containing inorganic acids such as sulfuric acid, nitric acid, and hydrochloric acid; aqueous solutions containing organic acids such as formic acid, acetic acid, lactic acid, glycolic acid, and amino acids, etc. Examples of the alkaline aqueous solution include hydroxides of alkali metals such as sodium hydroxide and potassium hydroxide; amines such as ammonia, ethanolamine, monopropanolamine, and tetramethylammonium hydroxide; aqueous solutions of sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, ammonium carbonate, ammonium bicarbonate, sodium acetate, potassium acetate, sodium phosphate, disodium hydrogen phosphate, potassium phosphate, and dipotassium hydrogen phosphate, etc.
[0414] Before bringing the surface treatment liquid of the present invention into contact with the copper surface, an aqueous solution containing a known coupling agent may be brought into contact with the copper surface.
[0415] After the surface treatment liquid of the present invention is brought into contact with the copper surface, an aqueous solution containing a known coupling agent may be brought into contact with the copper surface.
[0416] After the surface treatment liquid of the present invention is brought into contact with the surface of copper, the surface may be brought into contact with a treatment liquid containing a known organic compound-based rust inhibitor such as a benzotriazole-based rust inhibitor.
[0417] The surface treatment liquid of the present invention can be used to treat the surface of at least one substrate selected from the group consisting of the metal, inorganic material and resin material. By using the surface treatment liquid of the present invention to treat the surface of the substrate, a conversion film can be formed on the substrate surface, thereby improving the adhesion to other materials.
[0418] In the present invention, the surface treatment liquid of the present invention can be used to make two materials selected from the group consisting of the metal, inorganic material, and resin material adhere to each other. By adhering the two materials through the layer of the conversion coating formed by the surface treatment liquid of the present invention, the affinity between the two materials can be improved, so that even materials of different materials can be more firmly adhered to each other.
[0419] (Gluing method)
[0420] The bonding method of the two materials can be carried out by a known method. The following method can be cited: the surface treatment liquid of the present invention is brought into contact with the surface of a substrate composed of a metal, an inorganic material or a resin material to form a conversion film, and another substrate is bonded to a part or the whole of the formed conversion film by means of coating, crimping, mixing, etc., using an adhesive, an adhesive sheet (film) or a combination of these means.
[0421] In addition, the following method can be listed: the surface treatment liquid of the present invention is brought into contact with the surfaces of two substrates selected from metals, inorganic materials, and resin materials, thereby forming conversion films on the surfaces of the two substrates respectively, and the two substrates are bonded together by means of coating, crimping, mixing, etc., using an adhesive, an adhesive sheet (film), or a combination of these means.
[0422] By using the surface treatment liquid of the present invention, two materials, particularly two materials of different materials, can be bonded together as described above, and thus the surface treatment liquid can be applied to electronic devices such as various electric and electronic parts, semiconductor wafers, and printed wiring boards.
[0423] It should be noted that, in the present invention, the surface treatment liquid of the present invention can be preferably used for a substrate formed of a metal, particularly copper or a copper alloy. For example, it is suitable for surface treatment of copper or a copper alloy for the purpose of improving the adhesion (adhesion) between a copper circuit (copper wiring layer) and a semi-cured or cured prepreg, solder resist, semi-cured or cured dry film resist (insulating resin layer), and in a printed wiring board having an insulating resin layer in contact with the copper wiring layer, it can improve the adhesion between the copper wiring layer and the insulating resin layer.
[0424] In the use example in semiconductor chips, it is suitable for surface treatment of semiconductor circuits for the purpose of improving the adhesion (stickiness) between the semiconductor circuits formed on the semiconductor chips and protective films (for example, insulating protective films such as photosensitive positive type, photosensitive negative type, non-photosensitive buffer coatings, bump protection films, etc.).
[0425] In addition, in a packaging substrate (WL-CSP, FO-WLP, PLP) or a 2.5-dimensional (2.5D) or 3-dimensional (3D) interposer substrate in which a rewiring layer is formed on a semiconductor chip, it is suitable for surface treatment of the copper circuit rewiring layer for the purpose of improving the adhesion (adhesion) between the copper circuit rewiring layer and the insulating material.
[0426] Examples of the protective film and insulating material include polyimide resin, polybenzoic acid, Azole resin, polysiloxane resin, etc.
[0427] The printed wiring board can be made by contacting the surface treatment liquid of the present invention with the surface of the copper wiring, then washing and drying, and then forming an insulating resin layer on the surface of the copper wiring. As described above, the contact method is simple and reliable, and is preferably used to immerse the copper wiring in the surface treatment liquid or spray the treatment liquid onto the copper wiring.
[0428] The water washing method is not particularly limited, but immersing the copper wiring in washing water or spraying the washing water onto the surface of the copper wiring is simple and reliable, and is preferred.
[0429] In forming the insulating resin layer, a known method can be used, such as a method of pasting a semi-cured resin material, a method of applying a liquid resin material containing a solvent, etc. Next, a via hole is formed to connect the upper and lower wirings. By repeating this process, a multilayer printed wiring board can be manufactured.
