Crucible, crystal production method, and single crystal

By designing crucibles and crystallization manufacturing methods with different additive concentration distributions in multiple regions, the problem of uneven additive concentrations in oxide single crystals is solved, and the uniform distribution and quality improvement of additives in single crystals is achieved.

CN118922591APending Publication Date: 2024-11-08TDK CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380029359.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-25
Filing Date
2023-01-13
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The problem of uneven concentration of additives in the oxide single crystal in the prior art affects the quality and performance of the single crystal.

Method used

A crucible is designed, whose main body includes multiple regions arranged along a single axis, with different concentrations of additives in each region. By stacking and joining multiple oxide plates to control the concentration distribution of additives, and crystallizing during the crystallization manufacturing process. The species contacts the molten liquid and moves in the vertical direction to grow single crystals.

Benefits of technology

The uniformity of additive concentration is achieved, the quality and performance of single crystals are improved, and the uniform distribution of additives in single crystals is ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922591A_ABST
    Figure CN118922591A_ABST
Patent Text Reader

Abstract

The invention relates to a crucible, a crystal manufacturing method and a single crystal. This crucible (G) is used for growing an oxide single crystal, and is provided with a plurality of oxide plates (G1-G10) that are laminated and joined in the thickness direction, and the concentrations of additives in the oxide plates (G1-G10) are different. In the method for producing a crystal, an oxide single crystal is grown by moving the position of an exposed surface in the vertical direction while bringing a seed crystal into contact with the exposed surface of a melt in a crucible. In the single crystal of gallium oxide, the concentration of the additive in the growth axis direction may preferably be within an average value range of + / -5%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a crucible, a crystal manufacturing method and a single crystal. Background Art

[0002] Patent document 1 discloses a crucible made of a metal such as platinum (Pt) or iridium (Ir). The crucible is used in the Czochralski (CZ) method. In the CZ method, a seed crystal fixed to the front end of a rod is brought into contact with a molten liquid and then slowly pulled up while rotating, thereby growing a single crystal.

[0003] Patent Document 2 discloses a method for growing a gallium oxide (β-Ga2O3) single crystal from a melt contained in an iridium crucible.

[0004] Patent Document 3 discloses a crucible made of gallium oxide. This crucible is used for growing a gallium oxide single crystal.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: U.S. Patent No. 6997986

[0008] Patent Document 2: U.S. Patent No. 11028501

[0009] Patent Document 3: Japanese Patent No. 6390568 Summary of the invention

[0010] Technical problem to be solved by the invention

[0011] The inventors of the present application have conducted special research and found that the concentration of additives in an oxide single crystal becomes non-uniform. A crucible, a crystal production method, and a single crystal are desired that can obtain a single crystal having a highly uniform additive concentration.

[0012] Means for solving technical problems

[0013] The crucible of the present invention is characterized in that it is a crucible for growing oxide single crystals and has a main body, which includes an oxide containing an additive, and in the oxide of the main body, a plurality of regions arranged along a single axis are set, and among the plurality of regions, the concentration of the additive in the first region is higher than the concentration of the additive in the second region.

[0014] The crucible of the present invention is characterized in that it is a crucible for growing a gallium oxide single crystal and comprises a main body, wherein the main body comprises gallium oxide containing an additive, and in the gallium oxide of the main body, a plurality of regions arranged along a single axis are set, and among the plurality of regions, the concentration of the additive in the first region is higher than the concentration of the additive in the second region.

[0015] The crucible of the present invention is a crucible used for growing an oxide single crystal and includes a plurality of oxide plates stacked and joined in a thickness direction, wherein the concentration of an additive in each of the oxide plates is different.

[0016] The crystal production method of the present invention is characterized by using the above-mentioned crucible and comprising the step of growing the oxide single crystal by moving the position of the exposed surface in the vertical direction while bringing the seed crystal into contact with the exposed surface of the melt in the crucible.

[0017] The single crystal of the present invention is obtained by the above-mentioned crystal manufacturing method. The single crystal of the present invention is characterized in that it is a single crystal of gallium oxide composed of a crystal ingot to which Sn or Si is added as an additive, and the concentration of the additive along the growth axis direction is within the range of ±5% of the average value of the concentration of the additive.

