Composition and crosslinked material
By co-precipitating perfluoroelastomers with polytetrafluoroethylene and using inorganic acid precipitants, a crosslinked material that is not easily broken at high temperatures and has excellent plasma resistance and compression set properties was prepared. This solves the problem of the difficulty in preparing such materials in the prior art and is suitable for sealing materials in semiconductor manufacturing equipment.
Patent Information
- Application Number
- CN202380029375.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-06
- Filing Date
- 2023-04-05
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-04-05
AI Technical Summary
Existing technologies make it difficult to prepare perfluoroelastomer crosslinks that are not easily broken and have excellent plasma resistance and compression set properties at high temperatures.
By co-precipitating perfluoroelastomer with polytetrafluoroethylene (PTFE), selecting appropriate PTFE melt viscosity and melting point range, and using inorganic acid as a precipitant during the crosslinking process, a composition with excellent plasma resistance and compression set properties was prepared.
A crosslinked compound that is not easily broken at high temperatures, has excellent plasma resistance and compression set properties, is suitable for sealing materials in semiconductor manufacturing equipment.
Smart Images

Figure BDA0005054159630000051 
Figure BDA0005054159630000171 
Figure BDA0005054159630000172
Abstract
Description
Technical Field
[0001] The present invention relates to compositions and cross-linked products. Background Art
[0002] Conventionally, in order to improve the physical properties of perfluoroelastomer, a technique of adding fluororesin to perfluoroelastomer is known.
[0003] For example, Patent Document 1 describes a composition comprising fluoroplastic particles having an average particle size of less than 500 nm and an amorphous fluoropolymer.
[0004] Patent document 2 describes a fluorine-based composition for sealing materials, which is obtained by adding an inorganic acid solution to a mixed solution prepared by mixing a suspension of a fluorine-based elastomer and a suspension of a fluorine-based resin in a mass mixing ratio of the fluorine-based elastomer to the fluorine-based resin in the range of 95:5 to 5:95, and subjecting the mixture to co-precipitation.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application No. 2018-531316
[0008] Patent Document 2: Japanese Patent Application Publication No. 2003-26811 Summary of the invention
[0009] Problems to be solved by the invention
[0010] An object of the present invention is to provide a composition which can produce a cross-linked product which is not easily cracked even when compressed at high temperatures and has excellent plasma resistance and excellent compression set characteristics.
[0011] Means for solving problems
[0012] According to the present invention, there is provided a composition comprising a perfluoroelastomer and polytetrafluoroethylene, wherein the melt viscosity of the polytetrafluoroethylene is 1.0×10 3 Mooring ~7.0×10 6 The melting point of the polytetrafluoroethylene is above 322° C., and the composition is obtained by co-precipitating the perfluoroelastomer and the polytetrafluoroethylene.
[0013] Effects of the Invention
[0014] According to the present invention, there can be provided a composition capable of obtaining a cross-linked product which is not easily broken even when compressed at high temperatures and has excellent plasma resistance and excellent compression set characteristics. DETAILED DESCRIPTION
[0015] Hereinafter, specific embodiments of the present invention will be described in detail, but the present invention is not limited to the following embodiments.
[0016] The composition of the present invention contains a perfluoroelastomer and polytetrafluoroethylene (PTFE).
[0017] The prior art of adding fluoroplastics and fluorine-based resins to perfluoroelastomers has advantages such as less generation of particles compared to the art of adding fillers such as inorganic particles to perfluoroelastomers. However, there is a need for a perfluoroelastomer composition that can produce a cross-linked product having excellent plasma resistance, which is less likely to break even when compressed at high temperatures, and which easily recovers its shape after being released from compression.
[0018] The present inventor has found that by selecting PTFE as fluororesin, and then appropriately selecting the melt viscosity and fusing point of PTFE, and selecting a method for coprecipitating perfluoroelastomer and PTFE as a method for preparing a composition, the crosslinked product obtained by crosslinking such a composition is also not easy to break even if compressed at high temperature, and has excellent plasma resistance and excellent compression set characteristics, thereby completing the composition of the present invention.
[0019] (PTFE)
[0020] The melt viscosity of PTFE contained in the composition of the present invention is 1.0×10 3 Mooring ~7.0×10 6 The melt viscosity is preferably 1.0×10 4 poise or more, more preferably 1.0×10 5 Poise or more, preferably 5.0×10 6 Poise or less, more preferably 3.0×10 6 Poise or less, more preferably 1.0×10 6 Below the moor.
[0021] By using PTFE having a melt viscosity within the above range, when the composition is cross-linked, a cross-linked product having excellent plasma resistance and excellent compression set characteristics can be obtained. When the melt viscosity of PTFE is too high, the compression set characteristics of the cross-linked product cannot be fully improved. For example, when the cross-linked product is compressed for a long time at a high temperature of about 300°C, the cross-linked product may be crushed due to compression, or the shape of the cross-linked product may be difficult to restore. PTFE with too low a melt viscosity may produce high-temperature volatile components, and therefore is sometimes not suitable for use in cross-linked products used at high temperatures (e.g., about 300°C).
[0022] The molecular weight of the PTFE with melt viscosity in the above-mentioned scope is low, for example, the PTFE with number average molecular weight of less than 600,000. " High molecular weight PTFE " with number average molecular weight exceeding 600,000 shows the unique fibrillation characteristic of PTFE (for example, with reference to Japanese Patent Publication No. 10-147617). The melt viscosity of high molecular weight PTFE is high, which is non-melt processability. The PTFE contained in the composition of the present invention preferably does not show the fibrillation characteristic of the degree that can carry out paste extrusion molding. The melt viscosity and number average molecular weight of PTFE can be adjusted by adjusting the polymerization conditions of TFE when manufacturing PTFE or irradiating PTFE with electron beams.
[0023] Melt viscosity was measured using a flow tester (manufactured by Shimadzu Corporation) according to ASTM D 1238. The value is measured by holding a 2 g sample heated in advance at 380° C. for 5 minutes at the above temperature under a load of 0.7 MPa using a die. The number average molecular weight can be calculated from the melt viscosity measured by the above measurement method.
[0024] The melting point of PTFE contained in the composition of the present invention is 322° C. or higher, preferably 323° C. or higher, more preferably 324° C. or higher, further preferably 325° C. or higher, preferably 333° C. or lower, more preferably 332° C. or lower, further preferably 330° C. or lower.
[0025] If the melting point of PTFE is too low, the compression set characteristics of the cross-linked product cannot be sufficiently improved. For example, when the cross-linked product is compressed for a long time at a high temperature of about 300°C, PTFE melts, and the shape of the cross-linked product is difficult to restore.
[0026] The melting point of PTFE can be measured as follows: using a differential scanning calorimeter X-DSC7000 (DSC) manufactured by Hitachi High-Technologies Corporation, about 3 mg of PTFE that has not been heated to a temperature of 300°C or above after temperature correction using indium and lead as a standard sample is placed in an aluminum pan, and the temperature is raised at 10°C / min in a temperature range of 230°C to 350°C under a nitrogen gas flow of 40 ml / min, and differential scanning calorimetry is performed, and the temperature corresponding to the minimum point of the melting curve in the above-mentioned range is measured as the melting point.
[0027] The specific surface area of PTFE is preferably 0.5 m 2 / g~20m 2 The specific surface area was measured by the BET method using a surface analyzer (trade name: BELSORP-miniII, manufactured by Microtrac BEL) using a mixed gas of 30% nitrogen and 70% helium as a carrier gas and liquid nitrogen for cooling.
[0028] The average primary particle size of PTFE is preferably 10 nm to 1000 μm, more preferably 100 nm or more, further preferably 200 nm or more, more preferably 100 μm or less, further preferably 10 μm or less, particularly preferably 1 μm or less, and particularly preferably 500 nm or less.
[0029] The average primary particle size is calculated as follows: after determining the correlation between the transmittance when 550nm light is incident on a specified unit injected with a PTFE aqueous dispersion adjusted to a solid content of 0.15% by mass and the number average primary particle size calculated by measuring the oriented diameter using a transmission electron microscope photograph, the transmittance measured on the obtained sample is substituted into the above correlation to thereby calculate the average primary particle size (standard curve method).
[0030] PTFE can be a homopolymer of tetrafluoroethylene (TFE), or a modified PTFE comprising a TFE unit and a modified monomer unit copolymerizable with TFE. As PTFE, from the aspect of further improving the compression set characteristics of the crosslinked product, a PTFE comprising a TFE unit and a modified monomer unit copolymerizable with TFE is preferred.
[0031] The content of the modified monomer unit of PTFE is 0 mol% to 0.10 mol% based on all monomer units, more preferably 0.02 mol% or more, further preferably 0.05 mol% or more, and more preferably 0.09 mol% or less.
[0032] In the present invention, the modified monomer unit refers to a part of the molecular structure of PTFE and derived from the modified monomer, and the total monomer unit refers to the part derived from all monomers in the molecular structure of PTFE. The content of the modified monomer unit is a value measured by infrared spectroscopy or NMR (nuclear magnetic resonance).
[0033] The modifying monomer in the modified PTFE is not particularly limited as long as it can be copolymerized with TFE, and examples thereof include perfluoroolefins such as hexafluoropropylene [HFP]; fluorochloroolefins such as trifluorochloroethylene [CTFE]; hydrogen-containing fluoroolefins such as trifluoroethylene and vinylidene fluoride [VDF]; perfluorovinyl ether; perfluoroalkylethylene: ethylene, etc. In addition, the modifying monomer used may be one or more.
[0034] The perfluorovinyl ether is not particularly limited, and examples thereof include those of the general formula (I):
[0035] CF 2 =CF-ORf(I)
[0036] (wherein Rf represents a perfluoro organic group) and the like. In this specification, the above-mentioned "perfluoro organic group" refers to an organic group in which all hydrogen atoms bonded to carbon atoms are replaced by fluorine atoms. The above-mentioned perfluoro organic group may have an ether oxygen.
