Method and apparatus for producing electrically conductive bulk beta-GA2O3 single crystals and electrically conductive bulk beta-GA2O3 single crystals

By using low radiation reflectivity internal heat insulation parts and dynamically reducing the growth rate in the Chaikolasky method, combined with high thermal conductivity atmosphere, the problem of unstable growth of large diameter high conductivity β-Ga2O3 single crystals is solved, and large-scale Diameter and high conductivity crystal growth, suitable for high-performance power electronic devices.

CN118922590APending Publication Date: 2024-11-08SILTRONIC AG

Patent Information

Application Number
CN202380019587.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-01-31
Filing Date
2023-01-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art is difficult to grow bulk β-Ga2O3 single crystals with large diameter and high conductivity, and the Chaiklasky method causes growth instability due to heat accumulation caused by free carrier absorption during the growth process, which limits the crystal. cylindrical length.

Method used

The use of low radiation reflectivity internal heat insulation in the growth chamber and dynamically reduces growth rates, combined with a non-reducing atmosphere with high thermal conductivity (such as helium) to reduce heat reflection and accumulation, ensuring high conductivity and large size β-Ga2O3 single crystal growth.

Benefits of technology

It is achieved to grow high conductivity β-Ga2O3 single crystals with a diameter greater than one inch and a length greater than 25mm, and maintain high structural quality, which is suitable for power electronic devices with vertical configuration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922590A_ABST
    Figure CN118922590A_ABST
Patent Text Reader

Abstract

A method and apparatus for producing electrically conductive bulk beta-Ga2O3 single crystals grown from a melt, in particular by the firecoraski process. In order to grow beta-Ga2O3 single crystals (7) of high conductivity, large diameter (greater than one inch) and bonding length of more than 25 mm, the growth furnace is provided with an inner insulation (8) having a low radiative reflectance (R) in the near infrared spectrum region of 1 [mu] m to 3 [mu] m, which reduces the heat reflection back to the single crystal (7) being grown and thus increases the heat dissipation from the single crystal (7) being grown. The low reflectance may be achieved by high emissivity or high transmittance. Furthermore, the beta-Ga2O3 single crystal (7) is grown at a rate that is dynamically reduced as the growth proceeds to dynamically reduce the latent heat of crystallization and the heat that will dissipate from the single crystal (7) being grown.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention generally relates to a method for growing bulk β-Ga by the Czochralski method. 2 O 3 The present invention also relates to a method and apparatus for growing conductive bulk β-Ga single crystals by the Czochralski method. 2 O 3 Single crystals, especially large diameter conductive bulk β-Ga 2 O 3 Single crystal. Background Art

[0002] Ga 2 O 3 The β phase (β-Ga 2 O 3 ) is an emerging ultra-wide bandgap n-type oxide semiconductor that has great potential in UV optoelectronics and high-power electronics applications. This is due to the wide bandgap of 4.85 eV and the high theoretical breakdown field of 8 MV / cm that makes the compound transparent down to the UV spectral region.

[0003] For devices, a bulk single crystal is required, which serves as a base (or substrate) for the epitaxial layers, on which the device structures are then fabricated. Although foreign substrates can be used for such purposes, they usually degrade the quality of the layers, and thus the device performance, due to the lattice mismatch between the substrate and the layers. For this reason, native substrates are required.

[0004] Based on β-Ga 2 O 3 Power devices such as Schottky diodes and field effect transistors (FETs) can be cost-effective in terms of energy conservation and energy management. They can be applied to many industrial fields, such as mobile transportation (including electric vehicles, aircraft and ships), as well as railways or power grids. Generally, power switching devices can be designed in two configurations: horizontal (planar) configuration and vertical configuration. In the horizontal configuration, the substrate is electrically insulating and serves as a support for the layer with all contacts located thereon (such as source, drain and gate contacts in FET devices). In the vertical configuration, the substrate is highly conductive and, in addition to supporting the epitaxial layer, also serves as an electrical contact. Compared with the horizontal configuration, devices in the vertical configuration can switch higher voltages.

[0005] Bulk β-Ga 2 O 3Single crystals are known in the art and can be grown from the melt by different techniques: optical floating zone (OFZ), guided mode freezing (EFG), Bridgman or vertical gradient solidification (VGF) and Czochralski (Czochralski) methods.

[0006] The OFZ method, which is a crucible-free method, can only produce small crystals with a diameter of no more than one inch. 2 O 3 An example of this approach for single crystals can be found in E.G. Villora et al., entitled “Large-size β-Ga 2 O 3 The OFZ method enables the growth of both electrically insulating and conductive bulk β-Ga along different crystallographic directions. 2 O 3 Single crystal, because growth occurs on top of the seed crystal.

