Sheet of composite material comprising polymer and hexagonal boron nitride particles and method for producing same
By using high-content sheet hexagonal boron nitride particles in composite materials and using porous polymer network structure and heat-induced phase separation technology, the problem of insufficient thermal conductivity and dielectric characteristics of existing materials is solved, and efficient thermal Manage and electrical insulation performance.
Patent Information
- Application Number
- CN202380029620.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-24
- Filing Date
- 2023-03-13
- Publication Date
- 2024-11-08
AI Technical Summary
There are limitations in the improvement of thermal conductivity of existing thermal polymer materials, especially in the application of 5G technology, which requires high through-plane thermal conductivity, electrical insulation and low capacitance, which are difficult to achieve.
Using a composite material containing at least 70% by weight of sheet hexagonal boron nitride particles, the hexagonal boron nitride particles are oriented perpendicular to the plane of the sheet by a specific manufacturing method to form highly anisotropic thermal conductivity and pass through porous Polymer network structure and thermally induced phase separation technology improve particle load and thermal conductivity.
High through-plane thermal conductivity and good dielectric properties are achieved, ensuring efficient thermal management and electrical insulation performance of the material, exceeding the thermal conductivity limitations of traditional materials.
Smart Images

Figure CN118922483A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a sheet material comprising a composite material comprising a polymer and hexagonal boron nitride particles, wherein the hexagonal boron nitride particles comprise platelet-shaped hexagonal boron nitride particles oriented in a direction perpendicular to a planar direction of the sheet material. Background Art
[0002] Thermally conductive polymer compounds are used for thermal management solutions. For electronic devices such as in mobile devices, LED technology, electric vehicles and 5G technology, there is a growing demand for thermally conductive and electrically insulating polymer materials. In order to improve the performance of these materials, it is necessary to increase the thermal conductivity. For this purpose, thermally conductive fillers such as boron nitride, aluminum oxide, aluminum nitride, silicon carbide, silicon nitride, magnesium oxide or minerals are used. With increasing loading of thermally conductive fillers, higher thermal conductivity values can be achieved. The maximum loading of fillers in a compound usually limits the achievable thermal conductivity.
[0003] For 5G technology applications, materials with high thermal conductivity, electrical insulation, and low permittivity (i.e., low dielectric constant) and low dissipation factor are required. For many 5G applications, these thermal interface materials need to be in the form of films or sheets. It is usually desired that the thermal conductivity of these films or sheets is as high as possible in the direction perpendicular to the plane of the film, that is, high through-plane thermal conductivity is required.
[0004] US2010 / 0200801 A1 discloses a thermal interface material comprising a base matrix comprising a polymer and 5 wt% to 90 wt%, preferably 20 wt% to 60 wt% of a boron nitride filler having a platelet structure, wherein the platelet structures of the boron nitride particles are substantially aligned so that the thermal interface material has a bulk thermal conductivity of at least 1 W / m*K. The thermal interface material is extruded into sheets. As a second step, the sheets can be stacked, pressed, solidified, and sliced in a direction perpendicular to the stacking direction, or the sheets can be compression rolled into a coil, solidified, and cut into a plurality of circular pads in a direction perpendicular to the rolling direction.
[0005] WO 2019 / 097445 A1 discloses a polymer matrix composite material comprising a porous polymer network and a plurality of thermally conductive particles distributed within the polymer network structure.
[0006] There is a need for thermally conductive, electrically insulating thermal interface materials having high through-plane thermal conductivity and good dielectric properties (ie, low dielectric constant and low dielectric loss factor).
[0007] As used herein, "a", "an", "the / said", "at least one", and "one or more" are used interchangeably. The term "comprising" should also include the terms "consisting essentially of" and "consisting of". Summary of the invention
[0008] In a first aspect, the present disclosure is directed to a sheet comprising a composite material comprising a polymer and hexagonal boron nitride particles, wherein the hexagonal boron nitride particles comprise platelet-shaped hexagonal boron nitride particles, and wherein the platelet-shaped hexagonal boron nitride particles are oriented in a direction perpendicular to a planar direction of the sheet, and wherein the composite material comprises at least 70 wt % of the hexagonal boron nitride particles based on the total weight of the composite material, and wherein the sheet has a through-plane thermal conductivity greater than 12 W / m*K.
[0009] In another aspect, the present disclosure also relates to a method for producing a sheet as disclosed herein, the method comprising:
[0010] providing a polymer, a solvent, and hexagonal boron nitride particles including plate-like hexagonal boron nitride particles,
[0011] mixing a polymer, a solvent and hexagonal boron nitride particles to form a suspension of the hexagonal boron nitride particles in a polymer-solvent solution, wherein the polymer in the polymer-solvent solution has a melting point, and wherein the solvent has a boiling point, and wherein the mixing of the polymer, the solvent and the hexagonal boron nitride particles is performed at a temperature above the melting point of the polymer in the polymer-solvent solution and below the boiling point of the solvent,
[0012] forming the suspension into a film in which the plate-like hexagonal boron nitride particles are oriented in a direction parallel to the plane direction of the film,
[0013] Induce phase separation between polymer and solvent,
[0014] removing at least a portion of the solvent from the membrane to obtain a porous membrane,
[0015] optionally compressing the porous membrane to obtain a dense membrane,
[0016] stacking a plurality of layers of porous membranes or dense membranes one after another to obtain a membrane stack, pressing the membrane stack to obtain a bonded membrane stack, and
[0017] Sheets are cut from the bonded film stack in a direction perpendicular to the plane of the stacked film layers.
[0018] In another aspect, the present disclosure also relates to a method for producing a sheet as disclosed herein, the method comprising:
[0019] providing a polymer, a solvent, and hexagonal boron nitride particles including plate-like hexagonal boron nitride particles,
[0020] mixing a polymer, a solvent, and hexagonal boron nitride particles to form a slurry, wherein the slurry is a suspension of the polymer and the hexagonal boron nitride particles in the solvent, and wherein the polymer has a melting point, and wherein the solvent has a boiling point, and wherein the mixing of the polymer, the solvent, and the hexagonal boron nitride particles is performed at a temperature below the melting point of the polymer and below the boiling point of the solvent,
[0021] forming the slurry into a film in which the plate-like hexagonal boron nitride particles are oriented in a direction parallel to the plane direction of the film,
[0022] heating the film in an environment such that at least 90 weight percent of the solvent, based on the weight of the solvent in the film, remains in the film and at least 50 weight percent of the polymer, based on the total weight of the polymer, is dissolved in the solvent,
[0023] Induce phase separation between polymer and solvent,
[0024] removing at least a portion of the solvent from the membrane to obtain a porous membrane,
[0025] optionally compressing the porous membrane to obtain a dense membrane,
[0026] stacking a plurality of layers of porous membranes or dense membranes one after another to obtain a membrane stack, pressing the membrane stack to obtain a bonded membrane stack, and
[0027] Sheets are cut from the bonded film stack in a direction perpendicular to the plane of the stacked film layers.
[0028] The sheet materials disclosed herein comprise highly oriented boron nitride platelet-like particles and thus have highly anisotropic properties, particularly highly anisotropic thermal conductivity properties.
[0029] The films disclosed herein contain boron nitride platelet-like particles oriented perpendicular to the plane of the sheet and have high through-plane thermal conductivity.
[0030] Due to the high through-plane thermal conductivity, the sheet as disclosed herein allows for faster and more efficient removal of heat.Compared to other polymer sheets filled with boron nitride, the sheet disclosed herein has a higher through-plane thermal conductivity than the in-plane thermal conductivity.
[0031] Furthermore, the sheets disclosed herein have good dielectric properties, particularly low permittivity and low dissipation factor.
[0032] Typically, the sheets disclosed herein are free of silicone.
[0033] As used herein, "phase separation" refers to a process in which particles are uniformly dispersed in a homogeneous polymer-solvent solution that is transformed (e.g., by changes in temperature or solvent concentration) into a continuous three-dimensional composite material, i.e., a polymer matrix composite material. In the first method disclosed herein, phase separation is achieved by using a wet or dry solvent-induced phase separation (SIPS) or thermally induced phase separation (TIPS) method. In the second method disclosed herein, the desired article (i.e., film) is formed before the polymer becomes miscible with the solvent, and the phase separation is a thermally induced phase separation method.
[0034] As used herein, "miscible" refers to the ability of substances to mix in all proportions (i.e., completely dissolve in each other at any concentration) to form solutions, wherein for certain solvent-polymer systems, heat may be required to miscible the polymer and solvent. Conversely, substances are immiscible if a significant portion does not form a solution. For example, butanone is significantly soluble in water, but the two solvents are immiscible because they do not dissolve in all proportions.
[0035] Typically, based on the volume of particles and binder, the maximum particle loading that can be achieved in a composite material (compact polymer film, adhesive, etc.) filled with traditional particles is no more than about 40 volume % to 60 volume %. It is usually not achievable to incorporate particles exceeding 60 volume % into a traditional particle-filled composite material because such high particle-loaded materials cannot be processed via a coating or extrusion method and / or the resulting composite material becomes very fragile. Traditional composite materials are also usually completely encapsulated with binders to prevent access to the particle surface and minimize potential particle-particle contact. Typically, the thermal conductivity of the composite material filled with thermally conductive particles increases with the increase of particle loading, so that a higher particle loading can be expected. Surprisingly, the high content of solvent and phase separation morphology obtained with the method described herein enables a relatively high particle loading to be achieved with a relatively low amount of high molecular weight binder. Although not wanting to be limited by theory, it is believed that another advantage of the embodiment of the composite material described herein is that the particles are not completely coated with a binder, so that a high degree of particle surface contact can be achieved without being masked by the porous nature of the binder. The compression of the film significantly enhances the contact of the particles with the particles. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] The present disclosure is explained in more detail on the basis of the accompanying drawings, in which
[0037] Figure 1a and Figure 1b showing a scanning electron micrograph of a cross-section of a sheet as disclosed herein; and
[0038] Figure 2The stacking and slicing steps of a method for producing a sheet material as disclosed herein are schematically shown. DETAILED DESCRIPTION
[0039] The sheet material disclosed herein comprises a composite material comprising hexagonal boron nitride particles. The hexagonal boron nitride particles comprise flaky hexagonal boron nitride particles. The flaky hexagonal boron nitride particles may also be referred to as flake-like or scale-like hexagonal boron nitride particles.
[0040] The plate-like hexagonal boron nitride particles have a basal plane. The basal plane of the plate-like hexagonal boron nitride particles is oriented perpendicular to the plane of the sheet. In other words, in the sheet as disclosed herein, the plate-like hexagonal boron nitride particles are oriented in a direction perpendicular to the plane direction of the sheet.
[0041] The orientation in the direction perpendicular to the plane direction of the sheet was confirmed by scanning electron microscopy and by X-ray diffraction measurements, indicating that the hexagonal boron nitride particles in the composite material were oriented in the direction perpendicular to the plane direction of the sheet.
[0042] Typically, at least 50% by weight of the hexagonal boron nitride particles are flaky hexagonal boron nitride particles, based on the total weight of the hexagonal boron nitride particles. Preferably, at least 80% by weight of the hexagonal boron nitride particles are flaky hexagonal boron nitride particles, based on the total weight of the hexagonal boron nitride particles. It is also possible that all hexagonal boron nitride particles are flaky. A portion or even all of the flaky hexagonal boron nitride particles may be agglomerated into boron nitride agglomerates. The flaky hexagonal boron nitride particles may also be non-agglomerated.
[0043] Sheet material disclosed herein comprises composite material, and this composite material comprises polymer.In some embodiments, polymer can be selected from the group consisting of: polyurethane, polyester, polyamide, polyether, polycarbonate, polyimide, polysulfone, polyethersulfone, polyphenylene oxide, polyacrylate, polymethacrylate, polyacrylonitrile, polyolefin, styrene, copolymer based on styrene, styrene-based copolymer, chlorinated polymer, fluorinated polymer, copolymer of ethylene and trifluorochloroethylene and their combination.Copolymer based on styrene can be random copolymer based on styrene, or block copolymer based on styrene.Polyolefin can be ultra-high molecular weight polyethylene (UHMWPE) or polypropylene.
[0044] The polymer can comprise, consist essentially of, or consist of at least one thermoplastic polymer. Exemplary thermoplastic polymers include polyurethanes, polyesters (e.g., polyethylene terephthalate, polybutylene terephthalate, and polylactic acid), polyamides (e.g., nylon 6, nylon 6,6, nylon 12, and polypeptides), polyethers (e.g., polyethylene oxide and polypropylene oxide), polycarbonates (e.g., bisphenol A-polycarbonate), polyimides, polysulfones, polyethersulfones, polyphenylene oxides, polyacrylates (e.g., thermoplastic polymers formed by addition polymerization of one or more monomers containing acrylate functional groups), polymethacrylates (e.g., thermoplastic polymers formed by addition polymerization of one or more monomers containing methacrylate functional groups), polyolefins (e.g., polyethylene and polypropylene), styrene and styrene-based random and block polymers, chlorinated polymers (e.g., polyvinyl chloride), fluorinated polymers (e.g., polyvinylidene fluoride; copolymers of tetrafluoroethylene, hexafluoropropylene, and vinylidene fluoride; copolymers of ethylene and tetrafluoroethylene; hexafluoropropylene; and polytetrafluoroethylene), and copolymers of ethylene and chlorotrifluoroethylene. In some embodiments, the thermoplastic polymer comprises a homopolymer or a copolymer (e.g., a block copolymer or a random copolymer). In some embodiments, the thermoplastic polymer comprises a mixture of at least two thermoplastic polymer types (e.g., a mixture of polyethylene and polypropylene or a mixture of polyethylene and polyacrylate). In some embodiments, the thermoplastic polymer may be at least one of polyethylene (e.g., ultra-high molecular weight polyethylene), polypropylene (e.g., ultra-high molecular weight polypropylene), polylactic acid, poly(ethylene co-chlorotrifluoroethylene), and polyvinylidene fluoride. In some embodiments, the thermoplastic polymer is a single thermoplastic polymer (i.e., it is not a mixture of at least two thermoplastic polymer types). In some embodiments, the thermoplastic polymer consists essentially of polyethylene (e.g., ultra-high molecular weight polyethylene), or consists of it.
[0045] In some embodiments, the thermoplastic polymer used to prepare the composite material of the sheets disclosed herein is a particle size less than 1000 microns (in some embodiments, in the range of 1 micron to 10 microns, 10 microns to 30 microns, 10 microns to 50 microns, 30 microns to 100 microns, 10 microns to 200 microns, 10 microns to 500 microns, 100 microns to 200 microns, 200 microns to 500 microns, 500 microns to 1000 microns).