[0037] Examples of the perfluorovinyl ether include perfluoro(alkyl vinyl ether) [PAVE] wherein Rf in the general formula (I) represents a perfluoroalkyl group having 1 to 10 carbon atoms. The perfluoroalkyl group preferably has 1 to 5 carbon atoms.
[0038] Examples of the perfluoroalkyl group in the above-mentioned PAVE include perfluoromethyl, perfluoroethyl, perfluoropropyl, perfluorobutyl, perfluoropentyl, and perfluorohexyl. Preferably, the perfluoroalkyl group is perfluoromethyl vinyl ether [PMVE] in which the perfluoroalkyl group is a perfluoromethyl group, or perfluoropropyl vinyl ether [PPVE] in which the perfluoroalkyl group is a perfluoropropyl group.
[0039] Examples of the perfluorovinyl ether include:
[0040] In the general formula (I), Rf is a perfluoro(alkoxyalkyl) group having 4 to 9 carbon atoms, and Rf is the following formula:
[0041] [Chemistry 1]
[0042]
[0043] (wherein m represents 0 or an integer of 1 to 4), and Rf is the following formula:
[0044] CF 3 CF 2 CF 2 -(O-CF(CF 3 )-CF 2 ) n -
[0045] (wherein n represents an integer of 1 to 4) and the like.
[0046] The perfluoroalkylethylene is not particularly limited, and examples thereof include perfluorobutylethylene (PFBE), perfluorohexylethylene, and perfluorooctylethylene.
[0047] As the modifying monomer in the modified PTFE, at least one monomer selected from the group consisting of HFP, CTFE, VDF, perfluorovinyl ether, PFBE and ethylene is preferred, at least one monomer selected from the group consisting of HFP and perfluorovinyl ether is more preferred, and at least one monomer selected from the group consisting of HFP, PMVE and PPVE is further preferred.
[0048] From the perspective of obtaining a cross-linked product having better plasma resistance and better compression set characteristics, the content of PTFE in the composition is preferably 1 to 100 parts by mass, more preferably 5 parts by mass or more, further preferably 10 parts by mass or more, particularly preferably 15 parts by mass or more, more preferably 70 parts by mass or less, further preferably 60 parts by mass or less, based on 100 parts by mass of the perfluoroelastomer. From the perspective of obtaining a cross-linked product having better compression set characteristics, the content of PTFE in the composition is further preferably 55 parts by mass or less, particularly preferably 50 parts by mass or less.
[0049] (Perfluoroelastomer)
[0050] The composition of the present invention contains a perfluoroelastomer. Since the composition of the present invention contains a perfluoroelastomer as a fluororubber, when the composition is crosslinked, a crosslinked product having excellent plasma resistance and excellent compression set characteristics can be obtained.
[0051] In the present invention, the perfluoroelastomer refers to a fluoropolymer in which the content of perfluoro monomer units relative to all monomer units is 90 mol% or more, preferably 91 mol% or more, has a glass transition temperature of 20°C or less, has a melting peak (ΔH) of 4.5 J / g or less, and further, is a polymer in which the concentration of fluorine atoms contained in the fluoropolymer is 71 mass% or more, preferably 71.5 mass% or more. In the present invention, the concentration of fluorine atoms contained in the fluoropolymer is obtained by calculating the concentration (mass%) of fluorine atoms contained in the fluoropolymer based on the type and content of each monomer constituting the fluoropolymer.
[0052] In the present invention, a perfluoromonomer refers to a monomer that does not contain a carbon atom-hydrogen atom bond in the molecule. The perfluoromonomer may be a monomer in which, in addition to carbon atoms and fluorine atoms, a number of fluorine atoms bonded to carbon atoms are replaced by chlorine atoms, or a monomer having nitrogen atoms, oxygen atoms, sulfur atoms, phosphorus atoms, boron atoms or silicon atoms in addition to carbon atoms. As the perfluoromonomer, a monomer in which all hydrogen atoms are replaced by fluorine atoms is preferred. The perfluoromonomer does not contain a monomer that provides a crosslinking site.
[0053] The monomer providing a crosslinking site refers to a monomer having a crosslinkable group that provides a crosslinking site for forming a crosslink with a curing agent to the fluoropolymer (curing site monomer).
[0054] In the present invention, the content of each monomer constituting the perfluoroelastomer can be calculated by appropriately combining NMR, FT-IR, elemental analysis, fluorescent X-ray analysis, and other known methods according to the types of monomers.
[0055] The perfluoromonomer providing the perfluoromonomer units constituting the perfluoroelastomer is preferably selected from
[0056] Tetrafluoroethylene [TFE],
[0057] Hexafluoropropylene [HFP],
[0058] General formula (13): CF 2 =CF-ORf 13
[0059] (Where Rf 13 represents a perfluoroalkyl group having 1 to 8 carbon atoms),
[0060] General formula (14): CF 2 =CFOCF 2 O 14
[0061] (Where Rf 14 a fluorinated monomer represented by a linear or branched perfluoroalkyl group having 1 to 6 carbon atoms, a cyclic perfluoroalkyl group having 5 to 6 carbon atoms, or a linear or branched perfluorooxyalkyl group having 2 to 6 carbon atoms containing 1 to 3 oxygen atoms, and
[0062] General formula (15): CF 2 =CFO(CF 2 CF(Y 15 )O) m (CF 2 ) n F
[0063] (In the formula, Y 15 represents a fluorine atom or a trifluoromethyl group. m is an integer of 1 to 4. n is an integer of 1 to 4) is at least one of the group consisting of fluorinated monomers represented by.
[0064] The perfluoroelastomer is preferably a perfluoroelastomer containing TFE units, for example, preferably at least one selected from the group consisting of a copolymer of TFE / a fluorinated monomer represented by the general formula (13), (14) or (15) and a copolymer of TFE / a fluorinated monomer represented by the general formula (13), (14) or (15) / a monomer providing a crosslinking site.
[0065] Regarding the composition, in the case of TFE / perfluoro(methyl vinyl ether) (PMVE) copolymer, it is preferably 45 to 90 / 10 to 55 (mol %), more preferably 55 to 80 / 20 to 45, further preferably 55 to 70 / 30 to 45, and most preferably 56 to 69.5 / 30.5 to 44.
[0066] In the case of a copolymer of TFE / PMVE / a monomer providing a cross-linking site, the ratio is preferably 45-89.9 / 10-54.9 / 0.01-4 (mol %), more preferably 55-77.9 / 20-49.9 / 0.1-3.5, further preferably 55-69.8 / 30-44.8 / 0.2-3, and most preferably 55.3-69.5 / 30.3-44.5 / 0.2-2.8.
[0067] In the case of a copolymer of TFE / a fluorinated monomer represented by the general formula (13), (14) or (15) having 4 to 12 carbon atoms, the ratio is preferably 50 to 90 / 10 to 50 (mol %), more preferably 60 to 88 / 12 to 40, further preferably 65 to 85 / 15 to 35, and most preferably 66 to 84 / 16 to 34.
[0068] In the case of a copolymer of TFE / a fluorinated monomer represented by the general formula (13), (14) or (15) having 4 to 12 carbon atoms / a monomer providing a crosslinking site, the ratio is preferably 50 to 89.9 / 10 to 49.9 / 0.01 to 4 (mol %), more preferably 60 to 87.9 / 12 to 39.9 / 0.1 to 3.5, further preferably 65 to 84.8 / 15 to 34.8 / 0.2 to 3, and most preferably 66 to 84.3 / 15.5 to 33.8 / 0.2 to 2.8.
[0069] Outside this composition range, the properties as a rubber elastic body are lost and the properties close to those of a resin tend to be exhibited.
[0070] The perfluoroelastomer is preferably at least one selected from the group consisting of a copolymer of TFE / fluorinated monomer represented by the general formula (15) / a monomer providing a cross-linking site, a copolymer of TFE / fluorinated monomer represented by the general formula (15), a copolymer of TFE / fluorinated monomer represented by the general formula (13), and a copolymer of TFE / fluorinated monomer represented by the general formula (13) / a monomer providing a cross-linking site.
[0071] Examples of the perfluoroelastomer include perfluoroelastomers described in International Publication No. 97 / 24381, Japanese Examined Patent Publication No. 61-57324, Japanese Examined Patent Publication No. 4-81608, Japanese Examined Patent Publication No. 5-13961, and the like.
[0072] The monomer providing a crosslinking site refers to a monomer having a crosslinkable group that provides a crosslinking site for forming a crosslink with a crosslinking agent to the perfluoroelastomer (curing site monomer).
[0073] Examples of the monomer providing a crosslinking site include
[0074] General formula (16): CX 42 =CX 5 R f 2 X 6
[0075] (Where X 4 , X 5 Each independently represents H, F or an alkyl group having 1 to 5 carbon atoms, Rf 2 is a linear or branched alkylene or oxyalkylene group which may have one or more ether-bonded oxygen atoms, may have an aromatic ring, and may have a part or all of hydrogen atoms substituted by fluorine atoms, X 6 The monomer is represented by an iodine atom, a bromine atom, a nitrile group, a carboxyl group, an alkoxycarbonyl group, a hydroxyl group, a vinyl group, an azido group, a sulfonylazido group, a carbonylazido group or an alkynyl group. The alkynyl group may be an ethynyl group.