[0007] For growing bulk β-Ga 2 O 3 The EFG method of single crystal uses an Ir crucible and an Ir mold (shaper) on top of the crucible. <010> Crystallographic orientation grows in the form of a slab with the major faces Or (001) (large face of the slab), which can be as large as 4 or 6 inches. However, (010) oriented substrates can only be made from 10×15 mm 2 Cross-section of a crystal slab is prepared. 2 O 3 An example of this approach for single crystals is given in A. Kuramata et al., entitled “High-quality β-Ga 2 O 3single crystals grown by edge-defined film-fed growth" (Jpn. J. Appl. Phys. 55 (2016) 1202 A2) and in patent or patent application documents: WO2013172227A1 (corresponding to JP6,421,357B2; EP 2851458 A4; US2015125699 Al), WO2013073497A1 (JP 5,491,483 B2; EP 2,801,645 Bl; US2014352604Al) and WO 2014073314Al (JP5,756,075B2, EP2,933,359Bl, US9,926,646B2). For example, cylindrical β-Ga grown by the EFG method 2 O 3 The crystal has been disclosed in patent application document No. CN 112210823 A.

[0008] For growing bulk β-Ga 2 O 3 The Bridgman and VGF methods of single crystals utilize a noble metal crucible, such as a Pt-Rh alloy crucible (Bridgman method) or an Ir crucible (VGF method), in which a melt solidifies into a single crystal on top of a seed crystal that may have a different crystallographic orientation. Both electrically insulating and conductive β-Ga can be grown in this way. 2 O 3 Single crystal. In the paper titled “Scaling-Up of Bulkβ-Ga 2 O 3 The VGF method described in the paper "Single Crystals by the Czochralski Method" (ECS J. Solid State Sci. Technol. 6 (2017) Q3007-Q3011) allows the growth of highly conductive β-Ga2O3 with a diameter of nearly 2 inches. 2 O 3 Single crystals, but they are very short, no longer than 20 mm. Bulk β-Ga grown by the Bridgman method 2 O 3 The method of single crystal is disclosed in US Pat. No. US10,570,528B2 by K. Hoshikawa et al. 2 O 3The Bridgman method reported in the paper "crystal growth by the vertical Bridgman technique in a resistance heating furnace in ambient air" (J. CrySt. Growth, 545 (2020) 125724) is able to grow electrically insulating crystals of 2 inches in diameter perpendicular to the (100) plane, but the cylinder length does not exceed about 25 mm. For example, in the paper entitled "50 mm diameter Sn-doped (001) β-Ga 2 O 3 As discussed in the paper "crystal growth using the vertical Bridgman technique in ambient air" (J. Cryst. Growth 546 (2020) 125778), the same crystal size involves conductive crystals with an orientation perpendicular to the (001) plane grown by the Bridgman method.

[0009] The Czochralski method provides the largest bulk β-Ga grown in terms of volume and with high structural quality. 2 O 3 The feasibility of single crystals. For example, Galazka et al. 2 O 3 Single Crystals by the Czochralski Method" (ECS J.Solid StateSci.Technol.6(2017)Q3007-Q3011); "β-Ga 2 O 3 for wide-bandgap electronics andoptoelectronics" (Semicond. Sci Technol. 33 (2018) 113001) and "Bulk single crystals of β-Ga 2 O 3and Ga-based spinels as ultrawide bandgap transparent semiconducting oxides" (Prog. Cryst. Growth Charact. Mater. 67 (2021) 100511), reported that two-inch diameter electrically insulating crystals can be 60 to 100 mm long. In order to grow such large crystals, it is necessary to maintain a high oxygen partial pressure in the growth atmosphere to minimize Ga 2 O 3 The formation of Ga in the melt has a significant negative impact on the growth process, crucible life and crystal quality (if it can be obtained). As taught by Galazka et al. in European Patent Specification No. EP 3,242,965 B1 (corresponding to US 11,028,501 B2), this requirement is particularly important for β-Ga crystals involving noble metal crucibles. 2 O 3 All melt growth methods for single crystals are necessary.