[0046] In some embodiments, the polymer used to prepare the composite material of the sheet disclosed herein has a 4 g / mol to 1×10 7 g / mol (in some embodiments, in the range of 1×10 6 g / mol to 8×10 6g / mol, 2×10 6 g / mol to 6×10 6 g / mol or even 2×10 6 g / mol to 5×10 6 g / mol range). For the purposes of this disclosure, the number average molecular weight can be measured by known techniques in the art (e.g., gel permeation chromatography (GPC)). GPC can be carried out in a suitable solvent for a thermoplastic polymer, together with the use of a narrow molecular weight distribution polymer standard (e.g., a narrow molecular weight distribution polystyrene standard). Thermoplastic polymers are generally characterized as partially crystalline, exhibiting a melting point. In some embodiments, the melting point of a thermoplastic polymer can be in the range of 120°C to 350°C (in some embodiments, in the range of 120°C to 300, 120°C to 250°C, or even 120°C to 200°C). The melting point of a thermoplastic polymer can be measured by techniques known in the art (e.g., a set temperature measured in a differential scanning calorimetry (DSC) test at a heating scan rate of 10°C / min with a 5 mg to 10 mg sample, while the sample is under a nitrogen atmosphere).
[0047] In some embodiments, the polymer used to prepare the composite material of the sheet disclosed herein is ultra high molecular weight polyethylene (UHMWPE), which has a molecular weight of 5×10 4 g / mol to 1×10 7 g / mol (in some embodiments, in the range of 1×10 6 g / mol to 8×10 6 g / mol, 2×10 6 g / mol to 6×10 6 g / mol or even 2×10 6 g / mol to 5×10 6 g / mol range).
[0048] The hexagonal boron nitride particles are dispersed in the polymer, i.e., the polymer is the matrix material of the hexagonal boron nitride particles. The hexagonal boron nitride particles have direct contact between particles in the composite material, i.e., a continuous path of the thermally conductive hexagonal boron nitride particles is formed in the composite material. The direct contact and continuous path between particles of the thermally conductive hexagonal boron nitride particles are demonstrated by the high through-plane thermal conductivity of the composite material of the sheet.
[0049] The degree of orientation of the flaky hexagonal boron nitride particles in the film can be characterized by an orientation index measured on a sheet sample. The value of the orientation index of hexagonal boron nitride with isotropic orientation (and therefore no preferred orientation) of the flaky hexagonal boron nitride particles is 1. For flaky hexagonal boron nitride particles oriented parallel to the sheet plane, the orientation index decreases with the degree of parallel orientation in the sheet sample and has a value less than 1. For flaky hexagonal boron nitride particles oriented perpendicular to the sheet plane, the orientation index increases with the degree of perpendicular orientation in the sheet sample and has a value greater than 1. As used herein, "flaky hexagonal boron nitride particles are oriented perpendicular to the sheet plane" should be understood as an orientation index greater than 4.0. As used herein, "flaky hexagonal boron nitride particles are oriented parallel to the sheet plane" should be understood as an orientation index of at most 0.5.
[0050] The orientation index of the sheet as disclosed herein is greater than 4.0. The orientation index of the sheet may be at least 4.5, or at least 5, or at least 6, or at least 7, or at least 8, or at least 10. Preferably, the orientation index of the sheet is at least 6.
[0051] The orientation index is determined by X-ray diffraction. To this end, the ratio of the (100) reflection intensity to the (002) reflection intensity of hexagonal boron nitride (hBN) measured on the X-ray diffraction pattern of the sheet sample is determined and divided by the corresponding ratio of an ideal, unoriented (i.e., isotropic) hBN sample. This ideal ratio can be determined from the powder diffraction pattern (PDF) #01-073-2095 of the International Center for Diffraction Data (ICDD) data (2020) and is 0.147. The theoretical peak positions of the (002) reflection and the (100) reflection are at 26.7 degrees and 41.6 degrees, respectively. The peak intensities of the (002) reflection and the (100) reflection are measured from the peak areas at these positions. The orientation index (OI) can be determined by the following formula:
[0052]
[0053] The composite material comprises at least 70 weight percent of the hexagonal boron nitride particles, based on the total weight of the composite material.
[0054] Based on the total weight of the composite material, the composite material may contain at least 80 wt%, or at least 85 wt%, or at least 90 wt%, or greater than 90 wt%, or at least 91 wt%, or at least 92 wt%, or at least 93 wt%, or at least 94 wt%, or at least 95 wt%, or at least 96 wt% of hexagonal boron nitride particles.
[0055] Based on the total weight of the composite material, the composite material may include 70 wt % to 98 wt %, or 80 wt % to 98 wt %, or 85 wt % to 98 wt %, or 90 wt % to 98 wt %, or more than 90 wt % to 98 wt %, or 91 wt % to 98 wt %, or 92 wt % to 98 wt %, or 93 wt % to 98 wt %, or 94 wt % to 98 wt %, or 95 wt % to 98 wt %, or 96 wt % to 98 wt % of hexagonal boron nitride particles.
[0056] Based on the gross weight of the composite material, the composite material may include at least 2 wt % of the polymer. Based on the gross weight of the composite material, the composite material may include up to 30 wt % or up to 20 wt % of the polymer. Based on the gross weight of the composite material, the composite material may include 2 wt % to 30 wt %, or 2 wt % to 20 wt %, or 2 wt % to 15 wt %, or 2 wt % to 10 wt %, or 2 wt % to 9 wt %, or 2 wt % to 8 wt %, or 2 wt % to 7 wt %, or 2 wt % to 6 wt %, or 2 wt % to 5 wt %, or 2 wt % to 4 wt % of the polymer.
[0057] The sheets disclosed herein have a through-plane thermal conductivity greater than 12 W / m*K. The through-plane thermal conductivity of the sheet may be at least 15 W / m*K, or at least 18 W / m*K, or at least 20 W / m*K, or at least 25 W / m*K, or at least 30 W / m*K, or at least 35 W / m*K, or at least 40 W / m*K, or at least 45 W / m*K, or at least 50 W / m*K. The through-plane thermal conductivity may be greater than 12 W / m*K to 25 W / m*K, or greater than 12 W / m*K to 65 W / m*K, or 15 W / m*K to 25 W / m*K, or 15 W / m*K to 65 W / m*K, or 20 W / m*K to 65 W / m*K, or 30 W / m*K to 65 W / m*K, or 40 W / m*K to 65 W / m*K.
[0058] The through-plane thermal conductivity of the sheet is higher than the in-plane thermal conductivity of the sheet. Typically, the ratio of the through-plane thermal conductivity to the in-plane thermal conductivity of the sheet is at least 2, and may be at least 3, or at least 4, or at least 5.
[0059] The through-plane thermal conductivity of the sheet can be measured using the laser flash analysis method according to ASTM E1461 (2013). The through-plane thermal conductivity can also be measured according to ASTM D-5470-17 (Standard Test Method for Thermal Interface Materials). The through-plane thermal conductivity can be measured on a sheet sample.
[0060] The in-plane thermal conductivity of the sheet may be at least 2 W / m*K. The in-plane thermal conductivity of the sheet may be measured using a laser flash analysis method according to ASTM E1461 (2013).
[0061] The composite material contained in the sheet material disclosed herein may be electrically insulating. The resistivity of the composite material contained in the sheet material may be at least 1×10 10 Ω*m.
[0062] The average particle size (d 50 ) may be 0.5 μm to 500 μm, or 3 μm to 500 μm.
[0063] The average particle size (d 50 ) may be 0.5 μm to 100 μm, or 3 μm to 100 μm.
[0064] Preferably, the average particle size (d 50 ) is at least 5 μm, more preferably at least 8 μm. In some embodiments, the average particle size (d 50 ) is 5 μm to 50 μm, or 5 μm to 30 μm, or 8 μm to 30 μm, or 30 μm to 60 μm, or 40 μm to 50 μm, or 8 μm to 15 μm, or 10 μm to 12 μm. The average particle size (d 50 ) can be measured by laser diffraction.
[0065] The average aspect ratio of the flaky hexagonal boron nitride particles is generally at least 5. The aspect ratio is the ratio of the diameter to the thickness of the flaky hexagonal boron nitride particles. As used herein, flaky hexagonal boron nitride particles are also referred to as boron nitride sheets. The aspect ratio of the boron nitride sheets may be at least 10, or at least 15, or at least 20. The average aspect ratio of the boron nitride sheets may also be at most 40, or at most 100. The average aspect ratio of the boron nitride sheets may be 7 to 20, or 20 to 40, or 7 to 40, or 10 to 40, or 50 to 100, or 5 to 500. Typically, the average aspect ratio of the boron nitride sheets is at most 500. The average aspect ratio can be measured by a scanning electron microscope (SEM), by determining the aspect ratio of 20 particles, and calculating the average of the 20 individual values determined. The aspect ratio of a single boron nitride sheet is determined by measuring the diameter and thickness of the boron nitride sheet and calculating the ratio of the diameter to the thickness. The required magnification of the SEM images for measuring the diameter and thickness of the boron nitride flakes depends on the size of the flakes. The magnification should be at least 1000x, preferably at least 2000x. Where appropriate, i.e. for the average particle size (d 50 ) For smaller pieces ranging from 5 μm to 10 μm, a magnification of 5000x should be used.
[0066] The hexagonal boron nitride particles may include agglomerates of hexagonal boron nitride primary particles, which primary particles include flaky hexagonal boron nitride particles. The hexagonal boron nitride particles may also be composed of agglomerates of hexagonal boron nitride primary particles, which primary particles include flaky hexagonal boron nitride particles. Agglomerates of primary particles of hexagonal boron nitride may also be referred to as "boron nitride agglomerates". The average particle size (d 50 ) may be at most 500 μm, or at most 250 μm, or at most 150 μm, or at most 100 μm. The average particle size (d 50 ) may be at least 20 μm, at least 30 μm or at least 50 μm. The average particle size (d 50 ) may be 20 μm to 500 μm, or 20 μm to 400 μm, or 30 μm to 500 μm, or 30 μm to 300 μm, or 50 μm to 400 μm, or 30 μm to 50 μm, or 50 μm to 100 μm, or 100 μm to 150 μm, or 100 μm to 200 μm, or 200 μm to 400 μm. The average particle size (d 50 ) may be 3 μm to 50 μm, or 3 μm to 30 μm, or 5 μm to 30 μm, or 8 μm to 30 μm, or 8 μm to 15 μm, or 10 μm to 15 μm, or 10 μm to 12 μm. The average particle size (d 50 ) can be measured by laser diffraction. Boron nitride agglomerates can have any shape, such as spherical, irregular or flake-like. Flake-like agglomerates can have an aspect ratio of 1 to 20.
[0067] In some embodiments, the hexagonal boron nitride particles may comprise or consist of agglomerates of primary particles of hexagonal boron nitride, the primary particles comprising plate-like hexagonal boron nitride particles, wherein the average particle size (d 50 ) is 30 μm to 300 μm, and wherein the average particle size (d 50 ) is 8μm to 15μm.
[0068] In some embodiments, if boron nitride agglomerates are used as hexagonal boron nitride particles, the agglomerates may be partially or completely decomposed into primary particles in the final product (i.e., sheet). In some embodiments, if boron nitride agglomerates are used as hexagonal boron nitride particles, such as flake-shaped boron nitride agglomerates, a portion or all of the agglomerates may still exist in the final product in the form of agglomerates, i.e., the agglomerates may not be decomposed into primary particles in the sheet.
[0069] The hexagonal boron nitride particles may also include non-agglomerated flaky hexagonal boron nitride particles. The hexagonal boron nitride particles may also consist of non-agglomerated flaky hexagonal boron nitride particles. The average particle size (d50 ) may be 3 μm to 100 μm, preferably 5 μm to 30 μm. The average particle size (d 50 ) may also be 10 μm to 100 μm, or 10 μm to 50 μm, or 30 μm to 70 μm, or 30 μm to 60 μm, or 40 μm to 50 μm.
[0070] In some embodiments, a mixture of agglomerated and unagglomerated platelet-shaped hexagonal boron nitride particles may be used.
[0071] Composite materials and sheets may have a porosity of up to 40%, or up to 30%, or up to 20%. Composite materials and sheets may have a porosity of at least 1%, or at least 2%, or at least 3%, or at least 4%, or at least 5%, or at least 8%, or at least 10%. In some embodiments, composite materials and sheets have a porosity of 0.5% to 40%, or 0.5% to 30%, or 0.5% to 20%, or 1% to 40%, or 1% to 30%, or 1% to 20%, or 2% to 40%, or 2% to 30%, or 2% to 20%, or 5% to 40%, or 5% to 30%, or 5% to 20%. In some embodiments, composite materials and sheets have a porosity of 0%.
[0072] The density of the composite material and the sheet material may be at least 60%, or at least 70%, or at least 80%, or even at least 90% of the theoretical density. The density of the composite material and the sheet material may be at most 100%, or at most 99.5%, or at most 99%, or at most 98%, or at most 97%, or at most 96%, or at most 95%, or at most 92%, or at most 90% of the theoretical density. The density of the composite material and the sheet material can be 60% to 95%, or 70% to 95%, or 80% to 95%, or 60% to 98%, or 70% to 98%, or 80% to 98%, or 60% to 99%, or 70% to 99%, or 80% to 99%, or 60% to 99.5%, or 70% to 99.5%, or 80% to 99.5%, or 60% to 100%, or 70% to 100%, or 80% to 100% of the theoretical density. The theoretical density can be calculated from the known densities of the components of the composite material and the sheet material and the weight fractions of the components.
[0073] The composite materials and sheets included in the sheet materials disclosed herein have good dielectric properties. Typically, the composite materials and sheets have a dielectric loss factor (Df) of at most 0.009 at 5.2 GHz, and can be 0.0001 to 0.009 at 5.2 GHz. The dielectric constant or relative permittivity (Dk) of the composite materials and sheets is typically at most 5.0 at 5.2 GHz, and can be 2.0 to 4.0 at 5.2 GHz.
[0074] The presence of pores in the composite and sheet material can improve the dielectric properties of the composite and sheet material. In addition, the presence of pores in the composite and sheet material allows the composite and sheet material to be compressible, which may be desirable for some applications. The pores in the composite and sheet material should be of small size and uniformly distributed in the composite and sheet material.
[0075] In some embodiments of the sheets disclosed herein, the composite material contained in the sheet does not contain fibers, such as carbon fibers, glass fibers, or fibers made of other materials.
[0076] The sheets disclosed herein may have a Shore D hardness of up to 150. The Shore D hardness of the sheet may be from 20 to 150, or from 30 to 150, or from 30 to 100. The sheet may also have a lower or higher hardness.
[0077] The thickness of the sheets disclosed herein may be from 0.01 mm to 6 mm, or from 0.05 mm to 6 mm, or from 0.1 mm to 3 mm, or from 0.5 mm to 2 mm. The size of the hexagonal boron nitride particles may be selected according to the film thickness.
[0078] The width and length of the sheet can be up to several inches (e.g., 1 inch, 5 inches, 10 inches, 50 inches) or more. Typically, the sheet has a constant thickness across the width and length of the sheet. The sheet can also have a variable thickness, i.e., the thickness of the sheet is not constant across the width and length of the sheet.
[0079] The composite material may also contain additional thermally conductive fillers such as alumina or other fillers.