[0430] In the circuit forming method of the printed wiring board, an example of a semi-additive method using the surface treatment liquid of the present invention is shown below.
[0431] (a) preparing an insulating substrate having a first conductive layer on a first surface of an insulating substrate or an insulating substrate having a through-hole and a through-hole, a second surface opposite to the first surface, and inner walls of the through-hole and the through-hole,
[0432] (b) forming a photo-crosslinkable resin layer and a mask layer on the first surface and the second surface, and covering the first surface and the second surface and the through hole and the first conductive layer on the inner wall of the through hole with the photo-crosslinkable resin layer and the mask layer,
[0433] (c) a step of pattern-exposing the first surface and the second surface and the photo-crosslinkable resin layer around the through holes and the vias,
[0434] (d) removing the mask layer around the first surface and the second surface and the through holes and the via holes,
[0435] (e) developing and removing the uncured photo-crosslinkable resin layer on the first surface, the second surface and the periphery of the through-holes and the vias using a photo-crosslinkable resin layer removing solution to expose the first conductive layer on the first surface, the first conductive layer on the second surface and the periphery of the through-holes and the vias,
[0436] (f) forming a second conductive layer on the first surface and the second surface and on the first conductive layer exposed on the inner wall of the through hole and the through hole by electroplating,
[0437] (g) removing the cured photo-crosslinkable resin layer on the first surface and the second surface and around the through holes and the via holes to expose the first conductive layer and the second conductive layer on the first surface and the second surface and the inner wall of the through holes and the via holes,
[0438] (h) a step of removing the exposed first conductive layer by flash etching,
[0439] (i) forming a third conductive layer on the first and second surfaces and on the through holes and the inner walls of the through holes by electroless plating and electroplating,
[0440] (j) a step of laminating an insulating resin layer on the first surface, the second surface and the first conductive layer, the second conductive layer and the third conductive layer on the inner wall of the through hole and the through hole,
[0441] In a method for manufacturing a circuit substrate including at least one of the above-mentioned steps, the surface treatment liquid of the present invention is brought into contact with the first conductive layer, the second conductive layer and the third conductive layer on the first surface and the second surface and the inner wall of the through hole and the through hole, the insulating resin substrate, the resist layer, the photo-crosslinkable resin layer used in the plated resist layer, and at least one metal layer or resist layer in the insulating resin layer, thereby manufacturing a printed wiring board.
[0442] Furthermore, an example of a subtractive method using the surface treatment liquid of the present invention in the circuit forming method of the printed wiring board is shown below.
[0443] (a) preparing an insulating substrate having a first conductive layer on a first surface of an insulating substrate or an insulating substrate having through holes and vias, a second surface opposite to the first surface, and inner walls of the through holes and vias,
[0444] (b) forming a photo-crosslinkable resin layer and a mask layer on the first surface and the second surface, and covering the first surface and the second surface and the through hole and the first conductive layer on the inner wall of the through hole with the photo-crosslinkable resin layer and the mask layer,
[0445] (c) a step of pattern-exposing the first surface and the second surface and the photo-crosslinkable resin layer around the through holes and the vias,
[0446] (d) removing the mask layer around the first surface and the second surface and the through holes and the via holes,
[0447] (e) developing and removing the uncured photo-crosslinkable resin layer on the first surface, the second surface and the periphery of the through-holes and the vias using a photo-crosslinkable resin layer removing solution to expose the first conductive layer on the first surface, the first conductive layer on the second surface and the periphery of the through-holes and the vias,
[0448] (f) removing the first conductive layer exposed on the first surface and the second surface and on the inner wall of the through hole and the through hole by etching,
[0449] (g) removing the cured photo-crosslinkable resin layer on the first surface and the second surface and around the through holes and the via holes to expose the first conductive layer and the second conductive layer on the first surface and the second surface and the inner wall of the through holes and the via holes,
[0450] (h) forming a third conductive layer on the first and second surfaces and on the first and second conductive layers on the inner walls of the through holes and the vias by electroless plating and electroplating,
[0451] (i) laminating an insulating resin layer on the first surface, the second surface and the first conductive layer, the second conductive layer and the third conductive layer on the inner wall of the through hole and the through hole,
[0452] In a method for manufacturing a circuit substrate including at least one of the above-mentioned steps, the surface treatment liquid of the present invention is brought into contact with the first conductive layer, the second conductive layer and the third conductive layer on the first surface and the second surface and the inner wall of the through hole and the through hole, the insulating resin substrate, the resist layer, the photo-crosslinkable resin layer used in the plated resist layer, and at least one metal layer or resist layer in the insulating resin layer, thereby manufacturing a printed wiring board.
[0453] The copper wiring and the conductive layer may be produced by any method such as electroless plating, electroplating, vapor deposition, sputtering, or damascene, and may include inner vias, through holes, connection terminals, and the like.