[0010] Although the electrically insulating bulk β-Ga 2 O 3 Single crystals can have large dimensions in terms of diameter and cylindrical length, but this is not relevant for conductive crystals which are subject to the so-called free carrier absorption. Simply put, the heat generated during the liquid-to-solid phase transition (latent heat of crystallization) cannot be easily dissipated by the growing crystal because this heat is absorbed by the free carriers in the growing crystal in the near-infrared spectral region, with most of the heat being transported through the growing crystal. This leads to an increase in temperature near the growth interface and, in turn, to a reversal of the interface from a convex surface towards the melt to a concave surface. This concave growth interface leads to growth instabilities, which change the growth morphology from a cylindrical to a corkscrew (spiral) shape. The spiral does not allow the manufacture of wafers of the required diameter. Compared to bulk β-Ga grown by the Czochralski method, 2 O 3 This phenomenon related to single crystals was described by Galazka et al. in a paper entitled “On the bulk β-Ga 2 O 3 single crystals grown by the Czochralski method"(J.Cryst.Growth 404(2014)184-191);"Czochralski-grown bulkβ-Ga 2 O 3singlecrystals doped with mono-,di-,tri-,and tetravalent ions"(J.CrySt.Growth 529(2020)125297);"Bulkβ-Ga 2 O 3 single crystals doped with Ce, Ce+Si, Ce+AI, and Ce+AI+Si for detection of nuclear radiation”(J.Alloy.Compd.818(2020)152842; and “Transparent Semiconducting Oxides-Bulk Crystal Growth and FundamentalProperties”(Chapter 4, Jenny Stanford Publishing(2020)). Therefore, with a crystal density higher than 10 18 cm -3 Highly conductive crystals with a free electron concentration of 1.5 Å can be grown by the Czochralski method as short cylinders of about 30 mm for crystals with a diameter of one inch or less and less than 25 mm for crystals with a diameter of two inches. For economic reasons, especially in view of the very high cost of crystal growth, the cylindrical portion of the crystal should be as long as possible to make as many wafers as possible from one crystal while maintaining the desired electrical properties of the electronic device, especially in a vertical configuration. The Czochralski method is able to grow along <010> The crystals are grown along the crystallographic direction, so a (010) oriented wafer is produced from a cross section of a cylindrical section. <010> Directionally grown 2-inch diameter crystals can produce 2-inch diameter (010) oriented high conductivity wafers suitable for power devices in a vertical configuration.

[0011] Undoped bulk β-Ga 2 O 3 The electrical conductivity of a single crystal (independent of the growth method) originates from residual impurities, primarily silicon and / or hydrogen, which can induce a conductivity that is classified as a normal (or ordinary) semiconductor, where the free electron concentration does not exceed about 10 18 cm -3 For higher conductivity, intentional doping is required, which is usually performed using silicon (Si) or tin (Sn) doping, as discussed in the state of the art described above. Also, other dopants such as Nb, Hf or Zr are occasionally used to increase the conductivity of β-Ga. 2 O 3 Induced conductivity. Summary of the invention

[0012] The object of the present invention is to provide a method for producing bulk β-Ga from a melt, in particular by the Czochralski process. 2 O 3 Single crystal conditions, which will ensure the growth of crystals with high conductivity, large size and high structural quality.

[0013] Another object of the present invention is to provide a bulk β-Ga with high conductivity and large size (preferably at least 2 inches in diameter and more than 1 inch in length) 2 O 3 Single crystal.

[0014] Another object of the present invention is to provide a method for producing β-Ga from a melt, in particular by the Czochralski process. 2 O 3 A device for growing single crystals which will be able to carry out the method described and thus grow crystals of high conductivity, large size and high structural quality.

[0015] In a more general aspect, a further object of the present invention is to provide a method and apparatus for producing by the Czochralski process various oxide compounds having high melting points (above 1400° C.) and exhibiting strong absorption in the near infrared spectral region.

[0016] According to a first aspect of the present invention, there is provided a method for producing conductive bulk β-Ga by the Czochralski method. 2 O 3 A method for forming a single crystal, the method comprising the steps of providing a growth furnace to a growth chamber, the growth furnace comprising a Ga 2 O 3 A noble metal crucible of the starting material, surrounding the crucible (3) on all sides and having free space to accommodate the growing bulk β-Ga 2 O 3 The method further comprises providing a thermal shield for the single crystal, and an induction RF coil for heating the crucible and controlling the melt temperature during crystal growth, wherein the RF coil is powered by an RF generator, while the growing crystal is fixed to the translation and rotation mechanism by the seed crystal, the seed crystal holder and the lifting rod. 2 O 3 Starting materials were provided in Ga 2 O 3 The step of forming a shallow donor dopant in the single crystal and the step of supplying a growth atmosphere comprising oxygen mixed with at least one non-reducing gas to the growth chamber and thus to the growth furnace. Next, the Ga 2 O 3 Crucible of starting materials until melting Ga 2 O 3Starting material: Melted Ga 2 O 3 After the starting material, the oriented seed crystal is immersed in the molten starting material and then pulled upward at a translation rate to achieve a predetermined growth rate while rotating at a predetermined rotation rate. During the initial pulling period, the seed crystal diameter is expanded to the final cylindrical diameter, which is pulled to a predetermined cylindrical length. Once the predetermined cylindrical length is reached, the single crystal is separated from the melt and cooled to room temperature together with the growth furnace.

[0017] The essence of the invention is to additionally provide the growth furnace with internal insulation having low radiation reflectivity in the near infrared spectral region of 1 μm to 3 μm to reduce the reflection of heat back to the growing single crystal and thus increase the heat dissipation from the growing single crystal. This is combined with a dynamic reduction in the growth rate from the start of seed pulling to crystal separation. The growth rate is reduced from an initial growth rate of 1 mm / h to 10 mm / h at the beginning of growth to a final growth rate of 0.2 mm / h to 1 mm / h at the end of growth (when the single crystal has reached a predetermined cylindrical length). This solution dynamically reduces the latent heat of crystallization as growth proceeds and dynamically reduces the heat to be dissipated from the growing single crystal.