[0080] In some embodiments of the sheet disclosed herein, the composite material may also include an organic liquid. Based on the total weight of the composite material, the amount of the organic liquid included in the composite material may be 0.1 wt % to 10 wt %. Useful organic liquids that may be included in the composite material are non-volatile organic liquids that have enough surface energy to wet the pores or remain in the pores. The organic liquid that may be included in the composite material may be, for example, at least one of mineral oil, paraffin oil / wax, orange oil, vegetable oil, castor oil or palm kernel oil. The organic liquid included in the composite material may reduce the hardness of the composite material and the sheet material and make it softer.
[0081] Small amounts of other additives may be added to the composite to impart additional functionality or to act as processing aids. These include viscosity modifiers (e.g., fumed silica, block copolymers, and waxes), plasticizers, heat stabilizers (e.g., such as, for example, commercially available under the trade name "Irganox 1010" from BASF, Ludwigshafen, Germany), antimicrobial agents (e.g., silver and quaternary ammonium), flame retardants, antioxidants, dyes, pigments, and ultraviolet (UV) stabilizers. Thermally conductive particles such as those having a low particle size (e.g., an average particle size (d 50 Carbon or hexagonal boron nitride with a particle size of less than 1 μm can also be used as a viscosity modifier.
[0082] Optionally, elastomer can be added to composite material to improve the elasticity of composite material, i.e. reduce its brittleness. Any elastomer that can be mixed with polymer and hexagonal boron nitride particles or blended therein can be used. Suitable elastomer is, for example, Santoprene 8211-35 derived from Celanese (Irving, TX, US) , Kraton 1645 derived from Kraton (Houston, TX, US) , Vector thermoplastic elastomer 2518 derived from TSRC Corporation (Taiwan, China) , Kraton D11671 PT derived from Kraton (Houston, TX, US) and Pebax 4033 derived from Arkema (Colombes, France) .
[0083] In some embodiments of the sheets disclosed herein, the composite material comprises at least 70 wt%, or at least 80 wt%, or at least 85 wt%, or at least 90 wt%, or greater than 90 wt%, or at least 91 wt%, or at least 92 wt% of hexagonal boron nitride particles, based on the total weight of the composite material, and the composite material has a porosity of at least 2%, preferably 2% to 30%.
[0084] In some embodiments of the sheets disclosed herein, the composite material comprises at least 70 wt%, or at least 80 wt%, or at least 85 wt%, or at least 90 wt%, or greater than 90 wt%, or at least 91 wt%, or at least 92 wt% of hexagonal boron nitride particles, based on the total weight of the composite material, and the sheet material has a through-plane thermal conductivity of at least 15 W / m*K, or at least 20 W / m*K.
[0085] In some embodiments of the sheets disclosed herein, the composite comprises at least 70 wt%, or at least 80 wt%, or at least 85 wt%, or at least 90 wt%, or greater than 90 wt%, or at least 91 wt%, or at least 92 wt% of hexagonal boron nitride particles, based on the total weight of the composite, and the sheet has an orientation index of at least 6, or at least 8, or at least 10.
[0086] In some embodiments of the sheets disclosed herein, the composite comprises at least 70 wt%, or at least 80 wt%, or at least 85 wt%, or at least 90 wt%, or greater than 90 wt%, or at least 91 wt%, or at least 92 wt% of hexagonal boron nitride particles, based on the total weight of the composite, and the composite has a porosity of at least 2%, preferably 2% to 30%, and the sheet has a through-plane thermal conductivity of at least 15 W / m*K, or at least 20 W / m*K, and the sheet has an orientation index of at least 6, or at least 8, or at least 10.
[0087] In some embodiments of the sheet materials disclosed herein, the hexagonal boron nitride particles comprise or consist of non-agglomerated plate-like hexagonal boron nitride particles having an average particle size (d ) of 3 μm to 100 μm, preferably 5 μm to 30 μm. 50 ).
[0088] In some embodiments of the sheet materials disclosed herein, the hexagonal boron nitride particles comprise agglomerates of primary particles of hexagonal boron nitride, and the primary particles comprise plate-like hexagonal boron nitride particles, and the average particle size (d 50 ) is 30 μm to 500 μm, and the average particle size (d 50 ) is 3μm to 50μm.
[0089] Typically, the composites and sheets of sheet material disclosed herein do not contain silicone.
[0090] The composite materials of the sheets disclosed herein are obtained by densifying a material comprising a porous polymer network.
[0091] First method
[0092] A first method for producing a sheet as disclosed herein comprises:
[0093] providing a polymer, a solvent, and hexagonal boron nitride particles including platelet-shaped hexagonal boron nitride particles;
[0094] A polymer, a solvent and hexagonal boron nitride particles are mixed to form a suspension of the hexagonal boron nitride particles in a polymer-solvent solution; wherein the polymer in the polymer-solvent solution has a melting point, and wherein the solvent has a boiling point, and wherein the mixing of the polymer, the solvent and the hexagonal boron nitride particles is performed at a temperature above the melting point of the polymer in the polymer-solvent solution and below the boiling point of the solvent,
[0095] forming the suspension into a film in which plate-like hexagonal boron nitride particles are oriented in a direction parallel to a planar direction of the film;
[0096] Inducing phase separation of polymer and solvent;
[0097] removing at least a portion of the solvent from the membrane to obtain a porous membrane;
[0098] optionally compressing the porous membrane to obtain a dense membrane;
[0099] stacking a plurality of layers of porous membranes or dense membranes one on top of another to obtain a membrane stack;
[0100] pressing the membrane stack to obtain a bonded membrane stack; and
[0101] Sheets are cut from the bonded film stack in a direction perpendicular to the plane of the stacked film layers.
[0102] To produce the sheets disclosed herein by the first method, the polymer and hexagonal boron nitride particles as described in more detail above may be used.
[0103] The solvent is typically selected so that it can dissolve the polymer and form a polymer-solvent solution, i.e., the solvent needs to be miscible with the polymer. [Can it?] Yes, heating the solution to an elevated temperature can promote the dissolution of the polymer. In some embodiments, the mixing of the polymer and the solvent is performed at a temperature in the range of 20°C to 350°C. The hexagonal boron nitride particles may be added at any or all of the mixing, before the polymer is dissolved, after the polymer is dissolved, or at any time in between.
[0104] The solvent is selected so that it forms a polymer-solvent solution. The solvent can be a blend of at least two separate solvents. In some embodiments, when the polymer is a polyolefin (such as at least one of polyethylene and polypropylene), the solvent can be such as at least one of the following: mineral oil, tetralin, decalin, o-dichlorobenzene, cyclohexane toluene mixture, dodecane, paraffin oil / wax, kerosene, isoparaffin fluid, o-xylene / cyclohexane mixture (1 / 1 weight / weight), camphene, 1,2,4 trichlorobenzene, octane, orange oil, vegetable oil, castor oil or palm kernel oil. In some embodiments, when the polymer is polyvinylidene fluoride, the solvent can be such as at least one of ethylene carbonate, propylene carbonate or 1,2,3-triacetoxypropane.
[0105] The polymer, solvent and hexagonal boron nitride particles may be mixed using conventional mixing aggregates such as a twin-screw extruder, a planetary extruder, a conical twin-screw extruder, a kneader, or an industrial mixer such as, but not limited to, a double planetary mixer.
[0106] In some embodiments of the first method, the polymer in the polymer-solvent solution has a melting point, and the solvent has a boiling point, and the mixing of the polymer, the solvent, and the hexagonal boron nitride particles can be performed at a temperature higher than the melting point of the polymer in the polymer-solvent solution and lower than the boiling point of the solvent. By mixing the polymer, the solvent, and the hexagonal boron nitride particles, a suspension of the hexagonal boron nitride particles in the polymer-solvent solution is formed.
[0107] After forming a suspension of hexagonal boron nitride particles in a polymer-solvent solution, the suspension is formed into a film. In the film, the flaky hexagonal boron nitride particles are oriented in a direction parallel to the planar direction of the film. The film can be a continuously formed film, or a film or layer comprising a micro-replication or macro-replication structure and made by micro-replication or micro-replication technology. The formation of the film can be carried out using techniques known in the art, including scraping, roller coating (e.g., roller coating by defining a roller gap) and extrusion (e.g., extrusion through a die (e.g., extrusion through a die with an appropriate layer size (i.e., the width and thickness of the die gap))).
[0108] In an exemplary embodiment, the polymer-solvent solution has a paste-like consistency and is formed into a film by extrusion, such as through a die having appropriate layer dimensions (ie, width and thickness of the die gap).
[0109] After the suspension is formed into a film in which the polymer is miscible in its solvent, the polymer phase separation can then be induced. Several techniques can be used to induce phase separation, including at least one of thermally induced phase separation or solvent induced phase separation. When the temperature for inducing phase separation is lower than the mixing temperature of the polymer, solvent and hexagonal boron nitride particles, thermally induced phase separation can occur. If the mixing is carried out at near room temperature, this can be achieved by cooling the polymer-solvent solution, or by first heating the polymer-solvent solution to an elevated temperature (during mixing or after mixing), and then reducing the temperature of the polymer-solvent solution, thereby inducing the phase separation of the polymer. In both cases, cooling can cause the polymer to separate from the solvent. Solvent-induced phase separation can be performed by adding a second solvent that is a poor solvent for the polymer to the polymer-solvent solution, or solvent-induced phase separation can be achieved by removing at least a portion of the solvent of the polymer-solvent solution (e.g., evaporating at least a portion of the solvent of the polymer-solvent solution), thereby inducing the phase separation of the polymer. A combination of phase separation techniques (e.g., thermally induced phase separation and solvent-induced phase separation) can be used. Thermally induced phase separation can be advantageous because it also facilitates dissolution of the polymer when mixing is performed at elevated temperatures. In some embodiments, thermally induced phase separation is performed at a temperature in the range of 5°C to 300°C (in some embodiments, in the range of 5°C to 250°C, 5°C to 200°C, 5°C to 150°C, 15°C to 300°C, 15°C to 250°C, 15°C to 200°C, 15°C to 130°C, or even 25°C to 110°C) below the mixing temperature.
[0110] In some embodiments of the first method, the polymer in the polymer-solvent solution has a melting point, and inducing phase separation is performed at a temperature below the melting point of the polymer in the polymer-solvent solution.
[0111] During the induced phase separation, a polymer network structure can be formed. In some embodiments, thermal induction (e.g., by quenching to a lower temperature of thermally induced phase separation (TIPS)), chemical induction (e.g., by replacing a bad solvent with a good solvent, solvent induced phase separation (SIPS)) or solvent ratio changes (e.g., by evaporating one of the solvents) induce phase separation. Other phase separation or pore formation techniques known in the art can also be used, such as discontinuous polymer blending (sometimes also referred to as polymer-assisted phase inversion (PAPI)), moisture-induced phase separation or steam-induced phase separation. The polymer network structure can be inherently porous (i.e., having holes). The pore structure can be open so that fluid communication can be performed from the internal region of the polymer network structure to the outer surface of the polymer network structure and / or between the first surface of the polymer network structure and the opposing second surface of the polymer network structure.
[0112] The polymer network structure can be described as a porous polymer network or a porous phase-separated polymer network. Generally speaking, the porous polymer network (as prepared) includes an interconnected porous polymer network structure, which comprises a plurality of interconnected morphologies (e.g., at least one of fibrils, nodules, nodes, open pores, closed pores, foliate lace, strands, spheres, or honeycomb structures). The interconnected polymer structure can be directly adhered to the surface of the hexagonal boron nitride particles and act as a binder for the hexagonal boron nitride particles. In this regard, in contrast to the solid matrix material, the space between adjacent hexagonal boron nitride particles (e.g., primary particles or agglomerates) can include a porous polymer network structure.
[0113] In some embodiments, the polymer network structure may include a three-dimensional mesh structure that includes an interconnected network of polymer fibrils. In some embodiments, the average width of a single fibril is in the range of 10 nm to 100 nm (in some embodiments, in the range of 100 nm to 500 nm, or even 500 nm to 5 microns).
[0114] In some embodiments, the hexagonal boron nitride particles are dispersed in the polymer network structure so that the outer surface of each unit of the hexagonal boron nitride particles (e.g., a single particle or a single agglomerate particle) is mostly not in contact with the polymer network structure or is not coated. In this regard, in some embodiments, based on the total surface area of the outer surface of the single particle, the average area coverage percentage of the polymer network structure on the outer surface of the single particle (i.e., the percentage of the outer surface area in direct contact with the polymer network structure) is not greater than 50% (in some embodiments, not greater than 40%, 30%, 25%, 20%, 10%, 5% or even not greater than 1%). Although not wanting to be bound by theory, it is believed that the large uncontacted surface area coating on the hexagonal boron nitride particles can increase the contact between the particles after compression, and thus increase thermal conductivity.
[0115] After the polymer and solvent are phase separated by the phase separation induction step, at least a portion of the solvent can be removed from the membrane (ie, from the polymer network structure of the membrane) to form a porous membrane. The porous membrane has a polymer network structure, and the hexagonal boron nitride particles are distributed in the polymer network structure.
[0116] The solvent (for example, the first solvent) can be removed by evaporation, and high vapor pressure solvents are particularly suitable for this removal method. However, if the first solvent has a low vapor pressure, it may be desirable to extract the first solvent with a second solvent having a higher vapor pressure, and then evaporate the second solvent. In some embodiments, the solvent and the second solvent (if used) can be removed from the film in the range of 10 wt % to 100 wt % (in some embodiments, in the range of 20 wt % to 100 wt %, 30 wt % to 100 wt %, 40 wt % to 100 wt %, 50 wt % to 100 wt %, 60 wt % to 100 wt %, 70 wt % to 100 wt %, 80 wt % to 100 wt %, 90 wt % to 100 wt %, 95 wt % to 100 wt % or even in the range of 98 wt % to 100 wt %).
[0117] For example, in some embodiments, when mineral oil is used as the first solvent, isopropanol or a blend of methyl nonafluorobutyl ether (C4F9OCH3), ethyl nonafluorobutyl ether (C4F9OC2H5) and trans-1,2-dichloroethylene (e.g., available from 3M Company, St. Paul, MN under the trade name "NOVEC 72DE") at an elevated temperature (e.g., about 60°C) can be used as a second solvent to extract the first solvent, followed by evaporation of the second solvent. In some embodiments, when at least one of vegetable oil or palm kernel oil is used as the first solvent, isopropanol at an elevated temperature (e.g., about 60°C) can be used as the second solvent. In some embodiments, when ethylene carbonate is used as the first solvent, water can be used as the second solvent.
[0118] In some embodiments of the first method, after solvent removal, the formed and phase separated membrane has a porosity of at least 5% (in some embodiments, at least 10%, 20%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, or even at least 80%; in some embodiments, in the range of 25% to 80%). The porosity is caused by the phase separation of the polymer and the solvent, which initially does not leave unfilled voids because the pores in the polymer network structure are filled with solvent. After complete or partial removal of the solvent, pores are formed in the polymer network structure.
[0119] Typically, the polymer used in the first method disclosed herein is a thermoplastic polymer.
[0120] The thickness of the porous and dense films can be, for example, 5 mils to 150 mils (0.127 mm to 3.81 mm). The thickness of the porous and dense films can also be less than 5 mils or greater than 150 mils.