[0454] In addition, the "copper" involved in the present invention refers to foils (electrolytic copper foil, rolled copper foil, copper foil with resin, copper foil with carrier, electroless copper foil, sputtered copper foil, thin copper foil) used in electronic devices such as printed wiring boards and lead frames, decorations, building materials, etc., plating (electroless copper plating, electrolytic copper plating), thin films formed by evaporation, sputtering, inlaying, etc., and copper used in applications and forms such as grains, needles, fibers, wires, rods, tubes, and plates. It should be noted that in the case of copper wiring through which high-frequency electrical signals flow in recent years, the surface of copper is preferably a smooth surface with an average roughness of less than 0.1 μm. The surface of copper can be plated with nickel, zinc, chromium, tin, etc. as a pretreatment.
[0455] In addition, for example, in the use example of a lead frame during wire bonding installation, the surface treatment liquid of the present invention is suitable for the surface treatment of the lead frame, wherein the surface treatment of the lead frame is for the purpose of improving the adhesion (adhesion) with the sealing resin or the adhesive during semiconductor chip installation, such as the metal surface of the lead frame manufacturing process or the frame metal surface after the semiconductor chip is installed (before and after the chip welding-prebaking process), the frame metal surface after the wire bonding installation, and the frame metal surface in the process before resin sealing (before and after the resin molding and baking process).
[0456] In addition, for example, in the use example of a lead frame during flip chip mounting, the surface treatment liquid of the present invention is suitable for the surface treatment of the lead frame, wherein the surface treatment of the lead frame is for the purpose of improving the adhesion (adhesion) with the sealing resin and the adhesive during semiconductor chip mounting, such as the metal surface in the lead frame manufacturing process or the metal surface of the lead frame after temporarily placing the bonding material (solder, Au plating, Sn plating, etc.), the metal surface of the frame after mounting the semiconductor chip (position alignment, chip mounting-baking process before and after), the metal surface of the lead frame after formal curing (before and after processes such as reflow heating, thermal compression bonding, ultrasonic waves, plasma, etc.), and the metal surface of the lead frame in the process before resin sealing.
[0457] In addition, for example, in the use example of a fine wiring substrate that improves the integration technology for densely arranged semiconductor chips, the surface treatment liquid of the present invention is also suitable for the surface treatment of copper circuit wiring layers in 2.1-dimensional (2.1D) organic substrates or glass substrates, component-embedded substrates (EPS substrates) in which semiconductors are built into the substrate, and coreless substrates for the purpose of improving the adhesion (adhesion) between the copper circuit wiring layer and the insulating material.
[0458] In addition, for example, in the case of embedding pattern wiring, laser through-hole processing on the upper and lower layers and filling-hole plating, in the case of using a circuit embedded substrate (ETS substrate) in which the upper and lower layers are connected using copper pillars formed by plating and the insulating layer uses MIS using a molded resin, the metal surface treatment liquid of the present invention is suitable for the surface treatment of the copper circuit wiring layer for the purpose of improving the adhesion (adhesion) between the copper circuit wiring layer and the insulating material.
[0459] In addition, the copper foil with a carrier treated with the surface treatment liquid of the present invention refers to an ultra-thin electrolytic copper foil used in a printed wiring board including a process of forming a circuit by any of a semi-additive method, a subtractive method, a partial additive method or a modified semi-additive method, and has a copper foil carrier, a peeling layer laminated on the copper foil carrier, and an ultra-thin copper layer laminated on the peeling layer. The surface of the copper may be subjected to at least one pretreatment selected from the group consisting of pickling treatment, roughening treatment, heat resistance treatment, rust prevention treatment or conversion treatment.
[0460] (Insulating composition)
[0461] By incorporating the coupling agent of the present invention into a resin material or an inorganic material, an insulating composition can be obtained.
[0462] Alternatively, an insulating composition can be obtained by dissolving the triazole compound (IV) in an organic solvent or the like and mixing the mixture with a resin material or an inorganic material.
[0463] The content of the triazole compound (IV) in the insulating composition is preferably 0.001% to 10% by weight, and more preferably 0.01% to 5% by weight. When the content of the triazole compound (IV) in the insulating composition is 0.001% by weight or more, the effect of improving the adhesiveness can be fully obtained. When the concentration is greater than 10% by weight, the effect of improving the adhesiveness almost reaches the limit. Therefore, from an economic point of view, the content of the triazole compound (IV) is preferably set to 10% by weight or less.
[0464] The insulating composition can be prepared by a known method. For example, the insulating composition can be prepared by dissolving the triazole compound (IV) in an organic solvent and mixing it with a solid or liquid resin material. Alternatively, the insulating composition can be prepared by directly adding the triazole compound (IV) to a liquid resin material and mixing them.
[0465] The insulating composition of the present invention can provide an insulating material having high adhesive strength and can therefore be suitably used in various electric and electronic parts and electronic devices such as printed wiring boards.