[0018] Preferably, the inner thermal insulation with low radiation reflectivity has a high emissivity (emissivity) or a high reflectivity in the near infrared spectral region, which is higher than 0.3 at room temperature.

[0019] The growth rate may decrease linearly or non-linearly from the initial growth rate to the final growth rate.

[0020] In a preferred embodiment, the growth rate decreases at different rates from the initial growth rate to the final growth rate.

[0021] In another preferred embodiment, the growth rate may be decreased from the initial growth rate to the final growth rate continuously or in blocks combining a constant growth rate and a decreasing growth rate.

[0022] Advantageously, in addition to oxygen, the growth atmosphere comprises a non-reducing gas with high thermal conductivity, preferably He in a concentration of 10 vol.% to 95 vol.%, to further enhance heat dissipation from the growing crystal via gas convection.

[0023] According to a second aspect of the present invention, there is provided a conductive bulk β-Ga grown by the Czochralski method according to the above method. 2 O 3 Single crystal. β-Ga 2 O 3The single crystal has a cylindrical diameter greater than one inch, a cylindrical length greater than 25 mm, and the following electrical properties formed by shallow donors as measured by the Hall effect: 1×10 18 cm -3 Up to 10×10 18 cm -3 Free electron concentration, 50 cm 2 V -1 s -1 Up to 120cm 2 V -1 s -1 The electron mobility is 0.01Ωcm to 0.04Ωcm.

[0024] In a preferred embodiment of the present invention, β-Ga 2 O 3 The single crystals have a cylindrical diameter of two inches or more.

[0025] Advantageously, the dopants forming shallow donors are Si and / or Sn.

[0026] According to a third aspect of the present invention, there is provided a method for producing a conductive bulk β-Ga with a predetermined cylinder diameter and cylinder length by a Czochralski method. 2 O 3 The equipment includes a growth chamber and a growth furnace, wherein the growth furnace includes a Ga 2 O 3 A precious metal crucible of the starting material, surrounding the crucible on all sides and leaving free space to accommodate the growing bulk β-Ga 2 O 3 The apparatus also includes an RF generator for powering the RF coil, a translation and rotation mechanism coupled to the seed crystal through a seed crystal holder, a lifting rod, and a connection to the lifting rod or a growth furnace for monitoring bulk β-Ga 2 O 3 A scale for measuring the growth rate of a single crystal.

[0027] According to the present invention, the growth furnace further comprises an internal thermal insulator having low radiation reflectivity in the near infrared spectral region of 1 μm to 3 μm, which reduces heat reflection back to the growing single crystal and thereby increases heat dissipation from the growing single crystal.

[0028] Advantageously, the inner thermal insulation with low radiation reflectivity has a high emissivity in the near infrared spectral region, which is higher than 0.3 at room temperature. Here, the inner thermal insulation is preferably selected from the group consisting of opaque aluminum oxide, zirconium oxide, magnesium oxide and yttrium oxide.

[0029] In another advantageous solution of the invention, the inner thermal insulation with low radiation reflectivity has a high transmittance in the near infrared spectral region, which is higher than 0.3 at room temperature. This is preferably achieved by a transparent ceramic selected from the group consisting of aluminum oxide, yttrium oxide and yttrium aluminum garnet or crystalline sapphire.

[0030] In a preferred embodiment of the apparatus, the growth atmosphere contains, in addition to oxygen, a non-reducing gas with high thermal conductivity, most preferably He in a concentration of 5 to 95 vol.%, to further enhance heat dissipation from the growing crystal via gas convection.

[0031] Used to grow bulk β-Ga that exhibits high absorptivity in the near-infrared region 2 O 3 Further advantages and other features of the inventive method and apparatus for single crystal or other oxide crystals will become apparent from the detailed description with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 is a cross-sectional view of a schematic growth furnace for growing an oxide single crystal by the Czochralski method;

[0033] Figure 2 Bulk β-Ga grown by the Czochralski method 2 O 3 Different growth rate curves of single crystals; and

[0034] Figure 3 shows the growth of bulk β-Ga by the Czochralski method. 2 O 3 The actual growth rate curve output during the growth run of a single crystal. DETAILED DESCRIPTION