[0121] Second method
[0122] A second method for producing a sheet as disclosed herein comprises:
[0123] providing a polymer, a solvent, and hexagonal boron nitride particles including plate-like hexagonal boron nitride particles,
[0124] The polymer, solvent and hexagonal boron nitride particles are mixed (e.g., mixed or blended) to form a slurry, wherein the slurry is a suspension of the polymer and the hexagonal boron nitride particles in the solvent, and wherein the polymer has a melting point, and wherein the solvent has a boiling point, and wherein the mixing of the polymer, solvent and hexagonal boron nitride particles is performed at a temperature below the melting point of the polymer and below the boiling point of the solvent,
[0125] forming the slurry into a film in which the plate-like hexagonal boron nitride particles are oriented in a direction parallel to the plane direction of the film,
[0126] The film is heated in an environment such that at least 90 wt % (in some embodiments, at least 91 wt %, 92 wt %, 93 wt %, 94 wt %, 95 wt %, 96 wt %, 97 wt %, 98 wt %, 99 wt %, 99.5 wt %, or even 100 wt %) of the solvent is retained in the film based on the weight of the solvent in the film and at least 50 wt % (in some embodiments, at least 55 wt %, 60 wt %, 65 wt %, 70 wt %, 75 wt %, 80 wt %, 85 wt %, 90 wt %, 95 wt %, 96 wt %, 97 wt %, 98 wt %, 99 wt %, or even 100 wt %) of the polymer is dissolved in the solvent based on the total weight of the polymer,
[0127] Induce phase separation between polymer and solvent,
[0128] removing at least a portion of the solvent from the membrane (in some embodiments, at least 50%, 55%, 60%, 65%, 70%, 75%, 80%, 95%, 96%, 97%, 98%, 99%, 99.5%, or even 100% by weight of the solvent based on the weight of the solvent in the membrane) to obtain a porous membrane,
[0129] optionally compressing the porous membrane to obtain a dense membrane,
[0130] stacking a plurality of layers of porous membranes or dense membranes one after another to obtain a membrane stack, pressing the membrane stack to obtain a bonded membrane stack, and
[0131] Sheets are cut from the bonded film stack in a direction perpendicular to the plane of the stacked film layers.
[0132] Typically, the polymer used in the second method disclosed herein is a thermoplastic polymer.
[0133] To produce the sheets disclosed herein by the second method, the polymer and hexagonal boron nitride particles as described in more detail above may be used.
[0134] The solvent is typically selected so that it can dissolve the polymer and form a polymer-solvent solution, that is, the solvent needs to be miscible with the polymer. Heating the solution to an elevated temperature can facilitate the dissolution of the polymer. In some embodiments, the polymer and solvent are mixed at a temperature in the range of 20° C. to 350° C. The hexagonal boron nitride particles may be added at any or all of the mixing, before the polymer is dissolved, after the polymer is dissolved, or at any time therebetween.
[0135] In some embodiments of the second method, the solvent is a blend of at least two separate solvents. In some embodiments, when the polymer is a polyolefin (e.g., at least one of polyethylene or polypropylene), the solvent may be at least one of mineral oil, tetralin, decalin, o-dichlorobenzene, cyclohexane toluene mixture, dodecane, paraffin oil / wax, kerosene, p-xylene / cyclohexane mixture (1 / 1 weight / weight), camphene, 1,2,4 trichlorobenzene, octane, orange oil, vegetable oil, castor oil, or palm kernel oil. In some embodiments, when the polymer is polyvinylidene fluoride, the solvent is at least one of ethylene carbonate, propylene carbonate, or 1,2,3 triacetoxypropane.
[0136] The slurry can be continuously mixed or blended to prevent or reduce the settling or separation of the polymer and / or particles from the solvent. Typically, continuous mixing or blending is not required to prevent or reduce the settling or separation of the polymer and / or particles from the solvent. In some embodiments, the slurry is degassed using techniques known in the art to remove residual air.
[0137] The slurry obtained by mixing (eg, mixing or blending) a polymer, a solvent, and hexagonal boron nitride particles is a suspension of the polymer and the hexagonal boron nitride particles in the solvent.
[0138] The polymer, solvent and hexagonal boron nitride particles may be mixed using conventional mixing aggregates such as a twin-screw extruder, a planetary extruder, a conical twin-screw extruder, a kneader, or an industrial mixer such as, but not limited to, a double planetary mixer.
[0139] In some embodiments of the second method, the weight ratio of solvent to polymer is at least 9:1.
[0140] In some embodiments of the second method, the mixing is performed at a temperature below the melting point of the polymer and below the boiling point of the solvent.
[0141] The polymer provided for the method disclosed herein has a melting point, and the solvent has a boiling point. In some embodiments of the second method, mixing the polymer, the solvent and the hexagonal boron nitride particles is performed at a temperature below the melting point of the polymer and below the boiling point of the solvent. By mixing the polymer, the solvent and the hexagonal boron nitride particles, a slurry is formed, i.e., a suspension of the polymer and the hexagonal boron nitride particles in the solvent.
[0142] The slurry is formed into a film using techniques known in the art, including knife coating, roll coating (e.g., by a roller with a defined nip), and coating through any number of different dies of appropriate size or profile. These coating techniques can be performed between two liners.
[0143] In some embodiments, for ease of manufacturing, it may be desirable to form the film at room temperature.
[0144] In some embodiments of the second method, heating the film is performed at a temperature above the melting point of the miscible polymer-solvent solution and below the boiling point of the solvent.
[0145] In some embodiments of the second method, inducing phase separation is carried out at a temperature below the melting point of the polymer in the slurry. Although not wanting to be bound, it is believed that in some embodiments, the solvent used to prepare a miscible blend with the polymer can cause a melting point depression in the polymer. The melting point described herein includes any melting point depression below the polymer solvent system.
[0146] The induced phase separation occurs at a temperature below the melting point of the polymer.
[0147] During the induced phase separation, a polymer network structure can be formed. In some embodiments, (for example, thermally induced phase separation (TIPS) via quenching to a temperature lower than the temperature used during heating) thermally induced phase separation. Cooling can be provided, for example, in air, liquid or on a solid interface, and cooling can be varied to control phase separation. The polymer network structure can be inherently porous (that is, with holes). The pore structure can be open so that it is possible to communicate with fluid from the internal area of the polymer network structure to the outer surface of the polymer network structure and / or between the first surface of the polymer network structure and the opposing second surface of the polymer network structure.
[0148] The polymer network structure can be described as a porous polymer network or a porous phase-separated polymer network. Generally speaking, the porous polymer network (as prepared) includes an interconnected porous polymer network structure, which comprises a plurality of interconnected morphologies (e.g., at least one of fibrils, nodules, nodes, open pores, closed pores, foliate lace, strands, spheres, or honeycomb structures). The interconnected polymer structure can be directly adhered to the surface of the hexagonal boron nitride particles and act as a binder for the hexagonal boron nitride particles. In this regard, in contrast to the solid matrix material, the space between adjacent hexagonal boron nitride particles (e.g., primary particles or agglomerates) can include a porous polymer network structure.
[0149] The polymeric network structure may comprise a plurality of nodes interconnected by a plurality of fibrils. Typically, the nodes have a diameter of about 1 μm to 50 μm. The diameter is measured as the maximum diameter on a scanning electron micrograph of the composite material. The fibrils connecting the nodes to each other may have a diameter of 80 nm to 2000 nm and a length of 1 μm to 50 μm.
[0150] The nodes and fibrils comprise polymers. The nodes and fibrils may be composed of polymers. The hexagonal boron nitride particles may be located near or within the nodes. The hexagonal boron nitride particles may also be located near or connected to the fibrils. The fibrils may be mechanically anchored to the hexagonal boron nitride particles, or in other words, the hexagonal boron nitride particles may serve as nodes to which the fibrils are mechanically anchored. The porosity of the composite material is generated by the pores located between the fibrils.
[0151] The fibrils of the composite material included in the sheet disclosed herein are different from the fibers known in the art. Fiber is a possible macroscopic shape of the material, and generally has a length of at least 100 μm (e.g., at least 1 mm and at most 30 mm), and a plurality of fibers may be included in a non-uniform woven or braided structure. In contrast, the fibrils of the composite material included in the sheet disclosed herein are microstructures, with a typical diameter of 80 nm to 2000 nm (e.g., 80 nm to 800 nm) and a length of 1 μm to 50 μm, and each fibril is interconnected with a node.
[0152] In some embodiments, the polymer network structure may include a three-dimensional mesh structure that includes an interconnected network of polymer fibrils. In some embodiments, the average width of a single fibril is in the range of 10 nm to 100 nm (in some embodiments, in the range of 100 nm to 500 nm, or even 500 nm to 5 microns).
[0153] In some embodiments, the hexagonal boron nitride particles are dispersed in the polymer network structure so that the outer surface of each unit of the hexagonal boron nitride particles (e.g., a single particle or a single agglomerate particle) is mostly not in contact with the polymer network structure or is not coated. In this regard, in some embodiments, based on the total surface area of the outer surface of the single particle, the average area coverage percentage of the polymer network structure on the outer surface of the single particle (i.e., the percentage of the outer surface area in direct contact with the polymer network structure) is not greater than 50% (in some embodiments, not greater than 40%, 30%, 25%, 20%, 10%, 5% or even not greater than 1%). Although not wanting to be bound by theory, it is believed that the large uncontacted surface area coating on the hexagonal boron nitride particles can increase the contact between the particles after compression, and thus increase thermal conductivity.
[0154] After phase separation, at least a portion of the solvent is removed from the film. By removing at least a portion of the solvent from the film, a porous film is obtained. In some embodiments of the second method, at least 90% by weight of the solvent based on the weight of the solvent in the film is removed. Before removing at least 90% by weight of the solvent based on the weight of the solvent in the film, the film has a first volume, and after removing at least 90% by weight of the solvent based on the weight of the solvent in the film, the film has a second volume, and the difference between the first volume and the second volume (that is, (first volume minus second volume) divided by the first volume multiplied by 100) is less than 10% (in some embodiments, less than 9%, 8%, 7%, 6%, 5%, 4%, 3%, 2%, 1%, 0.75%, 0.5% or even less than 0.3%). Volatile solvents can be removed from the film, for example, by evaporating the solvent from at least one major surface of the film. Evaporation can be assisted, for example, by adding at least one of heat, vacuum or airflow. The evaporation of flammable solvents can be achieved in a solvent-grade oven. However, if the solvent (i.e., the first solvent) has a low vapor pressure, the first solvent can be extracted using a second solvent having a high vapor pressure, followed by evaporation of the second solvent. For example, in some embodiments, when mineral oil is used as the first solvent, isopropanol at an elevated temperature (e.g., about 60°C) or a blend of methyl nonafluorobutyl ether (C4F9OCH3), ethyl nonafluorobutyl ether (C4F9OC2H5) and trans-1,2-dichloroethylene (e.g., available under the trade name "NOVEC 72E" from 3M Company, St. Paul, MN) can be used as a second solvent to extract the first solvent, followed by evaporation of the second solvent. In some embodiments, when at least one of vegetable oil or palm kernel oil is used as the first solvent, isopropanol at an elevated temperature (e.g., about 60°C) can be used as the second solvent. In some embodiments, when ethylene carbonate is used as the first solvent, water can be used as the second solvent.
[0155] In some embodiments of the second method, the film has a first major surface and a second major surface, wherein the end is perpendicular to the first major surface and the second major surface, and during the removal of the solvent, the end is unconstrained. For example, this can be accomplished by drying a portion of the layer in an oven without constraints. Continuous drying can be achieved, for example, by drying a long portion of the layer supported on the strip when the long portion of the layer is transmitted through an oven. Alternatively, in order to promote the removal of non-volatile solvents, for example, a long portion of the film can be continuously transmitted through a compatible volatile solvent bath, thereby exchanging solvents and allowing the film to be dried without restriction subsequently. However, during the solvent exchange, not all non-volatile solvents need to be removed from the film. A small amount of non-volatile solvent can be retained and act as a plasticizer for polymers.
[0156] In some embodiments of the second method, after solvent removal, the formed and phase-separated membrane has a porosity of at least 5% (in some embodiments, at least 10%, 20%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, or even at least 80%; in some embodiments, in the range of 25% to 80%). The porosity is caused by the phase separation of the polymer and the solvent, which initially does not leave unfilled voids because the pores in the polymer network structure are filled with solvent. After complete or partial removal of the solvent, pores are formed in the polymer network structure.
[0157] In some embodiments of the first and second methods, after removing the solvent, up to 10% by weight of the non-volatile solvent or organic liquid remains in the porous membrane, thereby improving the elasticity of the porous membrane and the sheet made of the porous membrane. Up to 10% by weight of non-volatile organic liquid can also be added after removing the solvent.
[0158] The first and second methods optionally include compressing the porous membrane after removing at least a portion of the solvent from the membrane. By compressing the porous membrane, the porous membrane is densified. Compression of the porous membrane can be achieved, for example, by conventional calendaring methods known in the art.
[0159] By compressing the porous membrane, the polymer network structure of the porous membrane is plastically deformed. Vibrational energy can be imparted during the application of compressive force. In some embodiments, the porous membrane is in the form of a strip with infinite length, and the step of applying compressive force is performed when the strip passes through the roller gap. The tensile load can be applied during the passage through the roller gap. For example, the roller gap can be formed between two rollers, wherein at least one roller applies vibrational energy; between a roller and a strip, wherein at least one applies vibrational energy; or between two strips, wherein at least one strip applies vibrational energy. The application of compressive force and vibrational energy can be achieved in a continuous roll-to-roll manner or in a step-and-repeat manner. In other embodiments, a compressive force step is performed on a discrete layer such as between a plate and a platen, wherein at least one of the plate and the platen applies vibrational energy. In some embodiments, the vibrational energy is within the ultrasonic range (e.g., 20kHz), but other ranges are considered suitable.
[0160] The density of the dense film can be at least 60% (in some embodiments, at least 70%, at least 80%, at least 90%, or even 100%; in some embodiments, in the range of 60% to 98%, 70% to 98%, 80% to 98%, 60% to 100%, 70% to 100%, or even 80% to 100%) of the theoretical density after densification. The theoretical density can be calculated from the known densities of the components of the dense porous film and the weight fractions of the components.
[0161] By compressing the porous film, the particle-to-particle contact of the hexagonal boron nitride particles can be increased, thereby increasing the density and thermal conductivity of the film. Compressing the porous film can increase the density, which can reduce the insulating air volume (or porosity) of the film, and therefore increase the thermal conductivity. Likewise, the increased particle-to-particle contact of the hexagonal boron nitride particles can be measured by increased thermal conductivity.
[0162] By compressing the porous polymer network structure of the membrane, a membrane with a higher density and a compressed polymer network structure is obtained, wherein the hexagonal boron nitride particles are distributed within the polymer network and the contact between particles is increased.
[0163] If the porous membrane is not compressed before stacking multiple layers, pressing the membrane stack compresses the porous polymer network structure of the membrane to increase density and thermal conductivity. By pressing the membrane stack, the particle-to-particle contact of the hexagonal boron nitride particles is increased.