[0076] As the monomer providing a crosslinking site, preferably selected from the group consisting of
[0077] General formula (17): CX 16 2 =CX 16 -Rf 16 CHR 16 X 17
[0078] (Where X 16 are each independently a hydrogen atom, a fluorine atom or CH 3 , Rf 16 is a fluoroalkylene group, a perfluoroalkylene group, a fluoro(poly)oxyalkylene group or a perfluoro(poly)oxyalkylene group, R 16 A hydrogen atom or CH 3 , X 17 is an iodine atom or a bromine atom),
[0079] General formula (18): CX 16 2 =CX 16 -Rf 17 X 17
[0080] (Where X 16 are each independently a hydrogen atom, a fluorine atom or CH 3 , Rf 17 is a fluoroalkylene group, a perfluoroalkylene group, a fluoro(poly)oxyalkylene group or a perfluoro(poly)oxyalkylene group, X 17 is an iodine atom or a bromine atom),
[0081] General formula (19): CF 2 =CFO(CF 2 CF(CF3 )O) m (CF 2 ) n -X 18
[0082] (wherein, m is an integer from 0 to 5, n is an integer from 1 to 3, and X 18 is a cyano group, an azido group, a sulfonylazido group, a carbonylazido group, a carboxyl group, an alkoxycarbonyl group, an alkynyl group, an iodine atom, a bromine atom or a CH 2 I) the fluorine-containing monomer,
[0083] General formula (20): CH 2 =CFCF 2 O(CF(CF 3 )CF 2 O) m (CF(CF 3 )) n -X 19
[0084] (wherein, m is an integer from 0 to 5, n is an integer from 1 to 3, and X 19 is a cyano group, a carboxyl group, an alkoxycarbonyl group, an iodine atom, a bromine atom, or CH 2 OH) and
[0085] General formula (21): CR 20 2 =CR 20 -Z-CR 20 =CR 20 2
[0086] (Where R 20 Each is independently a hydrogen atom or an alkyl group having 1 to 5 carbon atoms. Z is a linear or branched alkylene group having 1 to 18 carbon atoms, a cycloalkylene group having 3 to 18 carbon atoms, an at least partially fluorinated alkylene group having 1 to 10 carbon atoms, or an oxyalkylene group having 1 to 10 carbon atoms, which may or may not have an oxygen atom.
[0087] -(Q) p -CF 2 O-(CF 2 CF 2 O) m (CF 2 O) n -CF 2 -(Q) p -
[0088] (wherein, Q is an alkylene group or an oxyalkylene group. p is 0 or 1. m / n is 0.2 to 5) and a (per)fluoropolyoxyalkylene group having a molecular weight of 500 to 10000) is a monomer.
[0089] X 16 It is preferably a fluorine atom. 16 and Rf 17 It is preferably a perfluoroalkylene group having 1 to 5 carbon atoms. 16 Preferably, it is a hydrogen atom. 18 Preferably, it is a cyano group, an alkoxycarbonyl group, an iodine atom, a bromine atom or a -CH 2 I. X 19 Preferably, it is a cyano group, an alkoxycarbonyl group, an iodine atom, a bromine atom or a -CH 2 OH.
[0090] As the monomer providing a crosslinking site, it is preferably selected from the group consisting of CF 2 =CFOCF 2 CF(CF 3 )OCF 2 CF 2 CN、CF 2 =CFOCF 2 CF(CF 3 )OCF 2 CF 2 COOH、CF 2 =CFOCF 2 CF(CF 3 )OCF 2 CF 2 CH 2 I. CF 2 =CFOCF 2 CF 2 CH 2 I. CH 2 =CFCF 2 OCF(CF 3 )CF 2 OCF(CF 3 )CN、CH 2 =CFCF 2 OCF(CF 3 )CF 2 OCF(CF 3 )COOH、CH 2 =CFCF 2 OCF(CF 3 )CF 2 OCF(CF 3 )CH 2 OH, CH 2 =CHCF 2 CF2 I. CH 2 =CH(CF 2 ) 2 CH=CH 2 , CH 2 =CH(CF 2 ) 6 CH=CH 2 CF 2 =CFO(CF 2 ) 3 CN and CF 2 =CFO(CF 2 ) 5 At least one selected from the group consisting of CN, more preferably CF 2 =CFOCF 2 CF(CF 3 )OCF 2 CF 2 CN、CF 2 =CFO(CF 2 ) 5 CN and CF 2 =CFOCF 2 CF 2 CH 2 At least one of the group consisting of I.
[0091] The glass transition temperature of the perfluoroelastomer is preferably -30°C or higher, more preferably -20°C or higher, and further preferably -10°C or higher, from the perspective of excellent compression set characteristics at high temperatures. In addition, from the perspective of good cold resistance, it is preferably 10°C or lower, more preferably 5°C or lower, and further preferably 0°C or lower.
[0092] The above-mentioned glass transition temperature can be calculated as follows: using a differential scanning calorimeter (manufactured by Hitachi High-Technologies Corporation, X-DSC7000), 3 mg of the sample is heated at 10°C / min to obtain a DSC curve, and the temperature of the midpoint of the two intersections of the extended line of the baseline before and after the secondary phase transition of the DSC curve and the tangent line at the inflection point of the DSC curve is calculated, and the midpoint is taken as the above-mentioned glass transition temperature.
[0093] For the perfluoroelastomer, from the viewpoint of good heat resistance, the Mooney viscosity ML (1+20) at 170°C is preferably 30 or more, more preferably 40 or more, and further preferably 50 or more. From the viewpoint of good processability, it is preferably 100 or less, more preferably 90 or less, and further preferably 80 or less.
[0094] The Mooney viscosity can be measured at 170° C. in accordance with JIS K6300 using a Mooney viscometer MV2000E manufactured by ALPHATECHNOLOGIES.
[0095] Perfluoroelastomer can be manufactured by conventional methods, but from the aspects of narrow molecular weight distribution of the obtained polymer, easy control of molecular weight, and ability to introduce iodine atoms or bromine atoms to the terminal, iodine compounds or bromine compounds can also be used as chain transfer agents. As a polymerization method using iodine compounds or bromine compounds, for example, a method of emulsification polymerization in an aqueous medium under pressure in the presence of iodine compounds or bromine compounds in a substantially oxygen-free state (iodine transfer polymerization method) can be cited. As a representative example of the iodine compounds or bromine compounds used, for example, the general formula can be cited:
[0096] R 21 I x Br y
[0097] (where x and y are integers from 0 to 2 and satisfy 1≤x+y≤2, R 21 is a saturated or unsaturated fluorocarbon or chlorofluorocarbon group having 1 to 16 carbon atoms, or a hydrocarbon group having 1 to 3 carbon atoms, wherein R 21 By using an iodine compound or a bromine compound, an iodine atom or a bromine atom is introduced into the polymer to function as a crosslinking point.
[0098] Examples of the iodine compound and the bromine compound include 1,3-diiodoperfluoropropane, 2-iodoperfluoropropane, 1,3-diiodoperfluoropropane, 1,4-diiodoperfluorobutane, 1,5-diiodoperfluoropentane, 1,6-diiodoperfluorohexane, 1,8-diiodoperfluorooctane, 1,12-diiodoperfluorododecane, 1,16-diiodoperfluorohexadecane, diiodomethane, 1,2-diiodoethane, 1,3-diiodoperfluoropropane, CF 2 Br 2 BrCF 2 CF 2 Br, CF 3 CFC 2 Br, CFClBr 2 BrCF 2 CFClBr, CFBrClCFClBr, BrCF 2 CF 2 CF 2 Br, BrCF 2 CFB 3, 1-bromo-2-iodoperfluoroethane, 1-bromo-3-iodoperfluoropropane, 1-bromo-4-iodoperfluorobutane, 2-bromo-3-iodoperfluorobutane, 3-bromo-4-iodoperfluoro-1-butene, 2-bromo-4-iodoperfluoro-1-butene, mono-iodine-mono-bromine substituted bodies, di-iodine-mono-bromine substituted bodies, and (2-iodoethyl) and (2-bromoethyl) substituted bodies of benzene, etc. These compounds can be used alone or in combination with each other.
[0099] Among these, 1,4-diiodoperfluorobutane, 1,6-diiodoperfluorohexane, and 2-iodoperfluoropropane are preferably used in view of polymerization reactivity, crosslinking reactivity, and availability.
[0100] The perfluoroelastomer preferably has a cyano group (-CN group). The perfluoroelastomer having a cyano group (-CN group) is a perfluoroelastomer formed by crosslinking by forming a triazine ring through cyclotrimerization of the cyano group, or by forming an imidazole ring through crosslinking by using a tetraamine compound as a crosslinking agent, and can impart excellent compression set characteristics and heat resistance to the crosslinked product.
[0101] The above-mentioned perfluoroelastomer having a cyano group preferably has a cyano group (—CN group) at the main chain terminal and / or a side chain.
[0102] As a perfluoroelastomer having a cyano group (-CN group) at the main chain terminal and / or side chain, there can be mentioned a copolymer in which the monomer providing a crosslinking site is a monomer having a cyano group (-CN group) among the above-mentioned TFE / fluorine-containing monomers represented by the general formula (13), (14) or (15) / monomers providing a crosslinking site copolymers. In this case, from the perspective of good crosslinking characteristics and heat resistance, the content of the monomer units having a cyano group (-CN group) can be 0.1 mol% to 5 mol%, or 0.3 mol% to 3 mol% relative to the total amount of the TFE units and the fluorine-containing monomer units represented by the general formula (13), (14) and (15). The more preferred composition is as described above.