[0035] Figure 1 The growth furnace 1 shown in FIG. 1 is generally suitable for growing bulk oxide single crystals by the Czochralski method, and is particularly suitable for growing bulk β-Ga single crystals by the Czochralski method. 2 O 3 The growth furnace 1 is contained in a water-cooled growth chamber (not shown) into which a predetermined growth atmosphere 2 is introduced. The growth furnace 1 consists of a noble metal crucible 3 (which contains Ga 2 O 3 The crucible is composed of a starting material 4, preferably with a lid 5 on it, and a heat shield 6 surrounding the crucible from all sides. Above the crucible is a free space (growth zone) that accommodates the growing bulk β-Ga 2 O 3The growth furnace 1 also includes an inner thermal insulator 8 having defined optical properties, as further explained below. The noble metal crucible 5 is inductively heated by an RF coil 9 located outside the thermal insulator 6 and powered (or energized) by an RF generator (not shown). Bulk β-Ga 2 O 3 Single crystal 7 grown from crystallographically oriented β-Ga 2 O 3 On the seed crystal 10, β-Ga 2 O 3 The seed crystal 10 is fixed to a seed crystal holder 11 connected to a lifting rod 12. The lifting rod 12 is connected to a seed crystal holder 11 for making the growing β-Ga 2 O 3 The pulling and rotating mechanism (not shown) for the translation TR and rotation R of the single crystal 7 and the β-Ga 2 O 3 A weighing scale (not shown) is used to weigh the single crystal 7. Alternatively, the weighing scale is coupled to the growth furnace 1. In each case, the weighing scale indicates the growth rate of the growing single crystal 7 by weighing the mass of the crystal directly or by weighing the mass difference between the furnace and the growing crystal 7. The signal from the weighing scale is coupled to a controller, which controls the power of the generator and, therefore, the melt temperature.

[0036] The heat insulator 6 is a refractory material that is resistant to high temperatures, depending on the melting point of the oxide crystals to be grown. 2 O 3 The melting point of is about 1800°C. The thermal insulation 6 typically comprises a quartz tube and alumina or zirconia tubes, pellets, felts on the outer part of the growth furnace 1. The goal of the thermal insulation 6 is to reduce heat losses and establish a predetermined temperature gradient within the crucible and the growth zone to minimize thermal stresses and associated structural and point defects in the growing crystal 7. In particular, for growing bulk β-Ga 2 O 3 Single crystals require low temperature gradients and therefore the best possible thermal insulation. This is β-Ga with anisotropic mechanical, thermal and optical properties 2 O 3 Melt chemistry (decomposition) and monoclinic system and its consequences.

[0037] For β-Ga 2 O 3 The crystalline noble metal crucible 3 is iridium and its alloys, such as iridium platinum alloy. Moreover, other crucible materials are conceivable, such as the platinum-rhodium alloy described by Hoshikawa et al. (as mentioned above) for the Bridgman process.

[0038] For the growth of β-Ga 2 O3 The growth atmosphere 2 for the single crystal 7 (especially large diameter, greater than 1 inch) comprises oxygen (preferably at least 5 vol.%) and at least one other non-reducing gas, such as Ar, N 2 , CO 2 , He, Xe and Ne as described in Patent No. US11,028,501 B2 to Galazka et al., which is incorporated herein by reference.

[0039] For the Czochralski method, β-Ga 2 O 3 The seed crystal 10 is crystallographically oriented along the

[010] direction, which is parallel to the β-Ga 2 O 3 The (100) and (001) cleavage planes present in the monoclinic system of . Other seed orientations tilted relative to the

[010] direction, such as

[110] , may also be used.

[0040] The crystal growth process is as follows. After the growth furnace 1 is assembled, the noble metal crucible 3 with the starting material 4 is heated by the RF coil 9 until the Ga 2 O 3 Starting material 4. Once Ga 2 O 3 Melt heat stable, oriented β-Ga 2 O 3 The seed crystal 10 is immersed in Ga 2 O 3 The melt is rotated at a rotation rate R. Next, the oriented β-Ga 2 O 3 The seed crystal 10 is pulled upward at a translation rate TR while expanding its diameter to a predetermined cylindrical diameter D by gradually lowering the melt temperature via an RF generator. When the crystal reaches a predetermined cylindrical length L, it is separated from the melt, slowly cooled to room temperature, and removed from the growth furnace 1 .

[0041] The Czochralski method is used to convert conductive (normal or degenerate semiconductor) bulk β-Ga 2 O 3 The problem of growing a single crystal as a long straight cylinder stems from the intrinsic properties of the compound, namely from the absorption of heat by free carriers that is transmitted through the growing crystal. The heat that must be dissipated from the crystal is generated at the crystal growth interface during the liquid-solid phase transition. This interface protrudes toward the melt (i.e., the conical part of the crystal is immersed in the melt) and ensures stable growth. The heat absorbed by the free carriers raises the temperature of the crystal near the growth interface, and over a certain crystal length, the heat cannot be easily dissipated. Once the temperature in the crystal reaches Ga 2 O 3The melting point of the crystal is reached, and part of the crystal immersed in the melt is melted back. This phenomenon is called interface inversion. After the interface inversion, the growth becomes unstable and the growth morphology changes from a straight cylinder to a corkscrew shape (spiral). This crystal shape cannot produce wafers of the diameter expected from a straight cylinder, so the only usable part of the crystal used to make wafers is this cylindrical part. Highly conductive β-Ga with a diameter greater than one inch 2 O 3 The length of the cylindrical part of the crystal is not longer than 25 mm. Crystal β-Ga 2 O 3 The high conductivity is understood to be more than 10 18 cm -3 The value of the free electron concentration.