[0164] The through-plane thermal conductivity of the uncompressed porous film may be in the range of 0.2 W / m*K to 0.8 W / m*K, and the in-plane thermal conductivity of the uncompressed porous film may be 0.80 W / m*K to 2.0 W / m*K. The through-plane thermal conductivity of the compressed dense film may be in the range of 0.80 W / m*K to 3.5 W / m*K, and the in-plane thermal conductivity of the compressed dense film may be in the range of 4.0 W / m*K to 45 W / m*K.
[0165] The method for producing a sheet as disclosed herein, i.e., the first and second methods, comprises stacking multiple layers of porous membranes or dense membranes one after another. If the porous membrane is not densified before stacking, multiple layers of porous membranes are stacked one after another. If the porous membrane has been densified before stacking, multiple layers of dense membranes are stacked one after another. By stacking multiple layers of porous membranes or dense membranes, a membrane stack is obtained.
[0166] In order to stack a plurality of layers of the porous membrane or the dense membrane, respectively, the porous membrane or the dense membrane may be cut into membrane pieces of equal size, respectively, and the membrane pieces may be stacked.
[0167] The membrane stacks used in the first and second methods are pressed at a pressure and temperature, and for a time, sufficient to ensure that the individual membrane layers are bonded to the bonded membrane stack (ie, the bonded block).
[0168] Pressing the film stack for the first and second methods can be carried out at a temperature of at least 110°F (43°C) and typically at a temperature of up to 575°F (302°C). For example, if the polymer used to prepare the composite material of the sheet disclosed herein is ultra-high molecular weight polyethylene, pressing the film stack can be carried out at a temperature of at least 275°F (135°C), and typically at a temperature of up to 400°F (204°C). By this pressing step, a bonded film stack is obtained.
[0169] It has been found that a minimum pressing pressure is required to press the membrane stack.
[0170] Advantageously, the pressing of the film stack can be carried out at a pressing pressure of at least 2.0 MPa. By using a pressing pressure of at least 2.0 MPa, it is ensured that the layers of the film stack are bonded to each other and a bonded film stack, i.e. a bonded block, is obtained. In the bonded block, the individual film layers are seamlessly bonded to each other.
[0171] Furthermore, it has been found that by further increasing the pressing pressure to a value above the minimum pressing pressure of 2.0 MPa, the through-plane thermal conductivity of the sheet obtained after the subsequent slicing step can be significantly further increased. Without wishing to be bound by theory, it is believed that this can be explained by an increase in the particle-to-particle contact of the hexagonal boron nitride particles between the layers, i.e. the contact between the initially adjacent film layers in the bonded film stack formed during pressing.
[0172] Typically, the film stack is pressed at a press pressure of up to 40 MPa. Higher press pressures are possible but are generally not necessary, as the through-plane thermal conductivity of the sheet is generally not further increased by increasing the press pressure above 40 MPa.
[0173] Typically, the membrane stack is pressed for at least 2 minutes.
[0174] Advantageously, the pressed film stack can be carried out in the pressing direction (i.e., z direction), while the film stack is constrained in a first direction and a second direction perpendicular to the pressing direction, wherein the first direction is perpendicular to the second direction (i.e., x and y directions). For example, a mold (e.g., a steel mold) can be used to constrain the stack in the x and y directions. Another possibility is to press the film stack in the pressing direction (i.e., z direction), while constraining the film stack in a first direction perpendicular to the pressing direction (i.e., x direction), and allowing the film stack to expand in a second direction perpendicular to the pressing direction, wherein the first direction is perpendicular to the second direction (i.e., y direction).
[0175] The x-direction or the first direction perpendicular to the pressing direction is a first direction parallel to the plane of the multiple layers of the porous or dense membrane. The y-direction or the second direction perpendicular to the pressing direction is a second direction parallel to the plane of the multiple layers of the porous or dense membrane. The z-direction or the pressing direction is a direction perpendicular to the plane of the multiple layers of the porous or dense membrane.
[0176] The methods for producing the sheet material of the present disclosure, i.e., the first and second methods, as disclosed herein, may further include
[0177] The membrane stack is heated before pressing the membrane stack.
[0178] Advantageously, the film stack can be heated to a temperature of 110°F to 575°F (43°C to 302°C) before pressing the film stack. The selected temperature is generally close to or above the melting temperature of the polymer binder. For example, if the polymer used to prepare the composite material of the sheet disclosed herein is ultra-high molecular weight polyethylene, the film stack can be heated to a temperature of 275°F to 400°F (135°C to 204°C) before pressing the film stack.
[0179] By heating the film stack before pressing it, better bonding between the individual stacked film layers can be achieved.
[0180] The first and second methods include cutting sheets from the bonded film stack in a direction perpendicular to the plane of the stacked film layers.
[0181] Slicing (or cutting) can be performed by using a scraping knife. A pneumatic cylinder can be used to force the bonded film stack through the knife. The bonded film stack can be heated to make cutting easier. Force can also be applied to keep the bonded film stack pressed down against the knife.
[0182] The sheet obtained by the first and second methods comprises a composite material comprising a polymer and flaky hexagonal boron nitride particles, wherein the flaky hexagonal boron nitride particles are oriented in a direction perpendicular to the plane direction of the sheet. By the orientation of the flaky hexagonal boron nitride particles in a direction perpendicular to the plane direction of the sheet and by the high loading of the hexagonal boron nitride particles in the composite material, a sheet having a high through-plane thermal conductivity can be obtained.
[0183] The methods for producing the sheet material of the present disclosure, i.e., the first and second methods, as disclosed herein, may further include
[0184] The bonded film stack is heated before sheets are cut from the bonded film stack.
[0185] Advantageously, the bonded film stack may be heated to a temperature of 110°F to 575°F (43°C to 302°C) before the sheets are cut from the bonded film stack. The selected temperature is typically close to or above the melting temperature of the polymer binder. For example, if the polymer used to prepare the composite material of the sheet disclosed herein is ultra-high molecular weight polyethylene, the bonded film stack may be heated to a temperature of 275°F to 400°F (135°C to 204°C) before the sheets are cut from the bonded film stack.
[0186] By heating the bonded film stack before cutting sheets from the bonded film stack, the bonded film stack is softened, which makes slicing easier.
[0187] Figure 1a and Figure 1b Shown is a scanning electron micrograph (SEM) of a cross-section of a sheet as disclosed herein. Figure 1b yes Figure 1a A magnified detail of Figure 1b In the embodiment, the flake-shaped hexagonal boron nitride particles 1 are distributed in the network of the polymer material 2 in the sheet. The flake-shaped hexagonal boron nitride particles 1 have an orientation perpendicular to the plane direction of the sheet. The direction perpendicular to the plane direction of the sheet is Figure 1a Indicated by white arrows (through-plane direction).
[0188] exist Figure 2 In the diagram, it is schematically shown that multiple layers of dense membranes are stacked one after another to obtain a membrane stack, and sheets are cut from the bonded membrane stack in a direction perpendicular to the plane of the stacked membrane layers. In the first step of the method disclosed herein, a porous membrane 3 is formed, which contains plate-like hexagonal boron nitride particles 1 oriented in a direction parallel to the plane direction of the membrane. In an optional method step, the porous membrane can be densified to obtain a dense membrane. Figure 2 The white arrows in the figure indicate the direction perpendicular to the basal plane of the hexagonal boron nitride particle. Figure 2 The black arrows in the figure indicate the direction parallel to the basal plane of the hBN particles. Figure 2 In the figure of the single film layer 3 (porous or dense) on the left, the white arrow (indicating the direction perpendicular to the base plane of the hexagonal boron nitride particles, which is the direction of low thermal conductivity) is oriented perpendicular to the plane direction of the film, that is, oriented in the through-plane direction of the film. The black arrow (indicating the direction parallel to the base plane of the hexagonal boron nitride particles, which is the direction of high thermal conductivity) is oriented parallel to the plane direction of the film, that is, oriented in the in-plane direction of the film. In another step of the method disclosed herein, multiple layers of the porous or dense film 3 are stacked one after another to obtain a film stack 4. In Figure 2 In the figure of the film stack 4, the white arrow (indicating the direction perpendicular to the basal plane of the hexagonal boron nitride particles, which is the direction of low thermal conductivity) is oriented perpendicular to the plane direction of the multiple layers of the porous or dense film. In the next step of the method disclosed herein, the film stack 4 is pressed to obtain a bonded film stack 5. A sheet 6 is cut from the bonded film stack 5 in a direction perpendicular to the plane of the stacked film layers. Figure 2 In the figure of sheet 7 on the right side of the sheet 6, the sheet 6 obtained by the slicing step is rotated 90 degrees so that the plane direction of the obtained sheet is now parallel to the plane of the figure. In this figure of sheet 7, the white arrow (indicating the direction perpendicular to the base plane of the hexagonal boron nitride particles, which is the direction of low thermal conductivity) is oriented parallel to the plane direction of the sheet, that is, oriented in the in-plane direction of the sheet. The black arrow (indicating the direction parallel to the base plane of the hexagonal boron nitride particles, which is the direction of high thermal conductivity) is oriented perpendicular to the plane direction of the sheet, that is, oriented in the through-plane direction of the sheet.
[0189] The sheet materials as disclosed herein can be used as thermal interface materials. Such thermal interface materials can be used to manage heat flow into or out of different components such as electronic devices (e.g., batteries, motors, refrigerators, circuit boards, solar cells, and heaters). In some embodiments, the article (e.g., electronic device) includes a heat source and a sheet material described herein in contact with the heat source.
[0190] Exemplary embodiments
[0191] 1A. A sheet comprising a composite material, the composite material comprising a polymer and hexagonal boron nitride particles, wherein the hexagonal boron nitride particles comprise flaky hexagonal boron nitride particles, and wherein the flaky hexagonal boron nitride particles are oriented in a direction perpendicular to a planar direction of the sheet, and wherein the composite material comprises at least 70 wt % of the hexagonal boron nitride particles based on the total weight of the composite material, and wherein the sheet has a through-plane thermal conductivity greater than 12 W / m*K.
[0192] 2A. The sheet material according to example embodiment 1A, wherein the composite material is obtained by densifying a material comprising a porous polymer network.
[0193] 3A. A sheet according to any one of the aforementioned A exemplary embodiments, wherein the composite material comprises at least 80 wt.%, preferably at least 85 wt.%, more preferably at least 90 wt.%, and more preferably greater than 90 wt.% of the hexagonal boron nitride particles based on the total weight of the composite material.
[0194] 4A. The sheet according to any of the preceding A exemplary embodiments, wherein the sheet has a through-plane thermal conductivity of at least 15 W / m*K.
[0195] 5A. The sheet material according to any of the preceding A exemplary embodiments, wherein the composite material is electrically insulating.
[0196] 6A. The sheet according to any of the preceding A exemplary embodiments, wherein the sheet has an orientation index greater than 4.0.
[0197] 7A. A sheet according to any one of the preceding A exemplary embodiments, wherein the average particle size (d 50 ) is 0.5μm to 500μm.
[0198] 8A. A sheet according to any one of the preceding A exemplary embodiments, wherein the hexagonal boron nitride particles comprise agglomerates of primary particles of hexagonal boron nitride, and wherein the primary particles comprise plate-like hexagonal boron nitride particles, and wherein the average particle size (d 50 ) is 30μm to 500μm.
[0199] 9A. The sheet material according to exemplary embodiment 8A, wherein the average particle size (d 50 ) is 3μm to 50μm.
[0200] 10A. A sheet according to any one of the preceding A exemplary embodiments, wherein the hexagonal boron nitride particles comprise an average particle size (d 50) are non-agglomerated plate-like hexagonal boron nitride particles of 3 μm to 100 μm, preferably 5 μm to 30 μm.
[0201] 11A. The sheet material of any of the preceding A exemplary embodiments, wherein the flake-shaped hexagonal boron nitride particles have an aspect ratio of at least 5. 11A.
[0202] 12A. The sheet material according to any of the preceding A exemplary embodiments, wherein the composite material comprises at least 80 wt % and at most 98 wt % of the hexagonal boron nitride particles, based on the total weight of the composite material.
[0203] 13A. The sheet according to any of the preceding A exemplary embodiments, wherein the composite material comprises at least 2 wt % and at most 20 wt % of the polymer, based on the total weight of the composite material.
[0204] 14A. The sheet according to any of the preceding A exemplary embodiments, wherein the composite material further comprises 0.1 wt % to 10 wt % of mineral oil, based on the total weight of the composite material.
[0205] 15A. A sheet according to any of the preceding A exemplary embodiments, wherein the polymer is selected from the group consisting of polyurethanes, polyesters, polyamides, polyethers, polycarbonates, polyimides, polysulfones, polyethersulfones, polyphenylene oxides, polyacrylates, polymethacrylates, polyacrylonitrile, polyolefins, styrene, styrene-based copolymers, styrene-based copolymers, chlorinated polymers, fluorinated polymers, copolymers of ethylene and chlorotrifluoroethylene, and combinations thereof.
[0206] 16A. A sheet according to any one of the preceding A exemplary embodiments, wherein the polymer is 4 g / mol to 1×10 7 Ultra-high molecular weight polyethylene with a number average molecular weight in the g / mol range.
[0207] 17A. The sheet material of any of the preceding A exemplary embodiments, wherein the composite material has a porosity of up to 40%.
[0208] 18A. The sheet material of any of the preceding A exemplary embodiments, wherein the composite material has a porosity of 0.5% to 40%.
[0209] 19A. The sheet material of any of the preceding A exemplary embodiments, wherein the composite material has a porosity of 2% to 30%.
[0210] 20A. The sheet material according to any of the preceding A exemplary embodiments, wherein the sheet material has a dielectric loss factor of less than 0.009 at 5.2 GHz.
[0211] 21A. The sheet material of any of the preceding A exemplary embodiments, wherein the sheet material has a dielectric constant of at most 5.0 at 5.2 GHz.
[0212] 22A. The sheet according to any of the preceding A exemplary embodiments, wherein the through-plane thermal conductivity of the sheet is higher than the in-plane thermal conductivity of the sheet.
[0213] 23A. The sheet material of any of the preceding A exemplary embodiments, wherein the composite material does not comprise fibers.
[0214] 24A. The sheet according to any of the preceding A exemplary embodiments, wherein the sheet has a Shore D hardness of 30 to 150.
[0215] 25A. The sheet according to any of the preceding A exemplary embodiments, wherein the sheet has a thickness of 0.01 mm to 6 mm.