[0103] In addition, examples of the monomer having a cyano group (-CN group) include:
[0104] Formula: CY 1 2 =CY 1 (CF 2 ) n -CN
[0105] (In the formula, Y 1 are each independently a hydrogen atom or a fluorine atom, and n is an integer of 1 to 8)
[0106] Formula: CF 2 =CFCF 2 R 8 -CN
[0107] (Where Rf 8 OCF 2 ) n -or-(OCF(CF 3 )) n -, n is an integer from 0 to 5)
[0108] Formula: CF 2 =CFCF 2 (OCF(CF 3 )CF 2 ) m (OCH 2 CF 2 CF 2 ) n OCH 2 CF 2 -CN
[0109] (wherein m is an integer from 0 to 5, and n is an integer from 0 to 5)
[0110] Formula: CF 2 =CFCF 2 (OCH 2 CF 2 CF 2 ) m (OCF(CF 3 )CF 2 ) n OCF(CF 3 )-CN
[0111] (wherein m is an integer from 0 to 5, and n is an integer from 0 to 5)
[0112] Formula: CF 2 =CF(OCF 2 CF(CF 3 )) m O(CF 2 ) n -CN
[0113] (wherein m is an integer from 0 to 5, and n is an integer from 1 to 8)
[0114] Formula: CF 2 =CF(OCF 2 CF(CF 3 )) m -CN
[0115] (wherein m is an integer from 1 to 5)
[0116] Formula: CF 2 =CFOCF 2 (CF(CF3 )OCF 2 ) n CF(-CN)CF 3
[0117] (where n is an integer from 1 to 4)
[0118] Formula: CF 2 =CFO(CF 2 ) n OCF(CF 3 )-CN
[0119] (where n is an integer from 2 to 5)
[0120] Formula: CF 2 =CFO(CF 2 ) n -(C 6 H 4 )-CN
[0121] (where n is an integer from 1 to 6)
[0122] Formula: CF 2 =CF(OCF 2 CF(CF 3 )) n OCF 2 CF(CF 3 )-CN
[0123] (where n is an integer from 1 to 2)
[0124] Formula: CH 2 =CFCF 2 O(CF(CF 3 )CF 2 O) n CF(CF 3 )-CN
[0125] (where n is an integer from 0 to 5)
[0126] Formula: CF 2 =CFO(CF 2 CF(CF 3 )O) m (CF 2 ) n -CN
[0127] (wherein m is an integer from 0 to 5, and n is an integer from 1 to 3)
[0128] Formula: CH 2 =CFCF 2 OCF(CF 3)OCF(CF 3 )-CN
[0129] Formula: CH 2 =CFCF 2 OCH 2 CF 2 -CN
[0130] Formula: CF 2 =CFO(CF 2 CF(CF 3 )O) m CF 2 CF(CF 3 )-CN
[0131] (wherein m is an integer greater than 0)
[0132] Formula: CF 2 =CFOCF(CF 3 )CF 2 O(CF 2 ) n -CN
[0133] (where n is an integer greater than 1)
[0134] Formula: CF 2 =CFOCF 2 OCF 2 CF(CF 3 )OCF 2 -CN
[0135] Formula: CF 2 =CFO(CF 2 ) 3 CN
[0136] Formula: CF 2 =CFO(CF 2 ) 5 CN
[0137] The monomers shown above can be used alone or in any combination.
[0138] Among the above, preferably
[0139] Formula: CF 2 =CF(OCF 2 CF(CF 3 )) m O(CF 2 ) n -CN
[0140] (wherein m is an integer from 0 to 5, and n is an integer from 1 to 8), more preferably CF2 =CFOCF 2 CF(CF 3 )OCF 2 CF 2 CN.
[0141] These perfluoroelastomers can be produced by conventional methods.
[0142] Specific examples of the perfluoroelastomer include fluororubbers described in International Publication No. 97 / 24381, Japanese Examined Patent Publication No. 61-57324, Japanese Examined Patent Publication No. 4-81608, Japanese Examined Patent Publication No. 5-13961, and the like.
[0143] (Co-precipitation)
[0144] The composition of the present invention is obtained by coprecipitating a perfluoroelastomer with PTFE. By using the coprecipitation method to prepare the composition, when the composition is crosslinked, a crosslinked product with excellent plasma resistance and excellent compression set characteristics can be obtained. When the composition is prepared by a method other than the coprecipitation method, such as dry mixing, and the resulting composition is crosslinked, the plasma resistance and compression set characteristics of the crosslinked product are not fully improved. For example, when the crosslinked product is irradiated with NF 3 In the case of plasma, there is a problem of being cut, and when the cross-linked material is compressed for a long time at a high temperature of about 300°C, there is a problem that the cross-linked material is crushed due to compression, or there is a problem that the shape of the cross-linked material is difficult to restore even if it is released from compression.
[0145] The combination of perfluoroelastomer and PTFE in co-precipitation is selected according to the target function by taking into account whether the coagulation properties of the respective polymers are similar and whether they have affinity as polymers.
[0146] Examples of a method for co-precipitating a perfluoroelastomer and PTFE include a method of preparing an aqueous dispersion containing a perfluoroelastomer and PTFE and co-precipitating the perfluoroelastomer and PTFE in the obtained aqueous dispersion.
[0147] Examples of the method for preparing the aqueous dispersion include a method of mixing an aqueous dispersion containing a perfluoroelastomer with an aqueous dispersion containing PTFE, a method of mixing a powder of a perfluoroelastomer with an aqueous dispersion containing PTFE, and a method of mixing a powder of PTFE with an aqueous dispersion containing a perfluoroelastomer.
[0148] The temperature of each aqueous dispersion when mixing the aqueous dispersion containing perfluoroelastomer and the aqueous dispersion containing PTFE is preferably 10°C or higher, more preferably 15°C or higher, further preferably 20°C or higher, and preferably 60°C or lower, further preferably 50°C or lower.
[0149] As the method for making the perfluoroelastomer in the aqueous dispersion thus obtained and PTFE coprecipitate, the method for mixing aqueous dispersion with precipitating agent, the method for freezing can be enumerated.As precipitating agent, known precipitating agents such as acid can be used, for example, aluminum salt, calcium salt or magnesium salt can be enumerated, as organic system precipitating agent, ammonium acetate, ammonium carbonate etc. can be enumerated, as inorganic acid precipitating agent, hydrochloric acid, nitric acid, hydrofluoric acid, sulfuric acid, trifluoroacetic acid etc. can be enumerated.Wherein, by using inorganic acid precipitating agent as precipitating agent, metal content is few, clean, can not make the crosslinking sites such as cyano group possessed by perfluoroelastomer damaged during precipitation, can obtain the crosslinked product with high crosslink density when the composition is crosslinked, the crosslinked product obtained demonstrates excellent plasma resistance and excellent compression set characteristic.
[0150] The temperature when the aqueous dispersion is mixed with the precipitating agent is preferably above 10°C, more preferably above 15°C, further preferably above 20°C, preferably below 60°C, further preferably below 50°C. The temperature when the aqueous dispersion is mixed with the precipitating agent can be the temperature of the mixture obtained by mixing. When the aqueous dispersion is mixed with an aqueous solution containing a precipitating agent, the temperature when the aqueous dispersion is mixed with the precipitating agent can be adjusted by adjusting the temperature of the aqueous dispersion and the aqueous solution.
[0151] The composition obtained by coprecipitation can be washed with water, and after removing impurities such as a small amount of buffer solution and salt present in the composition, the washed composition is dried with a hot air stove, a vacuum dryer, etc. The drying temperature is preferably above 40°C, more preferably above 50°C, further preferably above 60°C, preferably below 200°C, more preferably below 150°C, and further preferably below 100°C.
[0152] The form of the composition obtained after the coprecipitation is not particularly limited, and can be gum, crumb, powder, granular material, etc., preferably gum or crumb. Gum is a granular piece consisting of the composition, and crumb refers to the perfluoroelastomer in the composition that cannot maintain a granular form as a gum at room temperature and is mutually fused to form an amorphous block form.
[0153] <Other ingredients>
[0154] Composition of the present invention can contain other components beyond perfluoroelastomer and PTFE.The composition containing other components can be prepared by adding other components when making perfluoroelastomer and PTFE coprecipitation, and can also be prepared by mixing coprecipitation composition with other components after making perfluoroelastomer and PTFE coprecipitation.Common polymer processing machinery, for example mill, Banbury mixer, kneader, closed mixer etc. can be used for mixing.
[0155] As other components, fillers can be mentioned, for example.
[0156] As fillers, there can be mentioned imide-based fillers having an imide structure, such as polyimide, polyamide-imide, and polyetherimide; organic fillers made of engineering plastics, such as polyarylate, polysulfone, polyethersulfone, polyphenylene sulfide, polyetheretherketone, polyetherketone, and polyoxybenzoate; metal oxide fillers, such as silicon oxide, aluminum oxide, and yttrium oxide; metal carbides, such as silicon carbide and aluminum carbide; metal nitride fillers, such as silicon nitride and aluminum nitride; and inorganic fillers, such as carbon black, aluminum fluoride, and carbon fluoride.
[0157] Among these, carbon black, aluminum oxide, silicon oxide, yttrium oxide, silicon carbide, silicon nitride, polyimide, and carbon fluoride are preferred from the viewpoint of shielding effects of various plasmas.
[0158] The above-mentioned inorganic fillers and organic fillers may be mixed alone or in combination of two or more.
[0159] In the field where high purity and non-polluting properties are not particularly required, conventional additives such as processing aids, plasticizers, colorants, etc. that are normally added to the composition as required may be mixed, and one or more conventional crosslinking agents or crosslinking aids different from the above may also be mixed.
[0160] The above composition may also contain an organic alkaline compound. Examples of the organic alkaline compound include:
[0161] Formula: CH 3 (CH 2 ) 17 -NH 2 Octadecylamine;
[0162] Formula: H 2 NC(O)-(CH 2 ) 11 -CH=CH-(CH 2 ) 7 CH 3 of erucamide;
[0163] Formula: H 2 NC(O)-(CH 2 ) 7-CH=CH-(CH 2 ) 7 CH 3 of oleamide;
[0164] Formula: H 2 N-(CH 2 ) 6 -NH 2 1,6-Hexanediamine
[0165] Mode:
[0166] [Chemistry 2]
[0167] 1,8-diazabicycloundec-7-ene (DBU), etc.
[0168] (cross-linking agent, etc.)
[0169] The composition of the present invention may further contain at least one selected from the group consisting of an inorganic nitride, an organic tin compound, a compound generating ammonia, and a crosslinking agent. By making the composition of the present invention contain such components as a crosslinking agent, a crosslinked product can be easily obtained from the composition of the present invention.
[0170] The inorganic nitride is not particularly limited, and examples thereof include silicon nitride (Si 3 N 4 ), lithium nitride, titanium nitride, aluminum nitride, boron nitride, vanadium nitride, zirconium nitride, etc. Among these, silicon nitride is preferred because it can provide nano-scale fine particles.