[0466] Japanese Patent Application Publication No. 2009-19266 discloses an invention regarding a method for forming a silane coupling agent coating, which is characterized in that it includes: a step of applying a liquid containing a silane coupling agent on a metal surface, a step of drying the metal surface coated with the liquid at a temperature of 25° C. to 150° C. within 5 minutes, and a step of washing the dried metal surface with water.
[0467] Alternatively, as a surface treatment, an adhesive metal layer of tin or the like may be formed on the metal surface by immersion in a plating solution.
[0468] The surface treatment liquid of the present invention can be used as the liquid containing the silane coupling agent. It should be noted that the matters described in the patent publication constitute a part of the present specification by reference.
[0469] Example
[0470] Hereinafter, the present invention will be specifically described by way of Examples (synthesis test, evaluation test), but the present invention is not limited thereto.
[0471] In addition, OEt in the chemical formula shown below represents an ethoxy group.
[0472] The triazole compound and the haloalkylsilane compound used as raw materials in the synthesis test are as follows.
[0473] [Triazole compounds]
[0474] ・Triazole compound (3,3'-bis(5-amino-1,2,4-triazole)) represented by the following formula (11): synthesized according to the method described in "European Journal of Chemistry", Vol. 18, p. 16742 (2012).
[0475] ・Triazole compound (3,3'-methylenebis(5-amino-1,2,4-triazole)) represented by the following formula (12): synthesized according to the method described in "Russ. J. Applied. Chem.", Vol. 82, p. 276 (2009).
[0476] ・Triazole compound represented by the following formula (13) (3,3'-tetramethylenebis(5-amino-1,2,4-triazole)): synthesized according to the method described in the specification of U.S. Patent No. 2744116.
[0477] ・Triazole compound (3,3'-bis(5-methyl-1,2,4-triazole)) represented by the following formula (14): synthesized according to the method described in "Indian J. Chem.", Vol. 44B, p. 568 (2005).
[0478]
[0479] [Haloalkylsilane compounds]
[0480] ・3-Chloropropyltriethoxysilane: Made by Tokyo Chemical Industry Co., Ltd.
[0481] The triazole compounds used in Comparative Example 1 (evaluation test) are as follows.
[0482] [Triazole compounds]
[0483] ・Triazole compound (3-amino-5-methyl-1,2,4-triazole) represented by the following formula (21): synthesized according to the method described in the specification of U.S. Patent No. 4734413.
[0484] ・Triazole compound represented by the following formula (22) (3-amino-5-methyl-1-[3-(triethoxysilyl)propyl]-1,2,4-triazole): synthesized according to the method described in International Publication No. 2018 / 186476.
[0485]
[0486] <Synthesis of triazole compound (I)>
[0487] The triazole compounds of Examples 1 to 5 below were synthesized.
[0488] [Example 1]
[0489] <Synthesis of a mixture of 1-[3-(triethoxysilyl)propyl]-3,3'-bis(5-amino-1,2,4-triazole) and 2-[3-(triethoxysilyl)propyl]-3,3'-bis(5-amino-1,2,4-triazole)>
[0490] A compound represented by the following formula (1) (a mixture of 1-[3-(triethoxysilyl)propyl]-3,3′-bis(5-amino-1,2,4-triazole) and 2-[3-(triethoxysilyl)propyl]-3,3′-bis(5-amino-1,2,4-triazole)) was synthesized.
[0491] A suspension consisting of 7.80 g (46.9 mmol) of 3,3'-bis(5-amino-1,2,4-triazole) and 200 mL of N,N-dimethylacetamide was heated to 80°C, 16.20 g (47.6 mmol) of 20% sodium ethanol ethanol solution was added, the temperature was raised to 100°C and stirred for 1 hour. Next, the temperature was adjusted to 70°C, and then 11.40 g (47.3 mmol) of 3-chloropropyltriethoxysilane was added and stirred for 1 hour. Next, the temperature was raised to 100°C and stirred for 16.5 hours. The reaction solution was cooled to 60°C, the insoluble matter was filtered off, and the filtrate was removed by decompression distillation, thereby obtaining 15.81 g (46.9 mmol, yield 91.0%) of brown maltose-like substance.
[0492] The resulting brown maltose 1 The H-NMR spectrum data are as follows.
[0493] 1 H-NMR(DMSO-d6)δ: 0.55(m,2H),1.14(m,9H),1.75(m,2H),3.34(m,2H),3.73(m,6H),5.23(s,2H),6.41(s,2H).
[0494] By 1 Based on H-NMR spectral data, the obtained brown maltose-like substance was identified as the title triazole compound represented by chemical formula (1).
[0495]
[0496] [Example 2]
[0497] <Synthesis of a mixture of 1-[3-(triethoxysilyl)propyl]-3,3'-methylenebis(5-amino-1,2,4-triazole) and 2-[3-(triethoxysilyl)propyl]-3,3'-methylenebis(5-amino-1,2,4-triazole)>
[0498] A compound represented by the following formula (2) (a mixture of 1-[3-(triethoxysilyl)propyl]-3,3'-methylenebis(5-amino-1,2,4-triazole) and 2-[3-(triethoxysilyl)propyl]-3,3'-methylenebis(5-amino-1,2,4-triazole)) was synthesized.