[0042] In order to increase the diameter of the highly conductive β-Ga grown by the Czochralski method to more than 1 inch 2 O 3 The length of the cylindrical part of the crystal, the following technical solutions were found to be effective:

[0043] (i) Reflection from the inner insulation back to the growing β-Ga 2 O 3 Reduction of heat in the single crystal; and / or

[0044] (ii) Dynamic decrease of latent heat of crystallization as growth proceeds.

[0045] like Figure 1 As shown, the crystal surface dissipates and exchanges heat with the surrounding environment in two ways: by gas convection C and by radiation RA, the latter being significantly more efficient. In radiative heat exchange, the heat leaving the crystal surface in all directions interacts with the metal crucible 3 and its lid 5 (if any) and the inner thermal insulation 8, where the heat is partially reflected, partially absorbed, and partially transmitted. This can be described in dimensionless measurements as: THA=1=R+E+T, where THA is the total heat, R is the reflectivity, E is the emissivity, and T is the transmittance. Therefore, the reflectivity can be described as R=1-ET. In order to minimize heat reflection from the inner thermal insulation 8, it should have a high emissivity E or a high transmittance T. These optical properties R, E and T are related to the near-infrared (NIR) region where most of the heat is transmitted. Considering Ga 2 O 3The NIR region is between 1 μm and 3 μm, taking into account the melting point (1800°C), the black body radiation at this temperature, and the lower temperature of the growing crystal (assuming a minimum of 1200°C). Therefore, the requirement for the inner thermal insulation 8 is a low reflectivity R in the spectral region of 1 μm to 3 μm, which can be achieved by a high E value or T value in this spectral region. The optical properties of the material depend to a large extent on the spectral region and the temperature. For example, the emissivity E varies over a wide range in the NIR spectral region, also at high temperatures, so it is difficult to define an exact value. However, at some sub-regions of the NIR region in question, smaller E values ​​will not have a large effect on the overall heat exchange. In any case, the emissivity E should be greater than 0.3 in the NIR spectral region of 1 μm to 3 μm when measured at room temperature. Suitable refractory materials for the inner thermal insulation 8 are: aluminum oxide, zirconium oxide, yttrium oxide and magnesium oxide, which preferably have a rough surface to enhance diffuse scattering.

[0046] Another solution is to increase the transmittance T of the inner thermal insulation 8. This can be achieved by a thermal insulation that is transparent to the NIR spectral region defined above. Since standard refractory materials are substantially opaque to the NIR (or substantially impermeable to the NIR), transparent ceramics or crystalline sapphire can be used. Both transparent ceramics (e.g., alumina and yttrium oxide) and crystalline sapphire in different shapes (tubular and cap-shaped) are available. For the transmittance T, the same considerations apply to wavelength and temperature as in the case of the emissivity E. Moreover, in this case, the transmittance T should be greater than 0.3 in the NIR spectral region from 1 μm to 3 μm when measured at room temperature.

[0047] Another solution mentioned above for more efficient heat removal from the crystal is the dynamic reduction of the heat generated during growth. This is accomplished by dynamically reducing the growth rate as the crystal length increases. It should be noted that the growth rate V combines the droplet (which transforms into a solid) and the translation rate TR of the crystal.

[0048] Figure 2The graph shows the curves of the growth rate V that can reduce the latent heat of crystallization in a dynamic way. In general, at the beginning of growth, i.e. during seeding, seed expansion (shoulder release) and the beginning of the cylindrical part, the growth rate V1 can be relatively high, between 1 mm / h and 10 mm / h, because the heat generated is small (seeding, shoulder release) or the crystal length is small enough to effectively dissipate the heat (early cylindrical part). Afterwards, the growth rate is reduced to a final value V2 of 0.2 mm / h to 1 mm / h to reduce the heat generated. The reduction of the growth rate V can be carried out from the beginning of growth, as indicated by the curves P1, P2 and P5 (especially when the initial growth rate is high); or it can be carried out afterwards, as indicated by the curves P3 and P4. It can be done in a linear or nonlinear way, such as a continuous reduction, or in step-wise blocks indicated by the crystal length segments L1, L2, L3 and L4. Figure 3 An example of growth rate from an actual growth experiment is shown, where initially in the first block 0 to L1 an initial value V1 = 1.7 mm / h is held constant, then in blocks L1 to L3 it decreases linearly to a final value V2 = 0.7 mm / h, which is held constant in the last block L3 to L4 of crystal growth.

[0049] Another means (or tool) for heat management is to use a non-reducing gas with high thermal conductivity, especially He, in the growth atmosphere 2. This will enhance the heat dissipation from the growing crystal 7 by gas convection C. Preferably, the He in the growth atmosphere 2 is used in combination with a reduction in the amount of heat reflected back to the crystal and a reduction in the amount of latent heat of crystallization. In addition to oxygen, the He concentration in the growth atmosphere is between 10 vol.% and 95 vol.%.