[0216] 1B. A method for producing a sheet material according to any one of the above exemplary embodiments A, the method comprising
[0217] providing a polymer, a solvent, and hexagonal boron nitride particles including plate-like hexagonal boron nitride particles,
[0218] mixing the polymer, the solvent and the hexagonal boron nitride particles to form a suspension of hexagonal boron nitride particles in a polymer-solvent solution, wherein the polymer in the polymer-solvent solution has a melting point, and wherein the solvent has a boiling point, and wherein the mixing of the polymer, the solvent and the hexagonal boron nitride particles is performed at a temperature above the melting point of the polymer in the polymer-solvent solution and below the boiling point of the solvent,
[0219] forming the suspension into a film in which the plate-like hexagonal boron nitride particles are oriented in a direction parallel to a planar direction of the film,
[0220] inducing phase separation of the polymer and the solvent,
[0221] removing at least a portion of the solvent from the membrane to obtain a porous membrane, optionally compressing the porous membrane to obtain a dense membrane,
[0222] stacking a plurality of layers of the porous membrane or the dense membrane one after another to obtain a membrane stack,
[0223] pressing the membrane stack to obtain a bonded membrane stack, and
[0224] Sheets are cut from the bonded film stack in a direction perpendicular to the plane of the stacked film layers.
[0225] 2B. A method for producing a sheet material according to any one of the above exemplary embodiments A, the method comprising
[0226] providing a polymer, a solvent, and hexagonal boron nitride particles including plate-like hexagonal boron nitride particles,
[0227] The polymer, the solvent and the hexagonal boron nitride particles are mixed to form a slurry, wherein the slurry is a suspension of the polymer and the hexagonal boron nitride particles in the solvent, and wherein the polymer has a melting point, and wherein the solvent has a boiling point, and wherein the mixing of the polymer, the solvent and the hexagonal boron nitride particles is performed at a temperature below the melting point of the polymer and below the boiling point of the solvent,
[0228] forming the slurry into a film in which the plate-like hexagonal boron nitride particles are oriented in a direction parallel to a planar direction of the film,
[0229] heating the film in an environment to retain in the film at least 90 weight percent of the solvent based on the weight of the solvent in the film and to dissolve in the solvent at least 50 weight percent of the polymer based on the total weight of the polymer,
[0230] inducing phase separation of the polymer and the solvent,
[0231] removing at least a portion of the solvent from the membrane to obtain a porous membrane, optionally compressing the porous membrane to obtain a dense membrane,
[0232] stacking a plurality of layers of the porous membrane or the dense membrane one after another to obtain a membrane stack,
[0233] pressing the membrane stack to obtain a bonded membrane stack, and
[0234] Sheets are cut from the bonded film stack in a direction perpendicular to the plane of the stacked film layers.
[0235] 3B. The method of Exemplary Embodiment 1B or Exemplary Embodiment 2B, wherein the polymer has a melting point, and wherein the induced phase separation occurs below the melting point of the polymer.
[0236] 4B. The method according to any one of the above B exemplary embodiments, further comprising:
[0237] The membrane stack is heated before pressing the membrane stack.
[0238] 5B. The method of any of the preceding B exemplary embodiments, wherein pressing the film stack is performed at a temperature of at least 110°F.
[0239] 6B. The method according to any one of the above B exemplary embodiments, further comprising:
[0240] The bonded film stack is heated before sheets are cut from the bonded film stack.
[0241] 7B. The method according to any of the preceding B exemplary embodiments, wherein pressing the membrane stack is performed at a pressing pressure of at least 2.0 MPa.
[0242] 8B. The method according to any of the preceding B exemplary embodiments, wherein pressing the film stack is performed in a pressing direction while constraining the film stack in a first direction perpendicular to the pressing direction.
[0243] 9B. A method according to any one of the aforementioned B exemplary embodiments, wherein pressing the film stack is performed in a pressing direction while constraining the film stack in a first direction perpendicular to the pressing direction and in a second direction perpendicular to the pressing direction, and wherein the first direction is perpendicular to the second direction.
[0244] Example
[0245] Test Method
[0246] Airflow resistance test
[0247] Airflow resistance was measured using a densitometer (available as Model 4110 from Gurley Precision Instruments, Troy, NY, US) and a timer (available as Model 4320 from Gurley Precision Instruments). The sample was clamped in the tester. The timer and photoeye were reset and the drum was released to allow air to pass through a 1 square inch (6.5 cm2) circle with a constant force of 4.88 inches (12.4 cm) of water (1215 N / m2). The velocity through the 50 cm 3 Air time.
[0248] Bubble Point Pressure Test
[0249] Bubble point pressure is a common technique for characterizing the largest pores in porous membranes. A 47 mm diameter disk was cut, and the sample was soaked in 100% isopropyl alcohol (IPA) to completely fill and wet the pores in the sample. Then, the wet sample was placed in a holder (47 mm stainless steel holder part #2220, from Pall Corporation, Port Washington, NY, US). A pressure controller was used to slowly increase the pressure at the top of the sample, and a gas flow meter was used to measure the gas flow at the bottom. When the flow rate from the baseline flow rate increased significantly, the pressure was recorded. This is reported as bubble point pressure (pounds per square inch, psi). This technique is a modification of ASTM F316-03 (2006) "Standard Test Methods for Pore Size Characteristics of Membrane Filters by Bubble Point and Mean Flow Pore Test" and includes an automatic pressure controller and flow meter to quantify when the bubble point pressure has been reached. The pore size is calculated according to ASTM using the following formula:
[0250] Limiting pore diameter (μm) = (surface tension in dynes / cm*0.415) / (pressure in psi)
[0251] A factor of 0.415 is included since the pressure is in psi. A surface tension of 21.7 dynes / cm is used for 100% isopropyl alcohol.
[0252] Density and porosity testing
[0253] If not otherwise specified, the density of the sample is calculated using a method similar to ASTM F-1315-17 (2017), "Standard Test Method for Density of a Sheet Gasket Material", which includes cutting a 47 mm diameter disk, weighing the disk on an analytical balance with an appropriate resolution (typically 0.0001 grams), and measuring the density on a thickness gauge with a deadweight of 7.3 psi (50.3 KPa) and a flat anvil of 0.63 feet (1.6 cm) in diameter (obtained as Model 49-70 from Testing Machines, Inc., New Castle, Delaware, USA). Castle, DE, US), with a dwell time of approximately 3 seconds and a resolution of + / - 0.0001 inches. The density was then calculated by dividing the mass by the volume, which was calculated from the thickness and diameter of the sample. Using the known densities and weight fractions of the components of the composite, the theoretical density of the composite was calculated by the rule of mixtures. Using the theoretical density and measured density, the porosity was calculated as follows:
[0254] Porosity = [1-(measured density / theoretical density)] × 100
[0255] For some samples, due to the uneven surface caused by band saw cutting, the density is measured using the Archimedean density method. Use an analytical balance (derived from Mettler Toledo (Schweiz) GmbH, Im Langacher 44, 8608 Griefensee, Switzerland, with model MS1003TS-C012187274) to measure the density of these samples. A glass container (similar to a beaker) is placed above the balance and filled with distilled water until at least 3 / 4 is full. The sample dish with a basket attached to the bottom is placed above the glass container so that the basket is completely immersed, and the dish and the basket are both attached to the balance to measure their mass. The mass of the balance is zeroed and an approximately 1" x 1" x 1 / 2" sample is placed in the top dish to measure its mass in air. After this data is stored, the sample is placed in a basket below the dish so that the mass of the sample when submerged in water can be measured. The difference in mass of the sample when dry and when submerged in water is used, and the density of distilled water at 22°C is 0.99777 g / cm 3 , calculate the density of the block.
[0256] Thermal conductivity test
[0257] Direct thermal diffusivity measurements were performed using a flash analysis method according to ASTM E1461 (2013) using a flash thermophysical property analyzer (obtained from Netzsch Instruments North America LLC, Boston, MA, US, as "HYPERFLASH LFA 467"). Each sample set included a reference sample (obtained from Poco Graphite, Decatur, TX, US, under the trade name "AXM-5Q POCO GRAPHITE"), which was used as a method control for diffusivity measurements. The samples were coated with a layer of sprayed graphite (sprayed 3 times at a distance of about 5 inches using a graphite spray obtained from Miracle Power Products Corporation, Cleveland, OH, US, under the trade name "DGF 123 DRY GRAPHITE FILM SPRAY") on both the light incident side and the detection side to standardize the surface thermal storage coefficient and absorptivity of the tested samples. The thickness of the sample was measured with a manual caliper (Fisher Scientific) at 5 different areas of the sample disk, and the average of these measurements was calculated. The thickness was used to calculate the geometric density of the sample. In a single measurement called "shooting", a short-duration pulse of light (Xenon flash lamp, 230V, 15 microsecond duration) was incident on one side of the sample, and the thermogram (time trajectory of the measured temperature) was recorded on the other side of the sample, as measured by the voltage on the InSb IR detector. The thermal diffusivity was calculated by fitting the thermogram to the Cowan Plus pulse correction model for the through-plane and the anisotropic model for the in-plane (the anisotropic model for the in-plane thermal diffusivity takes into account the through-plane data). Heat capacity was calculated by differential scanning calorimetry (DSC) according to ASTM E1269 (2011) "Quasi-Isothermal Moderated DSC" using a DSC instrument (obtained from TA Instruments, New Castle, DE, US under the trade name "Q2000 DSC"). Sapphire was used as the reference for the DSC. The through-plane diffusivity was calculated using the Cowan method with additional correction for the finite pulse width, while the in-plane diffusivity was calculated using an anisotropic model with the aid of software (obtained from Netzsch, Selb, Germany under the trade name "Proteus"). The measurements were made using samples with a diameter of 1 inch. Three shots were obtained for each sample at 25°C.Measured density (ρ) (based on 2.54 cm (1 inch) disk geometry), specific heat capacity (c. P The product of ) (by differential scanning calorimetry) and the diffusivity (α) provides the thermal conductivity. That is,
[0258] k(W / (m*K))=ρ(g / cm3)xc P (J / K / g)xα(mm 2 / s).
[0259] Hardness measurement (Shore D)
[0260] The Shore Durometer hardness of the samples was measured using the D scale according to ASTM D2240-15. Testing was conducted under ambient laboratory conditions of 23°C and less than 20% relative humidity. The reported measurements are from stacked, bonded blocks and are reported as the average of four measurements of the scraped surface parallel to the lamination plane.
[0261] Dielectric property measurement (split-pillar dielectric resonator measurement at 5.2 GHz)
[0262] All dielectric properties were measured at 5.2 GHz using a separated post dielectric resonator (SPDR) according to the IEC 61189-2-712 standard. Each 1 mm thick sample was inserted between two fixed dielectric resonators. The resonant frequency and quality factor of the post were affected by the presence of the sample, and this enabled the complex dielectric constant (dielectric constant and dielectric loss) to be calculated directly. The geometry of the separated dielectric resonator fixture used in the measurement was built and purchased from QWED in Warsaw, Poland in collaboration with Professor Jerzy Krupka of Warsaw University of Technology. The 5.2 GHz resonator operates in the TE01δ mode with only an azimuthal electric field component, so that continuity is maintained at the dielectric interface. The separated post dielectric resonator measures the permittivity in the sample plane. Ring coupling (critical coupling) is used in each dielectric resonator measurement in these dielectric resonator measurements. The 5.2 GHz SPDR measurement system was combined with a Keysight VNA (vector network analyzer model PNA 8364C, 10 MHz-50 GHz). Calculations were performed using commercial analysis software built by Professor Jerzy Krupka and supported by Keysight's N1500A dielectric measurement software suite.
[0263] Orientation index measurement
[0264] The orientation index is determined by X-ray diffraction. To this end, the ratio of the (100) reflection intensity to the (002) reflection intensity of hexagonal boron nitride (hBN) measured on the X-ray diffraction pattern of the sheet sample is determined and divided by the corresponding ratio of an ideal, unoriented (i.e., isotropic) hBN sample. This ideal intensity ratio or reference intensity ratio can be determined from the powder diffraction pattern (PDF) #01-073-2095 of the International Center for Diffraction Data (ICDD) data (2020) and is 0.147. The theoretical peak positions of the (002) reflection and the (100) reflection are at 26.7 degrees and 41.6 degrees, respectively. The peak intensities of the (002) reflection and the (100) reflection are measured from the peak areas at these positions.
[0265] To measure the peak intensity of the (002) reflection and the (100) reflection, the sample was cut and loaded on a zero-background silicon sample holder. Reflection geometry data was collected in a full-spectrum scan using a PANalytical Empyrean vertical diffractometer, copper Ka radiation, and a PIXcel-3D detector (1D mode with 255 channels or 3.35° opening) for recording scattered radiation. The X-ray source and detector were located at a circle with a radius of 240.00 mm. The diffractometer was equipped with a 0.04 rad Soller slit on both the incident and diffracted beam sides, a mask 20 and a Ni filter on the incident side, a programmable divergence slit at a sample distance of 140.00 mm to control the irradiation length at the sample to 5.0 mm, a receiving slit at a height of 2.00 mm, and a programmable anti-scatter slit to control the observation length to 2.0 mm. The full spectrum was scanned from 5 to 80 degrees (2q) using a 0.04 degree step size and a 1200 second dwell time setting. The X-ray generator settings were 40 kV and 40 mA.
[0266] The orientation index (OI) can be determined from the measured peak intensities of the (002) reflection and the (100) reflection using the following formula:
[0267]
[0268] Examples 1 to 4 (EX1 to EX4)
[0269] Ultra-high molecular weight polyethylene (UHMWPE) powder (obtained from Celanese Corporation, Irvine, TX, US under the trade designation "GUR-2126") was metered from a powder feeder (KT20, Coperion K-Tron, Stuttgart, Germany) into the feed hopper of a twin-screw extruder (25 mm co-rotating twin-screw extruder, Berstorff, Germany) at 200 rpm and 93°C at the rates shown in Table 1. The extruder was calibrated using a gear pump (Zenith Pumps, Monroe, NC, US) and a Coriolis mass flow meter (Micromotion mass flow meter, Emerson Electric Co., St. Louis, MO, US). Co, St. Louis, MO, US)) was pumped into the open barrel zone 2 of the extruder at 93°C at the rate shown in Table 1 with mineral oil (Kaydol white mineral oil from Brenntag Great Lakes, LLC) mixed and heated to 204°C to melt the UHMWPE into the mineral oil. Finally, hexagonal boron nitride particles (BN; grade shown in Table 1, 3M Company, St. Paul, MN, US) were fed from a powder feeder at 100 rpm to a side feeder (Side Feeder, Century Extrusion, Travers City, Michigan, USA) connected to zone 4 of the twin-screw extruder at 204°C. City, MI, US) and incorporated into the melt. The extruder mixes, disperses the melt and increases the temperature of the melt to prepare a stable mixture (i.e., a suspension). The mixture is then extruded onto a 60°C smooth casting roll through a 180°C drop hammer forging die (6" (15.24 cm), Wide Ultraflex U40, Nordson Extrusion Dies LLC, Chippewa Falls, WI, US) at the speed shown in Table 1, and quenched to form a film. After quenching, the ultra-high molecular weight polyethylene separates from the suspension to form a phase-separated porous polymer network structure connecting the hexagonal boron nitride particles and the mineral oil filling the voids. The mineral oil in the film is then extracted with 3M NOVEC 72DE (3M Company, St. Paul, Minnesota, USA) by passing the film through a countercurrent extraction bath at a rate of 10 fpm (feet per minute).The bath with a total capacity of 300 gallons was divided into seven tanks. The exchange rate of 3MNOVEC 72DE to the bath was 52 gallons / hour. The membrane was then transported through a dryer at 83°C to evaporate and recover the NOVEC 72DE to obtain a porous membrane. For each sample, 10 to 50 yards of porous membrane were produced.