[0171] Examples of the organic tin compound include tetraphenyltin and triphenyltin.
[0172] As the compound generating ammonia, a compound generating ammonia at 40°C to 330°C is preferred.
[0173] As the ammonia-generating compound, urea or its derivatives, ammonium salts are preferred, urea or ammonium salts are more preferred, and urea is further preferred. As the ammonium salt, it can be an organic ammonium salt or an inorganic ammonium salt. In addition, as the ammonia-generating compound, it can be a substance that reacts with a trace amount of water to generate ammonia.
[0174] Examples of urea derivatives include diurea, thiourea, urea hydrochloride, and biuret.
[0175] Examples of the organic ammonium salt include ammonium salts of non-fluorinated carboxylic acids or sulfonic acids such as ammonium benzoate, ammonium adipate, and ammonium phthalate.
[0176] Examples of the inorganic ammonium salt include compounds described in Japanese Patent Application Laid-Open No. 9-111081, for example, ammonium sulfate, ammonium carbonate, ammonium nitrate, ammonium phosphate, and the like.
[0177] In addition, examples of the ammonia-generating compound include acetaldehyde ammonia, hexamethylenetetramine, formamidine, formamidine hydrochloride, formamidine acetate, tert-butyl carbamate, benzyl carbamate, phthalamide, and the like.
[0178] As the crosslinking agent, there can be mentioned crosslinking agents used in peroxide crosslinking, polyol crosslinking, polyamine crosslinking, triazine crosslinking, oxazole crosslinking, imidazole crosslinking and thiazole crosslinking. In the case where the perfluoroelastomer has a cyano group (-CN group), the crosslinking agent is preferably at least one selected from the group consisting of an oxazole crosslinking agent, an imidazole crosslinking agent and a thiazole crosslinking agent.
[0179] The crosslinking agent used in the peroxide crosslinking may be any organic peroxide that can easily generate peroxide radicals in the presence of heat or a redox system. Specific examples thereof include 1,1-bis(tert-butylperoxy)-3,5,5-trimethylcyclohexane, 2,5-dimethylhexane-2,5-dihydroperoxide, di-tert-butyl peroxide (Perbutyl D), tert-butylcumyl peroxide (Perbutyl C), dicumyl peroxide (Percumyl D, Percumyl D-40, Percumyl D-40MB (T)), α,α-bis(tert-butylperoxy)-p-diisopropylbenzene, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane (Perhexa 25B, Perhexa 25B-40), 2,5-dimethyl-2,5-di(tert-butylperoxy)-3-hexyne (Perhexyne 25B, Perhexyne 25B-40), benzoyl peroxide, tert-butylbenzene peroxide, 2,5-dimethyl-2,5-di(benzoyl peroxide)hexane (Perhexa 25Z), tert-butyl peroxymaleate (t-butyl MA), tert-butyl peroxyisopropyl carbonate (Perbutyl I-75), methyl ethyl ketone peroxide (Permek D (DR), Permek H (HR, HY), Permek N (NR, NY), Permek S (SR), Permek F (FR), Permek G (GR, GY)), cyclohexanone peroxide (Perhexa H), acetylacetone peroxide (Percure AH, AL), 1,1-di(tert-hexylperoxy)-3,3,5-trimethylcyclohexane (Perhexa TMH), 1,1-di(tert-hexylperoxy)cyclohexane (Perhexa HC), 1,1-di(tert-butylperoxy)-2-methylcyclohexane (Perhexa MC), 1,1-di(tert-butylperoxy)cyclohexane (Perhexa C-80(S), Perhexa C-75(EB), Perhexa C(C), Perhexa C-40, Perhexa C-40MB(S)), 2,2-di(tert-butylperoxy)butane (Perhexa 22), 4,4-di(tert-butylperoxy)butyl valerate (Perhexa V, Perhexa V-40(F)), 2,2-di(4,4-di(tert-butylperoxy)cyclohexyl)propane (Pertetra A), terpene hydroperoxide (Permenta H), diisopropylbenzene hydroperoxide (Percumyl P), 1,1,3,3-Tetramethylbutyl hydroperoxide (Perocta H), cumene hydroperoxide (Percumyl H-80), tert-butyl hydroperoxide (Perbutyl H-69), di(2-tert-butylperoxyisopropyl)benzene (Perbutyl P, Perbutyl P-40, Peroximon F-40, Perbutyl P-40MB(K)), di-tert-hexyl peroxide (Perhexyl D), diisobutyryl peroxide (Peroyl IB), di(3,5,5-trimethylhexanoyl) peroxide (Peroyl 355(S)), dilauroyl peroxide (Peroyl L), succinyl peroxide (Peroyl SA), di(3-methylbenzoyl) peroxide, benzoyl (3-methylbenzoyl) peroxide and a mixture of dibenzoyl peroxide (NYPER BMT-K40, NYPER BMT-M), dibenzoyl peroxide (NYPER BW, NYPER BO, NYPER FF, NYPER BS, NYPER E, NYPER NS), di(4-methylbenzoyl) peroxide (NYPER PMB), di-n-propyl peroxydicarbonate (Peroyl NPP-50M), diisopropyl peroxydicarbonate (Peroyl IPP-50, Peroyl IPP-27), di(4-tert-butylcyclohexyl) peroxydicarbonate (Peroyl TCP), di(2-ethylhexyl) peroxydicarbonate (Peroyl OPP), di-sec-butyl peroxydicarbonate (Peroyl SBP), cumyl peroxyneodecanoate (Percumyl ND, Percumyl ND-50E), 1,1,3,3-tetramethylbutyl peroxyneodecanoate (Perocta ND, Perocta ND-50E), tert-hexyl peroxyneodecanoate (Perhexyl ND, Perhexyl ND-50E), tert-butyl peroxyneodecanoate (Perbutyl ND, Perbutyl ND-50E), tert-butyl peroxy neoheptanoate (Perbutyl NHP), tert-hexyl peroxy pivalate (Perhexyl PV, Perhexyl PV-50E), tert-butyl peroxy pivalate (PerbutylPV, Perbutyl PV-40E), 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate (Perocta O), 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane (Perhexa 25O), tert-hexyl peroxy(2-ethyl)hexanoate (PerhexylO, Percure HO(N)), tert-butyl peroxy(2-ethylhexanoate) (Perbutyl O, Percure O), tert-hexyl peroxyisopropyl monocarbonate (Perhexyl I), tert-butyl peroxy-3,5,5-trimethylhexanoate (Perbutyl355), tert-butyl peroxylaurate (Perbutyl L), tert-butyl peroxy-2-ethylhexyl monocarbonate (Perbutyl E), tert-hexyl peroxybenzoate (Perhexyl Z), tert-butyl peroxyacetate (Perbutyl A), a mixture of tert-butyl peroxy-3-methylbenzoate and tert-butyl peroxybenzoate (Perbutyl ZT), tert-butyl peroxybenzoate (Perbutyl Z), tert-butyl peroxyallyl monocarbonate (Peromer AC), 3,3',4,4'-tetra(tert-butylperoxycarbonyl)benzophenone (BTTB-25), 2,3-dimethyl-2,3-diphenylbutane (NOFMER BC-90), etc. Among them, dialkyl-type substances are preferred. In addition, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane is particularly preferred. The type and amount of organic peroxides are usually selected in consideration of the amount of active -OO-, decomposition temperature, etc.
[0180] In addition, as the crosslinking aid that can be used in this case, any compound that has a reaction activity with peroxide radicals and polymer radicals can be used, and examples thereof include -CH=CH 2 、-CH 2 CH=CH 2 , -CF=CF 2 ,-C(CF 3 )=CF 2 、-C(CH 3 )=CF 2 , -CF=CF(CF 3 ), -CF=CF(CH 3 )、-C(C 6 H 5 )=CF 2 , -CF=CF(C 6 H 5 ), -CH=CF 2 , -CF=CHF, -C(CF 3 )=CHF、-CF=CH(CF 3 ), -CH=CF(CF 3 ) and other functional groups (the "C 6 H5 ” represents phenyl). Specifically, for example, triallyl cyanurate, triallyl isocyanurate (TAIC), 1,3,5-triacryloylhexahydro-1,3,5-triazine, triallyl trimellitate, N,N'-n-phenylene bismaleimide, diallyl terephthalate, diallyl phthalate, tetraallyl terephthalamide, triallyl phosphate, bismaleimide, fluorinated triallyl isocyanurate (1,3,5-tris(2,3,3-trifluoro-2-propenyl)-1,3,5-triazine-2,4,6-trione), tris(diallylamine)-s-triazine, triallyl phosphite, N,N-diallylacrylamide, 1,6-divinyl dodecafluorohexane, etc. can be mentioned.
[0181] In addition, as a crosslinking auxiliary agent used together with the peroxide crosslinking agent, the general formula (31) can also be mentioned:
[0182] [Chemistry 3]
[0183]
[0184] (In the formula, 6 R 31 are each independently H, a halogen atom, or an optionally halogenated group having 1 to 5 carbon atoms which may be interposed with an ether bond, 31 It is a compound represented by a linear or branched chain having 1 to 18 carbon atoms and optionally containing a hetero atom, and optionally halogenated alkylene, cycloalkylene or (per)fluoropolyoxyalkylene.
[0185] Examples of the compound represented by the general formula (31) include the compound represented by the general formula (32), the compound represented by the general formula (33), the compound represented by the general formula (34), and the like.