[0050] By using the above technical solutions, it is possible to increase the yield of highly conductive bulk β-Ga grown by the Czochralski method. 2 O 3 The cylindrical length L of the single crystal 7 (whose diameter is greater than 1 inch). The bulk β-Ga with a diameter D = 2 inches 2 O 3 The single crystal can be grown to a cylindrical length L exceeding 25 mm, between 25 mm and 50 mm. Bulk β-Ga 2 O 3 High conductivity in single crystals can be achieved by intentionally doping the material with elements that form shallow donors. The most effective dopants are Si and Sn, but also Nb, Zr, and Hf. To achieve high conductivity, Ga 2 O 3 The starting material 4 should be doped with 0.05 mol.% to 0.3 mol.% SiO 2Due to the high partial pressure of Sn-containing species, 0.5 mol.% to 4 mol.% SnO should be doped 2 The dopants that form shallow donors can be used alone or in combination. Bulk β-Ga doped with Si and / or Sn at the above concentrations 2 O 3 The electrical properties of the single crystal are as follows (measured by the Hall effect): 1×10 18 cm -3 Up to 10×10 18 cm -3 Free electron concentration, electron mobility = 50-120cm 2 V -1 s -1 , and a resistivity of 0.01Ωcm to 0.04Ωcm. A 2-inch diameter bulk β-Ga with this electrical property 2 O 3 Single crystal 7 enables the production of 2-inch diameter conductive wafers suitable for homoepitaxial growth and, subsequently, for the manufacture of power electronics in a vertical configuration. In particular, this crystal enables the production of large wafers with a (010) surface orientation, which exhibits the highest growth rate for homoepitaxial films by molecular beam epitaxy. Furthermore, other wafer orientations, such as (100) or (001), including offcuts of a few degrees from these orientations, can also be produced. Bulk β-Ga obtained by the above method and apparatus 2 O 3 The single crystals have a high structural quality characterized by a narrow rocking curve with a full width at half maximum typically below 30 arcsec, which makes the fabricated wafers suitable for homoepitaxial films with high quality.

Claims

1. A method for producing a conductive bulk β-Ga2O3 single crystal having a predetermined cylinder diameter (D) and cylinder length (L) by a Czochralski method, the method comprising the following steps: (i) providing a growth chamber with a growth furnace (1), the growth furnace (1) comprising a noble metal crucible (3) having a Ga2O3 starting material (4) therein, a thermal insulator (6) surrounding the crucible (3) from all sides and having a free space to accommodate a growing bulk β-Ga2O3 single crystal (7), and an induction RF coil (9) for heating the crucible (3) and controlling the melt temperature during crystal growth, wherein the RF coil (9) is powered by an RF generator, and the growing crystal (7) is fixed to a translation and rotation mechanism via a seed crystal (10), a seed crystal holder (11) and a lifting rod (12); (ii) providing the Ga2O3 starting material (4) with a dopant that forms a shallow donor in the Ga2O3 single crystal (7); (iii) providing a growth atmosphere (2) to the growth chamber and thereby to the growth furnace (1), the growth atmosphere (2) comprising oxygen mixed with at least one non-reducing gas; (iv) heating the crucible (3) having the Ga2O3 starting material (4) by the RF coil (9), and subsequently melting the Ga2O3 starting material (4); (v) immersing the oriented seed crystals (10) into the molten starting material (4); (vi) pulling the seed crystal (10) upward at a translation rate (TR) to achieve a predetermined growth rate (V) while rotating at a rotation rate (R); (vii) while pulling, expanding the diameter of the seed crystal to the final cylindrical diameter (D) of the single crystal (7); (viii) pulling the single crystal (7) having the cylindrical diameter (D) to a predetermined cylindrical length (L); (ix) separating the single crystal (7) from the melt, and (x) cooling the growth furnace (1) with the grown single crystal (7) to room temperature, It is characterized in that - step (i) comprises additionally providing the growth furnace (1) with an internal thermal insulation (8) having a low radiation reflectivity (R) in the near infrared spectral region of 1 μm to 3 μm to reduce heat reflection back to the growing single crystal (7) and thereby increase heat dissipation from the growing single crystal (7); and - Steps (vi), (vii) and (viii) of pulling the single crystal (7) from seeding to separation include a dynamic reduction in the growth rate (V) from an initial growth rate (V1) of 1 mm / h to 10 mm / h at the beginning of growth to a final growth rate (V2) of 0.2 mm / h to 1 mm / h at the end of growth when the single crystal (7) has reached a predetermined cylindrical length (L), so as to dynamically reduce the latent heat of crystallization as the growth proceeds and dynamically reduce the heat to be dissipated from the growing single crystal (7).

2. The method according to claim 1, characterized in that The inner thermal insulation (8) with low radiation reflectivity (R) has a high emissivity (E) in the near infrared spectral region, which is higher than 0.3 at room temperature.

3. The method according to claim 1, characterized in that The inner thermal insulation (8) having a low radiation reflectivity (R) has a high transmittance (T) in the near infrared spectral region, which is higher than 0.3 at room temperature.

4. The method according to any one of claims 1 to 3, characterized in that The growth rate (V) decreases linearly (P1, P2) from the initial growth rate (V1) to the final growth rate (V2).