[0499] A suspension consisting of 6.08 g (33.8 moles) of 3,3'-methylenebis(5-amino-1,2,4-triazole) and 150 mL of N,N-dimethylacetamide was heated to 80°C, 11.72 g (34.4 moles) of a 20% sodium ethoxide ethanol solution was added, and the mixture was stirred for 2 hours, and then 8.30 g (34.5 moles) of 3-chloropropyltriethoxysilane was added, and the mixture was stirred for 30 minutes, and then stirred at 100°C for 20 hours. The reaction solution was cooled to 70°C, and then the insoluble matter was filtered off, and the filtrate was distilled off under reduced pressure, thereby obtaining 10.50 g (27.3 moles, yield 80.8%) of a light brown solid.
[0500] The obtained light brown solid 1 The H-NMR spectrum data are as follows.
[0501] 1 H-NMR(DMSO-d6)δ: 0.57(m,2H),1.15(m,9H),1.53(m,2H),2.94(s,2H),3.45(m,2H),3.73(m,6H),5.04(s,2H),5.98(s,2H).
[0502] By 1 Based on H-NMR spectral data, the obtained light brown solid was identified as the title triazole compound represented by chemical formula (2).
[0503]
[0504] [Example 3]
[0505] <Synthesis of a mixture of 1-[3-(triethoxysilyl)propyl]-3,3'-tetramethylenebis(5-amino-1,2,4-triazole) and 2-[3-(triethoxysilyl)propyl]-3,3'-tetramethylenebis(5-amino-1,2,4-triazole)>
[0506] A compound represented by the following formula (3) (a mixture of 1-[3-(triethoxysilyl)propyl]-3,3'-tetramethylenebis(5-amino-1,2,4-triazole) and 2-[3-(triethoxysilyl)propyl]-3,3'-tetramethylenebis(5-amino-1,2,4-triazole)) was synthesized.
[0507] A suspension consisting of 8.20 g (36.9 moles) of 3,3'-tetramethylenebis(5-amino-1,2,4-triazole) and 200 mL of N,N-dimethylacetamide was heated to 80°C, 12.70 g (37.3 moles) of 20% sodium ethanol ethanol solution was added, the temperature was raised to 100°C and stirred for 1 hour. Next, the temperature was adjusted to 70°C, and then 9.04 g (37.5 moles) of 3-chloropropyltriethoxysilane was added and stirred for 1 hour. Next, the temperature was raised to 100°C and stirred for 16 hours. The reaction solution was cooled to 60°C, the insoluble matter was filtered off, and the filtrate was distilled off under reduced pressure to obtain 13.8 g (32.3 moles, yield 87.7%) of a light brown maltose-like substance.
[0508] The obtained light brown maltose 1 The H-NMR spectrum data are as follows.
[0509] 1 H-NMR(DMSO-d6)δ: 0.50(m,2H),1.13(t,9H),1.61(m,4H),2.09(m,2H),2.42(m,4H),3.34(m,2H),3.73(m,6H),5.06(s,2H),5.96(s,2H).
[0510] By 1 Based on H-NMR spectrum data, the obtained light brown maltose-like substance was identified as the title triazole compound represented by chemical formula (3).
[0511]
[0512] [Example 4]
[0513] <Synthesis of a mixture of 3,3'-bis{1-[3-(triethoxysilyl)propyl]-5-amino-1,2,4-triazole}, 3,3'-bis{2-[3-(triethoxysilyl)propyl]-5-amino-1,2,4-triazole}, and 1-[3-(triethoxysilyl)propyl]-2'-[3-(triethoxysilyl)propyl]-3,3'-bis(5-amino-1,2,4-triazole)>
[0514] A compound represented by the following formula (4) (a mixture of 3,3'-bis{1-[3-(triethoxysilyl)propyl]-5-amino-1,2,4-triazole}, 3,3'-bis{2-[3-(triethoxysilyl)propyl]-5-amino-1,2,4-triazole} and 1-[3-(triethoxysilyl)propyl]-2'-[3-(triethoxysilyl)propyl]-3,3'-bis(5-amino-1,2,4-triazole)) was synthesized.
[0515] To a suspension consisting of 1.50 g (9.0 mmol) of 3,3'-bis(5-amino-1,2,4-triazole) and 5.60 g of water, 1.50 g (18.0 mmol) of 48% aqueous sodium hydroxide solution was added, and the mixture was stirred at room temperature for 30 minutes. Then, the water was distilled off under reduced pressure, and then 5.6 g of ethanol was added, and the mixture was stirred at room temperature for 1 hour. Then, the solid was filtered, washed with ethanol, and then dried to obtain 2.1 g of white powder.