[0186] General formula (32):
[0187] [Chemistry 4]
[0188]
[0189] (wherein, j is an integer of 2 to 10, preferably an integer of 4 to 8, and 4 R 32 Each independently represents H, F, or an alkyl group or a (per)fluoroalkyl group having 1 to 5 carbon atoms)
[0190] General formula (33):
[0191] [Chemistry 5]
[0192]
[0193] (Where Y 31 Each is independently F, Cl or H, Y 32Each independently is F, Cl, H or OR 33 (Here, R 33 is a branched or straight chain alkyl group which may be substantially or completely fluorinated or chlorinated), Z 33 is a divalent group having 2 to 10 carbon atoms which may be interposed with an ether bond and may be fluorinated, preferably Z 33 m is an integer from 3 to 5 -(CF 2 ) m - group, the compound represented by the general formula (33) is preferably F 2 C=CF-O-(CF 2 ) 5 -O-CF=CF 2 )
[0194] General formula (34):
[0195] [Chemistry 6]
[0196]
[0197] (In the formula, Y 31 , Y 32 and Z 33 As mentioned above, R 34 Each independently represents H, F, or an alkyl group or a (per)fluoroalkyl group having 1 to 5 carbon atoms)
[0198] As the crosslinking aid used together with the crosslinking agent or the peroxide crosslinking agent, there can also be mentioned at least one compound having the general formula (35):
[0199] [Chemistry 7]
[0200]
[0201] (Where R 35 ~R 37 are each independently a hydrogen atom, a fluorine atom, an alkyl group, a fluoroalkyl group, or a substituted or unsubstituted aryl group, R 35 ~R 37 At least one of them is a fluorine atom or a group containing a fluorine atom. m is an integer of 1 to 5. When m is 2 or more, m R 35 ~R 37 They may be the same or different. A compound having a structure represented by (a) a hydrogen atom of a benzene ring may or may not have a substituent. When m is 1, it is preferred that there are two or more of the structure.
[0202] Examples of the compound having a structure represented by the general formula (36) include the compound represented by the general formula (36), the compound represented by the general formula (37), and the like.
[0203] General formula (36):
[0204] [Chemistry 8]
[0205]
[0206] (Where R 35 ~R 37 As described above. p is an integer from 0 to 2, and n is an integer from 2 to 6)
[0207] General formula (37):
[0208] [Chemistry 9]
[0209]
[0210] (Where R 35 ~R 37 As above. 38 For a single bond, -SO 2 -, -O-, -S-, -CO-, a group containing a heteroatom, a substituted or unsubstituted alkylene group, a substituted or unsubstituted cycloalkylene group, or a substituted or unsubstituted arylene group. m is an integer from 1 to 5. These groups may be partially or fully fluorinated)
[0211] The heteroatom-containing group is not particularly limited as long as it is a divalent group containing a heteroatom. Examples of the heteroatom include an oxygen atom, a nitrogen atom, a sulfur atom, a boron atom, and a phosphorus atom.
[0212] Examples of the crosslinking agent used for the polyol crosslinking include polyol compounds such as bisphenol A and bisphenol AF.
[0213] Examples of the crosslinking agent used for the polyamine crosslinking include polyamine compounds such as 1,6-hexanediamine carbamate, N,N′-dicinnamylidene-1,6-hexanediamine, and 4,4′-bis(aminocyclohexyl)methane carbamate.
[0214] Examples of the crosslinking agent used in oxazole crosslinking, imidazole crosslinking, and thiazole crosslinking include bisdiaminophenyl-based crosslinking agents represented by general formula (41), diaminophenol-based crosslinking agents, bisaminothiophenol-based crosslinking agents, bisaminohydrazone-based crosslinking agents represented by general formula (42), bisaminohydrazone-based crosslinking agents represented by general formula (43), bisamide oxime-based crosslinking agents represented by general formula (44), and compounds represented by general formula (45).
[0215] General formula (41):
[0216] [Chemistry 10]
[0217]
[0218] (Where R 41 Yes-SO 2-, -O-, -CO-, an alkylene group having 1 to 6 carbon atoms, a perfluoroalkylene group having 1 to 10 carbon atoms, or a single bond, or
[0219] [Chemistry 11]
[0220]
[0221] The group shown, R 42 and R 43 One of them is -NH 2 and the other is -NHR 44 、-NH 2 , -OH or -SH, R 44 is a hydrogen atom, a fluorine atom or a monovalent organic group, preferably R 42 For -NH 2 , R 43 NHR 44 Preferred specific examples of the alkylene group having 1 to 6 carbon atoms include methylene, ethylene, propylene, butylene, pentylene, hexylene, and the like. Preferred specific examples of the perfluoroalkylene group having 1 to 10 carbon atoms include
[0222] [Chemistry 12]
[0223]
[0224] It should be noted that these compounds are known as examples of bisdiaminophenyl compounds in Japanese Patent Publication No. 2-59177, Japanese Patent Publication No. 8-120146, etc.)
[0225] General formula (42):
[0226] [Chemistry 13]
[0227]
[0228] (R 41 As mentioned above, R 45 Each independently represents any one of the following groups)
[0229] [Chemistry 14]
[0230]
[0231] General formula (43):
[0232] [Chemistry 15]
[0233]
[0234] (Where Rf 41 is a perfluoroalkylene group having 1 to 10 carbon atoms)
[0235] General formula (44):
[0236] [Chemistry 16]
[0237]
[0238] (where n is an integer from 1 to 10)
[0239] General formula (45): HN=CR 45 R 46
[0240] (Where R 45 Selected from H, NH 2 and NHR 47 In the group composed of 46 Select from Ph, SO 2 H, NR 48 R 49 , 2-pyridine and CH 2 CONH 2 In the group composed of 47 Selected from Ph, NH 2 In the group consisting of R 48 Selected from H, NHPh, CH 2 CONH 2 , a linear alkyl group having 1 to 8 carbon atoms and a branched alkyl group having 1 to 8 carbon atoms, and R 49 Selected from Ph, COOC(CH 3 ) 3 NH 2 , CH 2 COOH、CSNH 2 、CNHNH 3 + Cl - , p-phenyl CN,
[0241] [Chemistry 17]
[0242]
[0243] and COPh)
[0244] These diaminophenol-based crosslinking agents, bisaminothiophenol-based crosslinking agents, or bisdiaminophenyl-based crosslinking agents have been used in crosslinking systems with cyano groups as crosslinking points, but react with both carboxyl groups and alkoxycarbonyl groups to form oxazole rings, thiazole rings, and imidazole rings to provide crosslinked products.
[0245] In addition, the crosslinking agent may also be a compound of the general formula (46): X 41 -(CH 2 )n -R 50 -(CH 2 ) m -X 41 (Where X 41 are each independently an alkynyl group, a nitrile group or Y 41 P N 3 (Y 41 for SO, SO 2 , C 6 H 4 or CO, p is 0 or 1), n and m are independently integers of 1 to 4, R 50 Freedom to choose
[0246] i) a fluoroalkylene group having 3 to 10 carbon atoms,
[0247] ii) a fluoroalkyleneoxy group having 3 to 10 carbon atoms,
[0248] iii) substituted arylene,
[0249] iv) an oligomer comprising copolymerized units of vinylidene fluoride and perfluoro(methyl vinyl ether),
[0250] v) an oligomer comprising copolymerized units of vinylidene fluoride and hexafluoropropylene,
[0251] vi) oligomers comprising copolymerized units of tetrafluoroethylene and perfluoro(methyl vinyl ether) and
[0252] vii) a crosslinking agent as shown in the group consisting of oligomers comprising copolymerized units of tetrafluoroethylene and hydrocarbon olefins. The crosslinking agent is preferably used together with a perfluoroelastomer having a nitrile group, an azide group, a sulfonyl azide group, a carbonyl azide group or an alkyne group. For example, the nitrile group of the perfluoroelastomer reacts with the azide group of the crosslinking agent to form a tetrazole ring to provide a crosslinked product.
[0253] Particularly preferred crosslinking agents include compounds having two or more 3-amino-4-hydroxyphenyl groups or 3-amino-4-mercaptophenyl groups, or general formula (47):
[0254] [Chemistry 18]
[0255]
[0256] (Where R 41 , R 42 and R 43As described above), specifically, for example, 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (common name: bis(aminophenol) AF), 2,2-bis(3-amino-4-mercaptophenyl)hexafluoropropane, tetraaminobenzene, bis-3,4-diaminophenylmethane, bis-3,4-diaminophenyl ether, 2,2-bis(3,4-diaminophenyl)hexafluoropropane, 2,2-bis[3-amino-4-(N-phenylamino) Hexafluoropropane, 2,2-bis[3-amino-4-(N-methylamino)phenyl]hexafluoropropane, 2,2-bis[3-amino-4-(N-ethylamino)phenyl]hexafluoropropane, 2,2-bis[3-amino-4-(N-propylamino)phenyl]hexafluoropropane, 2,2-bis[3-amino-4-(N-perfluorophenylamino)phenyl]hexafluoropropane, 2,2-bis[3-amino-4-(N-benzylamino)phenyl]hexafluoropropane, etc.
[0257] Among these, as the crosslinking agent, 2,2-bis[3-amino-4-(N-phenylamino)phenyl]hexafluoropropane is preferred from the viewpoint of heat resistance, steam resistance, amine resistance, and good crosslinking properties.
[0258] The content of at least one selected from the group consisting of an inorganic nitride, an organic tin compound, an ammonia generating compound and a crosslinking agent is preferably 0.05 parts by mass or more, more preferably 0.1 parts by mass or more, further preferably 0.2 parts by mass or more, particularly preferably 0.3 parts by mass or more, and is preferably 10 parts by mass or less, more preferably 5.0 parts by mass or less, further preferably 2.0 parts by mass or less, and particularly preferably 1.0 parts by mass or less, based on 100 parts by mass of the perfluoroelastomer.
[0259] (cross-linked product)
[0260] The above composition can be suitably used as a molding material for crosslinking to obtain a crosslinked product. By crosslinking the composition of the present invention, a crosslinked product can be obtained. The crosslinked product of the present invention has a great influence on NF 3 Plasma has excellent durability and has a small compression set even when used at a high temperature exceeding 300°C.
[0261] The cross-linked product of the present invention preferably has a compression set (300°C) measured at 300°C for 70 hours at a compression rate of 25%, which is preferably 60% or less, and more preferably 55% or less. The compression set (300°C) can be calculated by compressing the cross-linked product at a compression rate of 25%, leaving it at 300°C for 70 hours, releasing the compression, leaving it at 23°C for 30 minutes, and measuring the thickness of the cross-linked product before and after compression.