5. The method according to any one of claims 1 to 3, characterized in that The growth rate (V) decreases non-linearly (P5) from the initial growth rate (V1) to the final growth rate (V2).

6. The method according to any one of claims 1 to 5, characterized in that The growth rate (V) decreases from the initial growth rate (V1) to the final growth rate (V2) at different rates (P2, P5).

7. The method according to any one of claims 1 to 6, characterized in that The growth rate (V) decreases continuously (P1, P2, P5) from the initial growth rate (V1) to the final growth rate (V2).

8. The method according to any one of claims 1 to 6, characterized in that The growth rate (V) decreases from the initial growth rate (V1) to the final growth rate (V2) in blocks (L1 to L4) that combine a constant growth rate and decreasing growth rates (P3, P4).

9. The method according to any one of claims 1 to 8, characterized in that The step (iii) of providing the growth atmosphere (2) comprises providing a non-reducing gas with high thermal conductivity in addition to oxygen, preferably He in a concentration of 10 vol.% to 95 vol.%.

10. A conductive bulk β-Ga2O3 single crystal (7) obtained according to any one of claims 1 to 9, It is characterized in that It has a cylindrical diameter (D) greater than one inch, a cylindrical length (L) greater than 25 mm, and the following electrical properties formed by shallow donors according to Hall effect measurements: 1×10 18 cm -3 Up to 10×10 18 cm -3 Free electron concentration, 50 cm 2 V -1 s -1 Up to 120cm 2 V -1 s -1 The electron mobility is 0.01Ωcm to 0.04Ωcm.

11. The bulk β-Ga2O3 single crystal (7) according to claim 10, characterized in that: The cylindrical diameter (D) is two inches or greater.

12. The bulk β-Ga2O3 single crystal (7) according to claim 10 or 11, characterized in that: Dopants forming shallow donors are Si and / or Sn.

13. An apparatus for producing a conductive bulk β-Ga2O3 single crystal having a predetermined cylinder diameter (D) and cylinder length (L) by a Czochralski method, the apparatus comprising: (i) Growth chamber, (ii) a growth furnace (1) comprising a noble metal crucible (3) having Ga2O3 starting material (4) therein, a thermal insulator (6) surrounding the crucible (3) and having free space to accommodate a growing bulk β-Ga2O3 single crystal (7), and an induction RF coil (9) for heating the crucible (3) and controlling the melt temperature during crystal growth; (iii) an RF generator for powering the RF coil (9); (iv) a translation and rotation mechanism connected to the seed crystal (10) through a seed crystal holder (11) and a lifting rod (12); (v) a weighing meter connected to the lifting rod (12) or the growth furnace (1), which is used to monitor the growth rate of the bulk β-Ga2O3 single crystal (7), It is characterized in that The growth furnace also includes an internal thermal insulation (8) having a low radiation reflectivity (R) in the near infrared spectral region of 1 μm to 3 μm, which reduces heat reflection back to the growing single crystal (7) and thereby increases heat dissipation from the growing single crystal (7).

14. The device according to claim 13, characterized in that The inner thermal insulation (8) with low radiation reflectivity (R) has a high emissivity (E) in the near infrared spectral region, which is higher than 0.3 at room temperature.

15. The device according to claim 13 or 14, characterized in that The inner thermal insulation member (8) having low radiation reflectivity (R) is selected from the group consisting of opaque aluminum oxide, zirconium oxide, magnesium oxide and yttrium oxide.

16. The device according to claim 13, characterized in that The inner thermal insulation (8) having a low radiation reflectivity (R) has a high transmittance (T) in the near infrared spectral region, which is higher than 0.3 at room temperature.

17. The device according to claim 13 or 16, characterized in that The inner thermal insulation (8) having low radiation reflectivity (R) is a transparent ceramic selected from the group consisting of aluminum oxide, yttrium oxide and yttrium aluminum garnet.

18. The device according to claim 13 or 16, characterized in that The inner thermal insulation (8) having low radiation reflectivity (R) is crystalline sapphire.

19. The device according to any one of claims 13 to 18, characterized in that In addition to oxygen, the growth atmosphere (2) also contains a non-reducing gas with high thermal conductivity, preferably He in a concentration of 5 vol.% to 95 vol.%.

Citation Information

Patent Citations

  • Method for growing 1-inch columnar gallium oxide single crystal by edge-defined film-fed growth method

    CN112210823A

  • Monocrystalline gallium oxide and monocrystalline gallium oxide substrate

    EP2851458A4

  • Method for growing beta phase of gallium oxide (beta-ga2o3) single crystals from the melt contained within a metal crucible by controlling the o2 partial pressure.

    EP3242965B1

  • Method for growing β-Ga2O3 single crystals

    JP5756075B2

  • Gallium oxide single crystal and gallium oxide single crystal substrate

    JP6421357B2

Cited By

  • Thermal field adjusting method for growing oxide crystal by Czochralski method

    CN121204812A