[0516] To the obtained white powder 2.1g, 30g of dimethyl sulfoxide was added and heated to 70°C, 4.80g (20.0 mmol) of 3-chloropropyltriethoxysilane was added and stirred for 1 hour, and then stirred at 100°C for 16 hours. The reaction solution was cooled to room temperature, and then the insoluble matter was filtered off, and the filtrate was distilled off under reduced pressure, and then 30g of isopropyl acetate was added and stirred at room temperature for 1 hour. Then, the solid was filtered, washed with isopropyl acetate, and then dried to obtain 4.67g (8.1 mmol, yield 90.0%) of yellow-brown powder.
[0517] The obtained yellow-brown powder 1 The H-NMR spectrum data are as follows.
[0518] 1 H-NMR(DMSO-d6)δ: 0.54(m,4H),1.11(m,18H),1.74(m,4H),3.69(m,12H),3.93(m,4H),5.22(s,2H),6.44(s,2H).
[0519] By 1 Based on H-NMR spectral data, the obtained yellow-brown powder was identified as the title triazole compound represented by chemical formula (4).
[0520]
[0521] [Example 5]
[0522] <Synthesis of a mixture of 1-[3-(triethoxysilyl)propyl]-3,3'-bis(5-methyl-1,2,4-triazole) and 2-[3-(triethoxysilyl)propyl]-3,3'-bis(5-methyl-1,2,4-triazole)>
[0523] A compound represented by the following formula (5) (a mixture of 1-[3-(triethoxysilyl)propyl]-3,3'-bis(5-methyl-1,2,4-triazole) and 2-[3-(triethoxysilyl)propyl]-3,3'-bis(5-methyl-1,2,4-triazole)) was synthesized.
[0524] A suspension consisting of 3.30 g (20.0 mmol) of 3,3'-bis(5-methyl-1,2,4-triazole) and 30 g of dimethyl sulfoxide was heated to 70°C, 6.80 g (20.0 mmol) of 20% sodium ethanol ethanol solution was added, and stirred for 1 hour. Next, 4.80 g (20.0 mmol) of 3-chloropropyltriethoxysilane was added and stirred for 30 minutes. Next, the temperature was raised to 100°C and stirred for 19 hours. The reaction solution was cooled to room temperature, and then the insoluble matter was filtered off, and the filtrate was removed by vacuum distillation, and then 30 g of isopropyl acetate was added and stirred at room temperature for 1 hour. Next, the solid was filtered, washed with isopropyl acetate, and then dried to obtain 3.39 g (9.2 mmol, yield 46.0%) of light brown powder.
[0525] The obtained light brown powder 1 The H-NMR spectrum data are as follows.
[0526] 1 H-NMR(DMSO-d6)δ: 0.55(m,2H),1.14(t,9H),1.75(m,2H),2.30(s,6H),3.43(q,6H),3.51(m,2H).
[0527] By 1 Based on H-NMR spectral data, the obtained light brown powder was identified as the title triazole compound represented by chemical formula (5).
[0528]
[0529] <Adhesion Test 1>
[0530] The surface treatment liquids prepared in the following Examples 6 to 9 and Comparative Examples 2 and 3 were evaluated for the following adhesiveness.
[0531] [Evaluation test of adhesiveness (i)]
[0532] (1) Metal
[0533] As the metal, an electrolytic copper foil (thickness: 35 μm) was used.
[0534] (2) Surface treatment of metal
[0535] The copper foil was treated according to the following steps a and b.
[0536] a. Acid cleaning (5% sulfuric acid aqueous solution) / 1 minute (room temperature), water washing
[0537] b. Apply the surface treatment liquid and dry for 1 minute (100℃)
[0538] (3) Adhesion between metal and resin
[0539] A glass cloth epoxy resin-impregnated prepreg (MEGTRON7 (manufactured by Panasonic Corporation)) was laminated and pressed on the S surface of the treated copper foil, and the copper foil and the prepreg were bonded to produce a copper-clad laminate.
[0540] (4) Evaluation of Adhesion
[0541] The copper-clad laminate was subjected to reflow heating once (peak temperature 260° C., air), and then a test piece having a width of 10 mm was prepared according to “JIS C6481 (1996)” and the peel strength (peel strength (kN / m)) of the copper foil was measured.
[0542] [Example 6]
[0543] To 1 g of the compound represented by the formula (1) as a coupling agent component was added 99 g of a 4:96 mixed solution (weight ratio) of 25% ammonia water and methanol, and the mixture was stirred at room temperature for 1 hour to prepare a surface treatment solution.
[0544] [Examples 7 to 9]
[0545] A surface treatment liquid was prepared in the same manner as in Example 6 except that the compound represented by the formula (2), the compound represented by the formula (3) or the compound represented by the formula (11) was used instead of the compound represented by the formula (1).
[0546] [Comparative Example 1]
[0547] The copper foil subjected to only the step (2) a. of the adhesion evaluation test (i) was subjected to the adhesion evaluation test (i).