[0270] Table 1
[0271] EX1 EX2 EX3 EX4 UHMWPE feed rate [lb / hr] 0.75 0.75 0.46 0.75 Mineral oil feed rate [lb / hr] 4.2 4.2 4.2 4.2 Boron Nitride Grades CFP 012P CFF 500-15 CFA 250S CFA 250S Boron Nitride Feed Rate [lb / hr] 5.05 5.05 5.63 5.05 Casting roll speed [fpm] 2.1 2.1 4.2 2.1 BN content [wt%] 87.1 87.1 92.4 92.1
[0272] CFP 012P is the average aggregate size (d 50 ) is a boron nitride agglomerate of 150 μm, and the average particle size (d 50 ) is made of primary particles of 12 μm (trade name "3M TM Boron nitride powder cooling filler sheet ("CFP 012P") was obtained from 3M Company, St. Paul, Minnesota, USA).
[0273] CFF 500-15 is the average aggregate size (d 50 ) is 310 μm of flake boron nitride agglomerates, and the average particle size (d 50 ) is made of primary particles of 15 μm (trade name "3M TM Boron nitride powder cooling filler sheets (CFF 500-15" were obtained from 3M Company, St. Paul, Minnesota, USA).
[0274] CFA 250S is the average aggregate size (d 50 ) is 130 μm spherical boron nitride agglomerates (made of flake boron nitride particles) (trade name "3M TM Boron nitride powder cooling filler agglomerate ("CFA 250S") was obtained from 3M Company, St. Paul, Minnesota, USA.
[0275] The test results of the obtained porous membrane are shown in Table 2.
[0276] Table 2
[0277]
[0278]
[0279] *) nm = not measured
[0280] The resulting porous membrane was then calendered to reduce porosity and improve thermal conductivity. This was done by passing a 3 inch wide sample at 4 fpm through two smooth 10 inch diameter horizontal calender rolls set at a force of 4000 pli (pounds per linear inch).
[0281] The test results of the obtained dense film are shown in Table 3.
[0282] Table 3
[0283]
[0284] The resulting dense film was then cut into 1" x 2" strips with scissors, stacked between two release liner films, and pressed in a heated hydraulic press at 149°C (300°F), with the pressing force gradually increased to 5000 lbf over 5 minutes, with 0.580" gaskets on two opposite sides of the stack to keep the stack vertical. The number of stacked strips is shown in Table 4. The resulting pressed film stack is a cohesive block (or cohesive film stack) made of stacked film strips, which is removed from the hydraulic press and allowed to cool to room temperature (23°C), and then a razor blade is used to cut through all the film layers to cut out the sheet. In the sheet obtained by cutting, the hexagonal boron nitride particles are oriented perpendicular to the plane of the sheet.
[0285] The test results of the obtained sheets are shown in Table 4.
[0286] Table 4
[0287]
[0288]
[0289] Example 5 (EX5)
[0290] For Example 5, a dense film was prepared as described for Example 1, except that the extrusion was carried out at 193°C (380°F) instead of 180°C, an 8" drop die was used instead of 6", countercurrent extraction was carried out at a rate of 2 fpm, and the formulation used was as shown in Table 5.
[0291] Table 5
[0292] EX5 UHMWPE feed rate [lb / hr] 0.46 Mineral oil feed rate [lb / hr] 4.2 Boron Nitride Grades CFA 50 Boron Nitride Feed Rate [lb / hr] 5.63 Casting roll speed [fpm] 2.1 BN content [wt%] 92.5
[0293] CFA 50 is a 50 μm protection screen with an average particle size (d 50 ) of boron nitride agglomerates, flakes and clusters (available under the trade name "3M TM Boron nitride powder cooling filler agglomerates (CFA 50" was obtained from 3M Company, St. Paul, Minnesota, USA).
[0294] The test results of the dense membrane prepared according to the procedure described for Example 1 are shown in Table 6.
[0295] Table 6
[0296]
[0297]
[0298] The resulting dense film was then cut into 2" x 2" strips with scissors, stacked between two release liner films, and pressed in a heated hydraulic press at 149°C (300°F), gradually increasing the pressing force to 2500 lbf over 2.5 minutes, with 1.375" spacers on two opposite sides of the stack to keep the stack vertical. The number of stacked strips is shown in Table 7. The resulting pressed film stack was a cohesive block (or cohesive film stack) made of stacked film strips, which was removed from the hydraulic press and allowed to cool to room temperature (23 ℃). The cohesive block was then placed in a laboratory oven at 149℃ for 10 minutes. The oven-heated cohesive block was then quickly returned to a heated hydraulic press at 176.6℃ (350℉) and compressed by gradually increasing the pressing force to 1700lbf over 3 minutes. The cohesive block was then removed from the hydraulic press and allowed to cool to room temperature (23℃) before a scraper was used to cut through all the film layers to cut the sheet. In the sheet obtained by cutting, the hexagonal boron nitride particles were oriented in a direction perpendicular to the plane direction of the sheet.
[0299] The test results of the obtained sheets are shown in Table 7.
[0300] Table 7
[0301] EX5 <![CDATA[Archimedes density of the sheet [g / cm 3 > 1.83 Sheet porosity [%] 9.9 Thermal conductivity of the sheet through the surface [W / m*K] 20.0 BN content of sheet [wt%] 92.5 UHMWPE content of sheet [wt%] 7.55
[0302] Examples 6 to 8 (EX6 to EX8)
[0303] For Examples 6 to 8, porous membranes were prepared using the composition and preparation method described for Example 5, except that the casting roll speed was 3 fpm. No calendering step was performed after the porous membrane was obtained. The porous membrane was then cut into 1"×1" squares with scissors. In order to stack and press these squares, that is, to stack multiple layers of porous membranes and to press the membrane stack, a steel mold was used to constrain the stack in the x and y directions. The steel mold had a cavity with a width of 1.0625", a length of 1.0625", and a height of 1.5" and a top plunger, and was placed in an oven at 300℉ (149℃) for 30 minutes to preheat the mold. The mold was removed from the oven and 1"×1" squares were stacked into the mold to a height of 1.4". Isolation pads were placed at the top and bottom of the stack. The top plunger was inserted, and the mold and the stacked membrane squares were placed in an oven at 300℉ (149℃) for 15 minutes. The mold and film stack are then quickly removed from the oven and placed on a heated hydraulic press at 176.6°C (350°F) and pressed by gradually increasing the force to the values shown in Table 8 over 3 minutes. The mold is then removed from the hydraulic press and opened; additional film squares are added. The heating, pressing, and adding additional squares are then repeated three times until the stack is approximately 1" high. The resulting pressed film stack is a cohesive block (or cohesive film stack) made of stacked film squares, which is removed from the hydraulic press and allowed to cool to room temperature (23°C) before a band saw is used to cut through all the film layers to cut out sheets. In the sheets obtained by cutting, the hexagonal boron nitride particles are oriented in a direction perpendicular to the planar direction of the sheet.
[0304] The results are shown in Table 8.
[0305] Table 8
[0306]
[0307] As can be seen in Table 8, although the porosity of the sheet of Example 8 is similar to that of the sheet of Example 5, the through-plane thermal conductivity of the sheet of Example 8 is significantly higher than that of the sheet of Example 5. This can be explained by the use of higher pressures when pressing the film stack, which results in increased particle-to-particle contact of the hexagonal boron nitride particles between layers (i.e., between initially adjacent film layers in the bonded film stack formed during pressing).
[0308] Example 9 (EX9)
[0309] For Example 9, a porous membrane was prepared as described for Example 7. No calendering step was performed after the porous membrane was obtained. The porous membrane was then cut into 1.5"×1.5" squares with scissors. In order to stack and press these squares, i.e., to stack multiple layers of porous membrane and to press the membrane stack, a steel mold was used to constrain the stack in the x and y directions. The steel mold had a cavity with a width of 1.625", a length of 1.625", a height of 2.625" and a top plunger of 1.25", and was placed in an oven at 300°F (149°C) for 60 minutes to preheat the mold. The mold was removed from the oven and 1.5" x 1.5" squares were stacked into the mold to a height of 1.4". Release liners were placed at the top and bottom of the stack. A top plunger was inserted into the mold. The mold and stacked film squares were placed in an oven at 300°F (149°C) for 15 minutes. The mold and stack were then quickly removed from the oven and placed on a heated hydraulic press at 176.6°C (350°F) and pressed by gradually increasing the force to the values shown in Table 9 over 3 minutes. The mold was then removed from the hydraulic press and opened; additional film squares were added. The heating, pressing, and adding of additional squares were then repeated three times until the stack was approximately 1.5" high. The resulting pressed film stack was a bonded block (or bonded film stack) made of stacked film squares, which was removed from the hydraulic press and allowed to cool to room temperature (23°C) before a band saw was used to cut through all the film layers to cut out the sheet. In the sheet obtained by cutting, the hexagonal boron nitride particles are oriented in a direction perpendicular to the plane direction of the sheet.
[0310] The results are shown in Table 9.
[0311] Table 9
[0312]
[0313] Examples 10 and 11 (EX10 and EX11)
[0314] A plastic mixing cup (obtained under the trade name "MAX 100 CUP"; both obtained from FlackTek, Inc., Landrum, SC, US) for a high-speed mixer (obtained under the trade name "SPEEDMIXER DAC 150.1FV") was charged with ultra-high molecular weight polyethylene (UHMWPE) powder (obtained under the trade name "GUR-2126" from Celanese Corporation, Irvine, Texas, USA), paraffin wax (obtained under the trade name "ISOPAR G" from Brenntag Great Lakes, Inc., Wauwatosa, WI, US) and hexagonal boron nitride powder (grades shown in Table 10, 3M Company, St. Paul, Minnesota, USA), and their amounts are shown in Table 10. UHMWPE, paraffin wax and hexagonal boron nitride powder were mixed in a high-speed mixer at 1000 rpm for 1 minute, followed by 2500 rpm for 30 seconds. The resulting slurry was then manually stirred with a wooden spatula to remove material from the corners and sides of the cup and mixed a second time at 1000 rpm for 1 minute, followed by 2500 rpm for 30 seconds.
[0315] Table 10
[0316] EX10 EX11 UHMWPE mass [g] 3.033 12.185 Isopar G mass [g] 43.0 43.0 Boron Nitride Grades CFP 007HS CFP 007HS Boron nitride mass [g] 38.63 29.48 BN content [wt%] 92.7 70.8
[0317] CPF 007HS is a high surface area boron nitride flake with an average particle size (d 50 ) and a controlled maximum size of 50 μm (available under the trade name “3M TM Boron nitride powder cooling filler sheet ("CFP 007HS") was obtained from 3M Company, St. Paul, Minnesota, USA).
[0318] After mixing, the slurry was applied to a 3 mil (75 micron) polyester (PET) liner at room temperature (about 23° C.) using a tongue depressor, and then another 3 mil (75 micron) PET liner was applied on top of the slurry to sandwich the slurry. The slurry was then spread between the PET liners using a notched bar set with a 30 mil (762 micron) gap, which is the wet coating thickness (excluding the liner).
[0319] The sandwiched, formed slurry was placed on an aluminum tray and placed in an oven at 150°C (302°F) for 5 minutes to activate (i.e., dissolve the UHMWPE into the solvent to form a single phase). The tray with the activated sandwiched formed slurry was removed from the oven, and the sandwiched formed slurry and liner were placed on a granite block to air cool to ambient temperature (about 23°C), thereby forming a solvent-filled (i.e., paraffin-filled) porous membrane sandwiched between two liners. The top liner was removed, exposing the porous membrane to air. The porous membrane on the PET liner on the tray was inserted into an oven at 100°C (212°F) for 45 minutes to evaporate the paraffin. After the paraffin evaporated, the porous membrane on the PET liner was removed from the oven, allowed to cool to ambient temperature (23°C), and then the liner was removed to obtain a porous membrane (i.e., a porous polymer network containing hexagonal boron nitride particles).
[0320] No calendering step is performed after the porous membrane is obtained. The resulting porous membrane is then cut into 1"×1" blocks. In order to stack and press these blocks, i.e., to stack multiple layers of the porous membrane and to press the membrane stack, a steel mold is used to constrain the stack in the x and y directions. The steel mold has a cavity with a width of 1.0625", a length of 1.0625", a height of 1.5" and a top plunger, and is placed in an oven at 300℉ (149℃) for 30 minutes to preheat the mold. The mold is removed from the oven and 1"×1" blocks are stacked into the mold to a height of 1.4". Isolation pads are placed at the top and bottom of the stack. The top plunger is inserted, and the mold and the stacked membrane blocks are placed in an oven at 300℉ (149℃) for 15 minutes. The mold and film stack are then quickly removed from the oven and placed on a heated hydraulic press at 176.6°C (350°F) and pressed by gradually increasing the force to 2000 lbf (corresponding to a pressing pressure of 2000 pounds per square inch (13.8 MPa)) over 3 minutes. The mold is then removed from the hydraulic press and opened, and additional film squares are added. The process is then repeated three times until the stack is approximately 1" high. The resulting pressed film stack is a cohesive block (or bonded film stack) made of stacked film squares, which is removed from the hydraulic press and allowed to cool to room temperature (23°C), and then a band saw is used to cut through all the film layers to cut out the sheet. In the sheet obtained by cutting, the hexagonal boron nitride particles are oriented in a direction perpendicular to the planar direction of the sheet.
[0321] The test results of the obtained sheets are shown in Table 11.
[0322] Table 11
[0323]
[0324]
[0325] Comparative Examples 1 to 3 (CEX1 to CEX3)
[0326] Comparative Examples 1 to 3 were prepared using silicone, with the same volume percent loading of hexagonal boron nitride particles as in Examples 10 to 12. A plastic mixing cup (obtained under the trade designation "MAX 100 CUP"; both available from Flecktech, Landrum, SC, USA) for a high-speed mixer (obtained under the trade designation "SPEEDMIXER DAC 150.1FV") was charged with two parts of silicone (obtained under the trade designation "Sylgard 184" from Dow Chemical Co., Midland, MI, US) and hexagonal boron nitride particles (grades shown in Table 12, 3M Company, St. Paul, MN, USA) in the amounts shown in Table 12. The two parts of silicone and hexagonal boron nitride particles were mixed in a high-speed mixer at 3500 rpm for 30 seconds.
[0327] Table 12
[0328] CEX1 CEX2 CEX3 Sylgard 184 Part A Mass [g] 7.233 2.473 5.709 Sylgard 184 Part B Mass [g] 0.723 0.247 0.571 Boron Nitride Grades CFP 007HS CFP 007HS CFP 007HS Boron nitride mass [g] 26.04 31.28 13.72 BN content [wt%] 76.6 92.0 68.6
[0329] The resulting slurry was then placed between two PET release liners and pressed on a heated hydraulic press at 130°C with a 0.576" spacer in an attempt to form a film. The sample was removed from the press, allowed to cool to room temperature (23°C) and the release liner removed to obtain a silicone / boron nitride sample.