[0262] The cross-linked product of the present invention is not easily crushed even when compressed at high temperature. According to the present invention, a cross-linked product is provided that does not break even when left at 300°C for 70 hours at a compression rate of 25%. In addition, according to the present invention, a cross-linked product is provided that does not break even in the above-mentioned test for measuring the compression set (300°C) and can measure the compression set (300°C) (i.e., a cross-linked product having a value of the compression set (300°C)).
[0263] The cross-linked product of the present invention is preferably 70% or less, and more preferably 65% or less, when the compression set (temperature changed from 200°C to 70°C) is measured by placing the cross-linked product at a compression rate of 25% at 200°C for 70 hours and further at 70°C for 24 hours. The compression set (temperature changed from 200°C to 70°C) can be calculated as follows: after the cross-linked product is compressed at a compression rate of 25%, it is placed at 200°C for 70 hours and further at 70°C for 24 hours, the compression is released, and the cross-linked product is placed at 23°C for 30 minutes, and the thickness of the cross-linked product before and after compression is measured.
[0264] As a method for obtaining a crosslinked product from a composition, there can be mentioned a method of obtaining a preform by molding the above composition as a molding material and then crosslinking the preform. The method for obtaining a preform from the above composition can be a common method, and can be carried out by a known method such as a method of heating and compressing with a mold, a method of pressing into a heated mold, and a method of extruding with an extruder. In the case of extruded products such as hoses or wires, a crosslinked product can be obtained by heating and crosslinking with steam or the like after extrusion.
[0265] The above crosslinking is called primary crosslinking, and can be performed in the order of primary crosslinking and secondary crosslinking. The primary crosslinking is preferably performed at 150°C to 250°C for 5 minutes to 120 minutes, and more preferably at 170°C to 200°C for 5 minutes to 60 minutes. As the crosslinking means, a known crosslinking means can be used, for example, press crosslinking, etc.
[0266] The secondary crosslinking is preferably carried out at 250°C to 320°C for 2 hours to 48 hours, more preferably at 280°C to 310°C for 5 hours to 24 hours. In addition, the secondary crosslinking can be carried out at 180°C to 320°C for 2 hours to 24 hours, or at 190°C to 310°C for 5 hours to 20 hours. It is also possible to have a temperature change within this temperature range. As a crosslinking means, a known crosslinking means can be used, for example, heating crosslinking can be cited. Crosslinking can be carried out, for example, in an air atmosphere or a nitrogen atmosphere.
[0267] The crosslinked product of the present invention can be suitably used as a sealing material for semiconductor manufacturing equipment that particularly requires heat resistance, especially semiconductor manufacturing equipment that performs high-density plasma irradiation. Examples of the above-mentioned sealing material include O-rings, square rings, gaskets, sealing pads, oil seals, bearing seals, lip seals, etc.
[0268] In addition, it can be used as various polymer products used in semiconductor manufacturing equipment, such as diaphragms, tubes, hoses, various rubber rollers, belts, etc. In addition, it can also be used as a coating material and a lining material.
[0269] It should be noted that the semiconductor manufacturing equipment referred to in the present invention is not particularly limited to equipment for manufacturing semiconductors, but broadly includes all manufacturing equipment used in the semiconductor field requiring high cleanliness, such as equipment for manufacturing liquid crystal panels or plasma panels, for example, the following equipment can be cited.
[0270] (1) Etching equipment
[0271] Dry etching equipment
[0272] Plasma etching equipment
[0273] Reactive ion etching equipment
[0274] Reactive ion beam etching equipment
[0275] Sputtering Etching Equipment
[0276] Ion beam etching equipment
[0277] Wet etching equipment
[0278] Ashing device
[0279] (2) Cleaning device
[0280] Dry Etching Cleaning Equipment
[0281] UV / O 3 Cleaning device
[0282] Ion beam cleaning device
[0283] Laser beam cleaning device
[0284] Plasma cleaning device
[0285] Gas Etching Cleaning Device
[0286] Extraction and cleaning device
[0287] Soxhlet extraction cleaning device
[0288] High temperature and high pressure extraction and cleaning device
[0289] Microwave extraction cleaning device
[0290] Supercritical extraction cleaning device
[0291] (3) Exposure device
[0292] Lithography Machine
[0293] Coating machine and developer
[0294] (4) Grinding device
[0295] CMP equipment
[0296] (5) Film forming device
[0297] CVD equipment
[0298] Sputtering device
[0299] (6) Diffusion and ion implantation equipment
[0300] Oxidation diffusion device
[0301] Ion implantation device
[0302] The crosslinked product of the present invention can exhibit excellent performance as a sealing material for, for example, a CVD device, a plasma etching device, a reactive ion etching device, an ashing device, or an excimer laser exposure device.
[0303] Although the embodiments have been described above, it will be appreciated that various modifications may be made to the embodiments and details without departing from the spirit and scope of the claims.
[0304] <1> According to a first aspect of the present invention, there is provided a composition comprising a perfluoroelastomer and polytetrafluoroethylene, wherein the melt viscosity of the polytetrafluoroethylene is 1.0×10 3 Mooring ~7.0×10 6 The melting point of the polytetrafluoroethylene is above 322° C., and the composition is obtained by co-precipitating the perfluoroelastomer and the polytetrafluoroethylene.
[0305] <2> According to a second aspect of the present invention, there is provided the composition according to the first aspect, wherein the perfluoroelastomer has a cyano group.
[0306] <3> According to a third aspect of the present invention, there is provided the composition according to the first aspect or the second aspect, wherein the polytetrafluoroethylene optionally contains a modified monomer unit, and the content of the modified monomer unit is 0 mol % to 0.10 mol % based on all monomer units.
[0307] <4> According to a fourth aspect of the present invention, there is provided the composition according to the first aspect or the second aspect, wherein the polytetrafluoroethylene contains a modified monomer unit, and the content of the modified monomer unit is 0.02 mol % to 0.10 mol % based on all monomer units.
[0308] <5> According to a fifth aspect of the present invention, there is provided the composition according to the fourth aspect, wherein the modified monomer unit is at least one selected from the group consisting of hexafluoropropylene units and perfluorovinyl ether units.
[0309] <6> According to a sixth aspect of the present invention, there is provided the composition according to any one of the first to fifth aspects, wherein the polytetrafluoroethylene has an average primary particle size of 200 nm or more.
[0310] <7> According to a seventh aspect of the present invention, there is provided the composition according to any one of the first to sixth aspects, wherein the content of the polytetrafluoroethylene is 1 to 100 parts by mass based on 100 parts by mass of the perfluoroelastomer.
[0311] <8> According to an eighth aspect of the present invention, there is provided a composition based on any one of the first to seventh aspects, wherein the composition is obtained by preparing an aqueous dispersion containing the perfluoroelastomer and the polytetrafluoroethylene and co-precipitating the perfluoroelastomer and the polytetrafluoroethylene in the obtained aqueous dispersion using an acid.
[0312] <9> According to a ninth aspect of the present invention, there is provided a composition according to any one of the first to eighth aspects, further comprising at least one selected from the group consisting of an inorganic nitride, an organic tin compound, an ammonia generating compound, and a crosslinking agent.
[0313] <10> According to a tenth aspect of the present invention, there is provided a cross-linked product obtained by cross-linking the composition according to any one of the first aspect to the ninth aspect.
[0314] Example
[0315] Next, embodiments of the present invention will be described with reference to examples, but the present invention is not limited to the examples.
[0316] Each numerical value in the examples was measured by the following method.
[0317] (Composition of PTFE)
[0318] pass 19 It was determined by F-NMR analysis.
[0319] (Average primary particle size of PTFE)
[0320] The average primary particle size is calculated as follows: after determining the correlation between the transmittance when 550 nm light is incident on a specified unit injected with a PTFE aqueous dispersion adjusted to a solid content of 0.15 mass%, and the number average primary particle size calculated by measuring the oriented diameter using a transmission electron microscope photograph, the transmittance measured on the obtained sample is substituted into the above correlation to thereby determine the average primary particle size (standard curve method).
[0321] (Melting point of PTFE)
[0322] The melting point of PTFE is measured as follows: using a differential scanning calorimeter X-DSC7000 (DSC) manufactured by Hitachi High-Technologies Corporation, about 3 mg of PTFE that has not been heated to a temperature of more than 300°C after temperature correction using indium and lead as a standard sample is placed in an aluminum pan, and the temperature is raised at 10°C / min in a temperature range of 230°C to 350°C under a nitrogen gas flow of 40 ml / min, and differential scanning calorimetry is performed, and the temperature corresponding to the minimum point of the melting curve in the above-mentioned range is measured as the melting point.
[0323] (PTFE melt viscosity)
[0324] Melt viscosity was measured according to ASTM D 1238 using a flow tester (manufactured by Shimadzu Corporation) and A 2 g sample preheated at 380°C for 5 minutes was placed in a die head and held at the temperature under a load of 0.7 MPa for measurement. "Insoluble" in the table means that the PTFE was not melted and the melt viscosity could not be measured.
[0325] (Composition of perfluoroelastomer)
[0326] pass 19 It was determined by F-NMR analysis.
[0327] (Mooney viscosity of perfluoroelastomer)
[0328] The viscosity was measured at 170° C. in accordance with JIS K6300 using a Mooney viscometer MV2000E manufactured by ALPHA TECHNOLOGIES.
[0329] (Compression set (300℃))
[0330] The compression set was measured according to the method described in ASTM D395 or JIS K6262. The O-rings prepared in Examples and Comparative Examples were compressed at room temperature to a compression rate of 25% (O-rings with a thickness (wire diameter) of 3.5 mm were compressed to a thickness of 2.625 mm) using a compression device.