[0548] [Comparative Examples 2 to 3]
[0549] A surface treatment liquid was prepared in the same manner as in Example 6 except that the compound represented by the formula (21) and the compound represented by the formula (22) were used instead of the compound represented by the formula (1).
[0550] The surface treatment liquids prepared above were subjected to an adhesiveness evaluation test (i). The obtained test results are shown in Table 1.
[0551]
[0552] As can be seen from the results in Table 1, the surface treatment liquids of the present invention (surface treatment liquids of Examples 6 to 9) have higher peel strengths than those of Comparative Examples 1 to 3, and are excellent in adhesion between metal and resin.
[0553] <Adhesion Test 2>
[0554] The surface treatment liquids prepared in the following Examples 10 and 11 and Comparative Examples 5 and 6 were evaluated for the following adhesiveness.
[0555] [Example 10]
[0556] To 1 g of the compound represented by the formula (1) as a coupling agent component, 99 g of a 1:9 mixed solution (weight ratio) of 10% acetic acid water and methanol was added, and the mixture was stirred at room temperature for 1 hour to prepare a surface treatment solution.
[0557] [Example 11]
[0558] A surface treatment liquid was prepared in the same manner as in Example 10 except that the compound represented by the formula (11) was used instead of the compound represented by the formula (1).
[0559] [Comparative Example 4]
[0560] The copper foil subjected to only the step (2) a. of the adhesiveness evaluation test (i) was subjected to the adhesiveness evaluation test (i).
[0561] [Comparative Examples 5-6]
[0562] A surface treatment liquid was prepared in the same manner as in Example 10 except that the compound represented by the formula (21) and the compound represented by the formula (22) were used instead of the compound represented by the formula (1).
[0563] The surface treatment liquids prepared above were subjected to an adhesiveness evaluation test (i).
[0564]
[0565] From the results in Table 2, it is understood that even when a mixed solution of acetic acid and methanol is used as a solubilizing agent, the surface treatment liquid of the present invention (surface treatment liquids of Examples 10 to 11) has higher peel strength than that of Comparative Examples 4 to 6.
[0566] <Adhesion Test 3>
[0567] The surface treatment liquids prepared in the following Example 12 and Comparative Example 7 were evaluated for the following adhesiveness.
[0568] [Evaluation test of adhesiveness (ii)]
[0569] (1) Metal
[0570] As the metal, an electrolytic copper foil (thickness: 35 μm) was used.
[0571] (2) Surface treatment of metal
[0572] The copper foil was treated according to the following steps a and b.
[0573] a. Acid cleaning (5% sulfuric acid aqueous solution) / 1 minute (room temperature), water washing
[0574] b. Apply the surface treatment liquid and dry for 1 minute (100℃)
[0575] (3) Adhesion between metal and resin
[0576] A build-up wiring board resin (GX-T31 (manufactured by Ajinomoto Fine Technologies Co., Ltd.) was laminated and pressed on the S surface of the treated copper foil to prepare a copper-clad laminate.
[0577] (4) Evaluation of Adhesion
[0578] The copper-clad laminate was subjected to reflow heating once (peak temperature 250° C., air), and then a test piece having a width of 10 mm was prepared according to “JIS C6481 (1996)” and the peel strength (peel strength (kN / m)) of the copper foil was measured.
[0579] [Example 12]
[0580] To 1 g of the compound represented by the formula (1) as a coupling agent component, 99 g of a 9:90 mixed solution (weight ratio) of 11% acetic acid water and methanol was added, and the mixture was stirred at room temperature for 1 hour to prepare a surface treatment solution.
[0581] [Comparative Example 7]
[0582] The copper foil subjected to only the step (2) a. of the adhesion evaluation test (ii) was subjected to the adhesion evaluation test (ii).
[0583] The surface treatment liquids prepared above were subjected to an adhesiveness evaluation test (ii). The obtained test results are shown in Table 3.
[0584]
[0585] As can be seen from the results in Table 3, the surface treatment liquid of the present invention (surface treatment liquid of Example 12) has higher peel strength than that of Comparative Example 7, and is excellent in adhesion between metal and resin.
[0586] Although the present invention is described in detail with reference to specific embodiments, it is apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention. This application is based on Japanese patent application (Japanese patent application 2022-054330) filed on March 29, 2022, the contents of which are incorporated herein by reference.
[0587] Industrial Applicability
[0588] The triazole compound of the present invention can be used as a coupling agent having the function of preventing metal from rusting and curing epoxy resin and polyurethane resin, which are the characteristics of triazole compounds, and is therefore expected to be used in composite materials such as printed wiring boards produced by combining a large number of different raw materials.
[0589] In addition, according to the present invention, since the adhesiveness (adhesion) of metals, inorganic materials and resin materials can be improved, a smooth state can be maintained without roughening the surface of the substrate. Therefore, the present invention can make a great contribution to the realization of miniaturization, thinning, high frequency, high density, etc. of multilayer printed wiring boards, and thus has great industrial practicality.