[0330] The test results of the silicone / boron nitride samples are shown in Table 13.
[0331] Table 13
[0332] CEX1 CEX2 CEX3 Can film samples be made [yes / no] yes no yes Is the membrane sample fragile? [Yes / No] yes - no
[0333] For Comparative Example 1, when attempting to form a film, the resulting sample was too brittle to cut strips from it, and it was impossible to form a film stack without layer breakage. The sample had dust around the edge and was easily broken when pressure was applied thereto.
[0334] For Comparative Example 2, when attempting to form a film, the resulting sample looked like a pile of powder. It was not possible to form a stack of film layers.
[0335] For Comparative Example 3, the resulting film sample was then cut into 2" x 2" squares with a razor. A thin layer of two-part silicone was applied to the top surface of the square with a foam head applicator, and 6 film layers were stacked to form a block with silicone between the layers. The block was then placed between 0.575" shims in a heated hydraulic press at 130°C and pressed for 30 minutes to cure the silicone. The bonded block was then removed from the press and allowed to cool to room temperature (23°C) before a band saw was used to cut through all the layers to cut out the sheets.
[0336] The test results of the obtained sheets are shown in Table 14.
[0337] Table 14
[0338]
[0339] As can be seen from Table 14, the through-plane thermal conductivity of Comparative Example 3 is lower than that of Example 11, even though both samples have similar hexagonal boron nitride particle contents (about 70 wt%). For Comparative Examples 1 and 2, film stacks could not be made, and therefore sheets could not be cut in a direction perpendicular to the plane of the stacked film layers.
[0340] Examples 12 and 13 (EX12 and EX13)
[0341] For Examples 12 and 13, porous membranes were prepared according to the procedure described in Examples 10 and 11, except that the formulations shown in Table 15 were used. Mineral oil was obtained from Bruntag Great Lakes LLC under the trade name "Kaydol White Mineral Oil". After evaporation of the paraffin-filled porous membrane (100° C., 45 minutes), a porous membrane containing mineral oil in the porous polymer network was obtained.
[0342] Table 15
[0343] EX12 EX13 UHMWPE mass [g] 1.953 2.022 Isopar G mass [g] 30.14 45.0 Mineral oil mass [g] 1.256 1.230 Boron Nitride Grades CFA 150 CFA 150 Boron nitride mass [g] 23.05 38.41 BN content [wt%] 87.8 92.2 Mineral oil content [wt%] 4.8 3.0 UHMWPE content [wt%] 7.4 4.8
[0344] CFA 150 is the average aggregate size (d 50 ) is a boron nitride agglomerate of a crystalline boron nitride sheet of 150 μm (trade name "3M TM Boron nitride powder cooling filler agglomerate CFA 150" was obtained from 3M Company, St. Paul, Minnesota, USA).
[0345] The resulting porous membrane was then calendered to reduce porosity and improve thermal conductivity. This was done by passing a 3 inch wide sample at 4 fpm through two smooth 10 inch diameter horizontal calender rolls set to the forces shown in Table 16.
[0346] The test results of the obtained dense film are shown in Table 16.
[0347] Table 16
[0348]
[0349] The resulting dense film was then cut into 1.5" x 1.5" strips with scissors, stacked between two release liner films, and pressed in a heated hydraulic press at 149°C (300°F), gradually increasing the pressing force to 2500 lbf over 2.5 minutes, with 1.375" spacers on opposite sides of the stack to limit compression and keep the stack vertical. The number of strips stacked is shown in Table 17. The resulting pressed film stack was a cohesive block (or cohesive film stack) made of the stacked film strips, which was removed from the hydraulic press and allowed to cool to Room temperature (23 ° C). The tack block is then placed in a laboratory oven at 149 ° C for 10 minutes. The oven-heated tack block is then quickly returned to a heated hydraulic press at 176.6 ° C (350 ° F) and compressed by gradually increasing the pressing force to 1700 lbs within 3 minutes. The tack block is then taken out of the hydraulic press and allowed to cool to room temperature (23 ° C), and then a band saw is used to cut through all the film layers to cut off the sheet. In the sheet obtained by cutting, the hexagonal boron nitride particles are oriented in a direction perpendicular to the planar direction of the sheet.
[0350] The test results of the obtained sheets are shown in Table 17.
[0351] Table 17
[0352]
[0353] *) nm = not measured
[0354] The hardness of the samples that included mineral oil in the final sheet was lower than the hardness of the samples that did not include mineral oil in the final sheet.
[0355] Example 14 (EX14)
[0356] For Example 14, a porous membrane was prepared using the composition and preparation method described for Example 13. No calendering step was performed after the porous membrane was obtained. The resulting porous membrane was then cut into 1"×1" squares. In order to stack the squares, that is, in order to stack multiple layers of the porous membrane, a steel mold was used to constrain the stack in the x and y directions. The steel mold had a cavity with a width of 1.0625", a length of 1.0625", and a height of 1.5" and a top plunger, and was placed in an oven at 300℉ (149℃) for 30 minutes to preheat the mold. The mold was removed from the oven and 1"×1" squares were stacked into the mold to a height of 1.4". Isolation pads were placed at the top and bottom of the stack. The top plunger was inserted, and the mold and the stacked membrane squares were placed in an oven at 300℉ (149℃) for 15 minutes. The mold and stack are then quickly removed from the oven and placed on a heated hydraulic press at 176.6°C (350°F) and pressed by gradually increasing the force to 2000 lbf (corresponding to a pressing pressure of 2000 pounds per square inch (13.8 MPa)) over 3 minutes. The mold is then removed from the hydraulic press and opened, and additional film squares are added. The process is then repeated three times until the stack is approximately 1" high. The resulting pressed film stack is a cohesive block (or bonded film stack) made of stacked film squares, which is removed from the hydraulic press and allowed to cool to room temperature (23°C), and then a band saw is used to cut through all the film layers to cut out the sheet. In the sheet obtained by cutting, the hexagonal boron nitride particles are oriented in a direction perpendicular to the planar direction of the sheet.
[0357] The test results of the obtained sheets are shown in Table 18.
[0358] Table 18
[0359]
[0360] Example 15 (EX15)
[0361] The mixture was prepared by mixing 0.4561 g of ultra-high molecular weight polyethylene (UHMWPE) powder, 12.6135 g of mineral oil (obtained from Bruntag Great Lakes LLC under the trade name "Kaydol White Mineral Oil"), 16.7774 g of hexagonal boron nitride particles (obtained from the trade name "3M TMBoron nitride powder (cooled filler agglomerate CFA 50" from 3M Company, St. Paul, Minnesota, USA) and 1.1309 g of elastomer (available under the trade name Krayton 1645 from Krayton Corporation, Houston, TX) were charged into the 176.6°C (350°F) bowl of a mixer (Brabender CW DR-2051, Brabender GmbH & Co. KG, Duisburg, Germany) to prepare Example 15. The bowl was mixed at 50 rpm for 5 minutes to melt the UHMWPE and mix the components.
[0362] The molten suspension was removed from the bowl with a tongue depressor and placed between two heat stable release liners. It was then placed on a heated hydraulic press at 176.6°C (350°F) with 61.5 mil shims on opposite sides of the stack between the release liners to limit compression and pressed by gradually increasing the force to 3000 lbf over 5 minutes to form a film. The film was then removed from the hydraulic press and placed between cooling plates for 5 minutes to quickly cool to room temperature (23°C).
[0363] The liner was removed and the membrane sample was washed three times in a pot of excess Novec 72DE with a 10 minute soak time, followed by draining and replacing the solvent each time. After the final wash, the sample was allowed to dry in a fume hood at room temperature (23°C) for at least 1 hour.
[0364] The test results of the obtained porous membrane are shown in Table 19.
[0365] Table 19
[0366]
[0367] The resulting porous film was cut into 3" wide strips, placed between two release liners, and then calendered at 1000 pli and 5 fpm to densify the sample.
[0368] The test results of the obtained dense film are shown in Table 20.
[0369] Table 20
[0370]
[0371]
[0372] The resulting dense film is then cut into 1" x 1" squares. To stack the squares, i.e., to stack multiple layers of dense film, a steel mold is used to constrain the stack in the x and y directions. The steel mold has a cavity with a width of 1.0625", a length of 1.0625", a height of 1.5" and a top plunger, and is placed in an oven at 300℉ (149℃) for 30 minutes to preheat the mold. The mold is removed from the oven and 1" x 1" squares are stacked into the mold to a height of 1.4". Isolation pads are placed on the top and bottom of the stack. The top plunger is inserted, and the mold and stacked film squares are placed in a laboratory oven at 300℉ (149℃) for 15 minutes. The mold and stack are then quickly removed and placed on a heated hydraulic press at 176.6°C (350°F) and pressed by gradually increasing the force to 2000 lbf (corresponding to a pressing pressure of 2000 pounds per square inch (13.8 MPa)) over 3 minutes. The mold is then removed from the hydraulic press and opened, and additional film squares are added. The process is then repeated three times until the stack is approximately 1" high. The resulting pressed film stack is a cohesive block (or bonded film stack) made of stacked film squares, which is removed from the hydraulic press and allowed to cool to room temperature (23°C), and then a band saw is used to cut through all the film layers to cut out the sheet. In the sheet obtained by cutting, the hexagonal boron nitride particles are oriented in a direction perpendicular to the planar direction of the sheet.
[0373] The test results of the obtained sheets are shown in Table 21.
[0374] Table 21
[0375]
[0376] The hardness of the samples including the elastomer in the final sheet was lower than the hardness of the samples not including the elastomer in the final sheet.
Claims
1. A sheet comprising a composite material, the composite material comprising a polymer and hexagonal boron nitride particles, wherein the hexagonal boron nitride particles comprise flaky hexagonal boron nitride particles, and wherein the flaky hexagonal boron nitride particles are oriented in a direction perpendicular to a planar direction of the sheet, and wherein the composite material comprises at least 70 wt % of the hexagonal boron nitride particles based on the total weight of the composite material, and wherein the sheet has a through-plane thermal conductivity greater than 12 W / m*K.
2. The sheet material according to claim 1, wherein the composite material is obtained by densifying a material comprising a porous polymer network.
3. The sheet material according to claim 1 or 2, wherein the composite material comprises at least 80 wt%, preferably at least 85 wt%, more preferably at least 90 wt%, more preferably greater than 90 wt% of the hexagonal boron nitride particles, based on the total weight of the composite material.
4. The sheet material according to any one of claims 1 to 3, wherein the sheet material has a through-plane thermal conductivity of at least 15 W / m*K.
5. The sheet material of any one of claims 1 to 4, wherein the sheet material has an orientation index greater than 4.
0.
6. The sheet material according to any one of claims 1 to 5, wherein the composite material further comprises 0.1 wt% to 10 wt% of mineral oil, based on the total weight of the composite material.
7. The sheet material according to any one of claims 1 to 6, wherein the polymer is selected from the group consisting of polyurethanes, polyesters, polyamides, polyethers, polycarbonates, polyimides, polysulfones, polyethersulfones, polyphenylene oxides, polyacrylates, polymethacrylates, polyacrylonitrile, polyolefins, styrene, styrene-based copolymers, styrene-based copolymers, chlorinated polymers, fluorinated polymers, copolymers of ethylene and chlorotrifluoroethylene, and combinations thereof.
8. The sheet material according to any one of claims 1 to 7, wherein the polymer has a 4 g / mol to 1×10 7 Ultra-high molecular weight polyethylene with a number average molecular weight in the g / mol range.
9. The sheet material according to any one of claims 1 to 8, wherein the composite material has a porosity of at most 40%. 10 . The sheet material according to claim 1 , wherein the sheet material has a Shore D hardness of 30 to 150.
11. A method for producing a sheet material according to any one of claims 1 to 10, the method comprising: A polymer, a solvent and hexagonal boron nitride particles including plate-like hexagonal boron nitride particles are provided, and the polymer, the solvent and the hexagonal boron nitride particles are mixed to form a suspension of the hexagonal boron nitride particles in a polymer-solvent solution, wherein the polymer in the polymer-solvent solution has a melting point, and wherein the solvent has a boiling point, and wherein the mixing of the polymer, the solvent and the hexagonal boron nitride particles is performed at a temperature higher than the melting point of the polymer in the polymer-solvent solution and lower than the boiling point of the solvent, forming the suspension into a film in which the plate-like hexagonal boron nitride particles are oriented in a direction parallel to a planar direction of the film, inducing phase separation of the polymer and the solvent, removing at least a portion of the solvent from the membrane to obtain a porous membrane, optionally compressing the porous membrane to obtain a dense membrane, stacking a plurality of layers of the porous membrane or the dense membrane one after another to obtain a membrane stack, pressing the membrane stack to obtain a bonded membrane stack, and Sheets are cut from the bonded film stack in a direction perpendicular to the plane of the stacked film layers.
12. A method for producing a sheet material according to any one of claims 1 to 10, the method comprising: A polymer, a solvent and hexagonal boron nitride particles including plate-like hexagonal boron nitride particles are provided, and the polymer, the solvent and the hexagonal boron nitride particles are mixed to form a slurry, wherein the slurry is a suspension of the polymer and the hexagonal boron nitride particles in the solvent, and wherein the polymer has a melting point, and wherein the solvent has a boiling point, and wherein the mixing of the polymer, the solvent and the hexagonal boron nitride particles is performed at a temperature lower than the melting point of the polymer and lower than the boiling point of the solvent, forming the slurry into a film in which the plate-like hexagonal boron nitride particles are oriented in a direction parallel to a planar direction of the film, heating the film in an environment to retain in the film at least 90 weight percent of the solvent based on the weight of the solvent in the film and to dissolve in the solvent at least 50 weight percent of the polymer based on the total weight of the polymer, inducing phase separation of the polymer and the solvent, removing at least a portion of the solvent from the membrane to obtain a porous membrane, optionally compressing the porous membrane to obtain a dense membrane, stacking a plurality of layers of the porous membrane or the dense membrane one after another to obtain a membrane stack, pressing the membrane stack to obtain a bonded membrane stack, and Sheets are cut from the bonded film stack in a direction perpendicular to the plane of the stacked film layers.
13. The method according to claim 11 or 12, further comprising: The membrane stack is heated before pressing the membrane stack.
14. The method of any one of claims 11 to 13, wherein pressing the film stack is performed at a temperature of at least 110°F.
15. The method according to any one of claims 11 to 14, further comprising: The bonded film stack is heated before sheets are cut from the bonded film stack.
16. The method according to any one of claims 11 to 15, wherein pressing the membrane stack is performed at a pressing pressure of at least 2.0 MPa.
17. The method according to any one of claims 11 to 16, wherein pressing the film stack is performed in a pressing direction while constraining the film stack in a first direction perpendicular to the pressing direction.
18. A method according to any one of claims 11 to 17, wherein pressing the film stack is performed in a pressing direction while constraining the film stack in a first direction perpendicular to the pressing direction and in a second direction perpendicular to the pressing direction, and wherein the first direction is perpendicular to the second direction.