[0331] Next, the compression device with the compressed O-ring fixed thereto was placed in an electric furnace at 300°C for 70 hours, and then the compression device was taken out of the electric furnace. The O-ring was removed from the compression device and placed in a constant temperature room at 23°C for 30 minutes to measure the thickness of the O-ring (t 2 The compression set is calculated by the following formula. The closer the compression set is to 0%, the better the compression set property of the cross-linked product is.
[0332] Compression set (%) = (t 0 -t 2 ) / (t 0 -t 1 )×100
[0333] t 0 : Original thickness of O-ring (mm)
[0334] t 1 :Thickness of spacer (mm)
[0335] t 2 : Thickness of O-ring after compression test (mm)
[0336] In the above test, t 0 =3.5mm, t 1 =2.625mm.
[0337] (Crack rate (300℃))
[0338] The occurrence of cracks in 12 O-rings after the above-mentioned "Compression Set (300°C)" test was visually confirmed. The crack rate was calculated by the following calculation formula. The closer the crack rate is to 0%, the less likely it is that the cross-linked product will crack even if compressed.
[0339] Crack rate (%) = (number of cracks) / (number of tests) × 100
[0340] In the above experiment, the number of experiments = 12.
[0341] (Compression set (temperature changed from 200°C to 70°C))
[0342] The compression set was measured according to the method described in ASTM D395 or JIS K6262. The O-rings prepared in Examples and Comparative Examples were compressed at room temperature to a compression rate of 25% (O-rings with a thickness (wire diameter) of 3.5 mm were compressed to a thickness of 2.625 mm) using a compression device.
[0343] Next, the compression device with the compressed O-ring fixed thereon was placed in an electric furnace at 200°C for 70 hours, and then the compression device was taken out of the electric furnace. After that, the compression device with the compressed O-ring fixed thereon was placed in another electric furnace at 70°C for 24 hours. The O-ring was removed from the compression device, and the removed O-ring was placed in a constant temperature room at 23°C for 30 minutes, and the thickness (t 2 ). The compression set is calculated by the following formula.
[0344] Compression set (%) = (t 0 -t 2 ) / (t 0 -t 1 )×100
[0345] t 0 : Original thickness of O-ring (mm)
[0346] t 1 :Thickness of spacer (mm)
[0347] t 2 : Thickness of O-ring after compression test (mm)
[0348] In the above test, t 0 =3.5mm, t 1 =2.625mm.
[0349] (Crack rate (temperature changed from 200℃ to 70℃))
[0350] The occurrence of cracks in 12 O-rings after the above-mentioned "compression set (temperature changed from 200°C to 70°C)" test was visually confirmed. The crack rate was calculated using the following calculation formula. The closer the crack rate is to 0%, the less likely it is that the cross-linked product will crack even if it is compressed.
[0351] Crack rate (%) = (number of cracks) / (number of tests) × 100
[0352] In the above experiment, the number of experiments = 12.
[0353] (Plasma resistance (weight reduction rate of cross-linked product before and after plasma treatment))
[0354] The O-rings (P24 size) prepared in the examples and comparative examples were placed in a process chamber. Plasma generated by a radical generator was introduced into the process chamber, and the O-rings were exposed under the following plasma irradiation conditions. The NF was calculated based on the mass of the O-rings before and after plasma irradiation. 3 Remote plasma weight reduction rate.
[0355] (Plasma irradiation conditions)
[0356] Fluorine radical generator: Astron Atomic Fluorine Generator Model AX7657-2 (manufactured by MKS)
[0357] Gas flow rate: Ar / NF 3 =1(L / min) / 1(L / min)
[0358] Pressure: 3 Torr
[0359] Irradiation temperature: 250℃
[0360] Irradiation time: 12 hours (the O-ring position in the chamber is moved every 2 hours)
[0361] The following materials were used in Examples and Comparative Examples.
[0362] Perfluoroelastomer:
[0363] TFE / PMVE / CF 2 =CFOCF 2 CF(CF 3 )OCF 2 CF 2 CN=59.3 / 39.9 / 0.8(mol%)
[0364] Mooney viscosity ML (1+20) (170°C) = 66
[0365] Crosslinking agent:
[0366] 2,2-Bis[3-amino-4-(N-phenylamino)phenyl]hexafluoropropane
[0367] PTFE:
[0368] PTFE having the properties listed in Table 1
[0369] Example 1
[0370] 880 g of an emulsion of perfluoroelastomer particles (solid content concentration 24 wt%) and 282 g of an emulsion of PTFE particles having the properties described in Table 1 (solid content concentration 15 wt%) were mixed at 23° C. and added dropwise to 500 g of 10% nitric acid at 23° C. for 10 minutes to perform coprecipitation. The coprecipitated product was washed with water and dried at 70° C. using a vacuum dryer to obtain an elastomer composition in which PTFE was finely dispersed in a fluorinated elastomer.
[0371] The elastomer composition was measured by differential thermal analysis (DTA), and as a result, absorption believed to be based on PTFE was confirmed at 327.7°C.
[0372] 0.9 parts by mass of a crosslinking agent (2,2-bis[3-amino-4-(N-phenylamino)phenyl]hexafluoropropane) was mixed with 120 parts by mass of the obtained elastomer composition, and the mixture was kneaded using an open roll mill to obtain a crosslinkable elastomer composition.
[0373] Furthermore, the cross-linkable elastomer composition was cross-linked under pressure at 180°C for 30 minutes, and then heat-cross-linked at 290°C for 18 hours to produce an O-ring of size P24. The obtained O-ring was used to measure the compression set (300°C), compression set (temperature changed from 200°C to 70°C), NF 3 The results are shown in Table 1.
[0374] Embodiment 2 to Embodiment 3
[0375] An elastomer composition, a crosslinkable elastomer composition, and an O-ring were obtained in the same manner as in Example 1. As a result of DTA measurement of the elastomer composition, absorption believed to be due to PTFE was confirmed at 327.5°C in Example 2 and at 329.5°C in Example 3.
[0376] Comparative Example 1
[0377] The 23°C perfluoroelastomer particle emulsion used in Example 1 was dropped into 10% nitric acid at 23°C for precipitation. The precipitate was washed and dried to obtain perfluoroelastomer particles. On the other hand, nitric acid was added to the PTFE particle emulsion used in Example 1 for precipitation. The precipitate was washed and dried to obtain white PTFE powder.
[0378] 100 parts by mass of perfluoroelastomer particles, 20 parts by mass of PTFE powder and 0.9 parts by mass of a crosslinking agent (2,2-bis[3-amino-4-(N-phenylamino)phenyl]hexafluoropropane) were kneaded with an open roll mill to obtain a crosslinkable elastomer composition.
[0379] O-rings were prepared in the same manner as in Examples 1 to 3. Compression set (300°C), compression set (temperature changed from 200°C to 70°C), NF 3 The results are shown in Table 1.
[0380] Comparative Example 2
[0381] O-rings were prepared in the same manner as in Examples 1 to 3 except that the PTFE described in Table 1 was used, and the obtained O-rings were used for evaluation in the same manner.
[0382] [Table 1]
[0383] Table 1
[0384]
[0385] Embodiment 4 to Embodiment 7
[0386] An elastomer composition, a crosslinkable elastomer composition, and an O-ring were obtained in the same manner as in Example 1 except that the amounts of the respective materials were changed so as to have the composition described in Table 2. The results are shown in Table 2 together with the results of Example 1.
[0387] Comparative Example 3
[0388] 0.9 parts by mass of a crosslinking agent (2,2-bis[3-amino-4-(N-phenylamino)phenyl]hexafluoropropane) was mixed with 100 parts by mass of the perfluoroelastomer particles prepared in Comparative Example 1 by an open roll mill to obtain a crosslinkable elastomer composition. An O-ring was prepared from the crosslinkable elastomer composition in the same manner as in Example 1, and the obtained O-ring was evaluated in the same manner. The results are shown in Table 2.
[0389] [Table 2]
[0390] Table 2
[0391]
Claims
1. A composition comprising a perfluoroelastomer and polytetrafluoroethylene, wherein: The melt viscosity of the polytetrafluoroethylene is 1.0×10 3 Mooring ~7.0×10 6 moor, The melting point of the polytetrafluoroethylene is above 322°C. The composition is obtained by co-precipitating the perfluoroelastomer and the polytetrafluoroethylene.
2. The composition according to claim 1, wherein The perfluoroelastomer has a cyano group.
3. The composition according to claim 1 or 2, wherein The polytetrafluoroethylene optionally contains a modified monomer unit, and the content of the modified monomer unit is 0 mol% to 0.10 mol% based on the total monomer units.
4. The composition according to claim 1 or 2, wherein The polytetrafluoroethylene contains a modified monomer unit, and the content of the modified monomer unit is 0.02 mol% to 0.10 mol% based on the total monomer units.
5. The composition according to claim 4, wherein The modified monomer unit is at least one selected from the group consisting of hexafluoropropylene units and perfluorovinyl ether units.
6. The composition according to any one of claims 1 to 5, wherein The average primary particle size of the polytetrafluoroethylene is greater than 200 nm.
7. The composition according to any one of claims 1 to 6, wherein The content of the polytetrafluoroethylene is 1 to 100 parts by mass based on 100 parts by mass of the perfluoroelastomer. 8 . The composition according to claim 1 , which is obtained by preparing an aqueous dispersion containing the perfluoroelastomer and the polytetrafluoroethylene and co-precipitating the perfluoroelastomer and the polytetrafluoroethylene in the obtained aqueous dispersion using an acid. 9 . The composition according to claim 1 , further comprising at least one selected from the group consisting of an inorganic nitride, an organic tin compound, a compound that generates ammonia, and a cross-linking agent. 10 . A cross-linked product obtained by cross-linking the composition according to claim 1 .
Citation Information
Patent Citations
Crosslinkable fluorine rubber composition, fluorine rubber molded article, and method for producing same
CN103842429A
Transparent elastomer composition and method for producing the same
JP2007246930A
Control system for power conversion based on high speed communication
KR1020230056527A
Transparent elastomer composition
US6756445B1