Claims
1. A triazole compound represented by the following chemical formula (I): In formula (I), R1 and R2 are the same or different and represent a hydrogen atom, a linear or branched alkyl group having 1 to 6 carbon atoms, an aryl group, an aralkyl group, an amino group, a hydroxyl group, or an alkylthio group having 1 to 6 carbon atoms, R3 and R4 are the same or different and represent a hydrogen atom or -(CH2) m -Si(OR)3, wherein R represents a methyl group or an ethyl group, and m represents an integer from 1 to 18, wherein Except when both R3 and R4 are hydrogen atoms, X represents phenylene, -NH- or -(CH2) n -, wherein n represents an integer of 0 to 12.
2. The method for synthesizing a triazole compound according to claim 1, wherein A triazole compound represented by the following chemical formula (II) is reacted with a compound represented by the following chemical formula (III), In formula (II), R1, R2 and X are the same as above, In the formula (III), R and m are the same as described above, and Hal represents a chlorine atom, a bromine atom or an iodine atom.
3. A coupling agent comprising a triazole compound represented by the following chemical formula (IV) as a component, In formula (IV), R1 and R2 are the same or different and represent a hydrogen atom, a linear or branched alkyl group having 1 to 6 carbon atoms, an aryl group, an aralkyl group, an amino group, a hydroxyl group, or an alkylthio group having 1 to 6 carbon atoms, R5 and R6 are the same or different and represent a hydrogen atom or -(CH2) m -Si(OR) 3-p (OH) p A group represented by, wherein R represents a methyl group or an ethyl group, m represents an integer of 1 to 18, and p represents an integer of 0 to 3, X represents phenylene, -NH- or -(CH2) n -, wherein n represents an integer of 0 to 12.
4. A surface treatment liquid comprising a triazole compound represented by the following chemical formula (IV), In formula (IV), R1 and R2 are the same or different and represent a hydrogen atom, a linear or branched alkyl group having 1 to 6 carbon atoms, an aryl group, an aralkyl group, an amino group, a hydroxyl group, or an alkylthio group having 1 to 6 carbon atoms, R5 and R6 are the same or different and represent a hydrogen atom or -(CH2) m-Si(OR) 3-p (OH) p A group represented by, wherein R represents a methyl group or an ethyl group, m represents an integer of 1 to 18, and p represents an integer of 0 to 3, X represents phenylene, -NH- or -(CH2) n -, wherein n represents an integer of 0 to 12.
5. The surface treatment liquid according to claim 4, wherein The surface treatment liquid is used to treat the surface of at least one selected from the group consisting of metal, inorganic material and resin material.
6. The surface treatment liquid according to claim 4, wherein The surface treatment liquid is used to bond two materials selected from the group consisting of metals, inorganic materials, and resin materials.
7. The surface treatment liquid according to claim 5 or claim 6, wherein: The metal is at least one selected from the group consisting of copper, aluminum, titanium, nickel, tin, iron, silver, gold, and alloys thereof. 8 . A surface treatment method, comprising bringing the surface treatment liquid according to claim 4 into contact with a surface of at least one selected from the group consisting of metals, inorganic materials, and resin materials.
9. The surface treatment method according to claim 8, wherein: The metal is at least one selected from the group consisting of copper, aluminum, titanium, nickel, tin, iron, silver, gold, and alloys thereof.
10. The surface treatment method according to claim 9, wherein: The metal is copper or a copper alloy.
11. The surface treatment method according to claim 10, wherein: Before bringing the surface treatment liquid into contact with the surface of copper or the copper alloy, an aqueous solution containing copper ions is brought into contact with the surface of the copper or the copper alloy.
12. The surface treatment method according to claim 10 or claim 11, wherein: After the surface treatment liquid is brought into contact with the surface of copper or the copper alloy, an acidic aqueous solution or an alkaline aqueous solution is brought into contact with the surface of the copper or the copper alloy.
13. A gluing method, wherein: The surface treatment liquid according to claim 4 is brought into contact with at least one selected from the group consisting of metals, inorganic materials, and resin materials to form a conversion film on the at least one material, and the two materials are bonded to each other via the conversion film.
14. A method for bonding metal to resin material, wherein: The surface treatment liquid according to claim 4 is brought into contact with at least one of a metal and a resin material to form a conversion film on the at least one, and the metal and the resin material are bonded to each other via the conversion film. 15 . A printed wiring board obtained by bonding two materials selected from the group consisting of metals, inorganic materials and resin materials via a conversion film formed from the surface treatment liquid according to claim 4 . 16 . A semiconductor wafer obtained by bonding two materials selected from the group consisting of metals, inorganic materials and resin materials via a conversion film formed using the surface treatment solution according to claim 4 .
17. An insulating composition comprising: The coupling agent according to claim 3, and Resin material or inorganic material.
18. An insulating material comprising the insulating composition according to claim 17.
19. A printed wiring board comprising an insulating layer obtained from the insulating composition according to claim 17.
20. A semiconductor wafer comprising an insulating layer obtained from the insulating composition according to claim 17.