[0018] Effects of the Invention

[0019] According to the crucible and the crystal production method of the present invention, a single crystal having a high uniformity of additive concentration can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is a three-dimensional image of a crucible.

[0021] Figure 2 It is an exploded perspective view of the crucible.

[0022] Figure 3 : is a graph showing the relationship between the position Z in the crucible and the concentration C of the additive.

[0023] Figure 4 It is a diagram showing a crystal production apparatus.

[0024] Figure 5 It is a figure which shows the structure around the crucible.

[0025] Figure 6 (A) Figure 6 (B) Figure 6 (C) Figure 6 (D) Figure 6 (E), and Figure 6 (F) is a diagram for explaining the method of producing a crystal.

[0026] Figure 7This is a graph showing the relationship between the position Z in the crucible and the Sn concentration C(Sn).

[0027] Figure 8 A three-dimensional image of a single crystal consisting of an ingot.

[0028] Fig. 9 This is a graph showing the relationship between the position Z in a single crystal and the Sn concentration C(Sn).

[0029] Fig.10 This is a graph showing the relationship between the position Z in the crucible and the Si concentration C(Si).

[0030] Fig.11 This is a graph showing the relationship between the position Z in a single crystal and the Si concentration C(Si).

[0031] Fig.12 : is a graph showing the relationship between the position Z in the crucible and the concentration C of the additive.

[0032] Fig.13 : is a graph showing the relationship between the position Z in the crucible and the concentration C of the additive.

[0033] Fig.14 It is the curing rate g and C g / C0 relationship diagram. DETAILED DESCRIPTION

[0034] Hereinafter, various exemplary embodiments will be described in detail with reference to the accompanying drawings. In each of the drawings, the same or corresponding parts are denoted by the same reference numerals, and repeated descriptions are omitted.

[0035] Figure 1 : is a perspective view of a crucible G. Crucible G is used for growing oxide single crystals. A recess 4 is formed in the central portion of the top surface GT of crucible G. During the crystal growth period, the melt is kept in the recess 4, and the seed crystal contacts the exposed surface of the melt. Crucible G has a plurality of oxide plates G1 to G10 stacked and joined in the thickness direction, forming a main body composed of oxides. The shape of the main body is cylindrical. The number of oxide plates used for crucible G is 2 or more, and the figure illustrates a case of 10.

[0036] The stacking direction (thickness direction) of the oxide plates G1 to G10 is set to the Z axis. The axis orthogonal to the Z axis is set to the X axis, and the axis orthogonal to both the X axis and the Z axis is set to the Y axis. In this figure, an XYZ three-dimensional orthogonal coordinate system is shown. The top surface GT of the crucible G is parallel to the XY plane. In the XY plane including the top surface GT of the crucible G, the center position of the recess 4 observed from the Z axis direction is set to the origin (0,0,0) of the XYZ three-dimensional orthogonal coordinate system. The positive direction of the Z axis is set to the direction extending downward from the origin.

[0037] The crucible G also serves as a raw material for the single crystal to be produced. When the solid material constituting the inner surface of the recess 4 is melted, it becomes a melt in a liquid phase. The melt is used as a raw material for the single crystal to be grown.

[0038] The concentration of additives in each oxide plate G1, G2, G3, G4, G5, G6, G7, G8, G9, and G10 is different. In other words, the concentration of additives varies depending on the location of the crucible G. The concentrations of additives in the oxide plates G1 to G10 are set to C(G1) to C(G10), respectively. As an example, these concentrations satisfy the relationship C(G1)>C(G2)>C(G3)>C(G4)>C(G5)>C(G6)>C(G7)>C(G8)>C(G9)>C(G10). Since the concentration of additives in each oxide plate G1 to G10 can be independently controlled during crystal growth, the degree of freedom in design is increased, and the distribution of additive concentrations in the single crystal of the finally grown ingot can be controlled.

[0039] In this example, the material of each oxide plate G1 to G10 is a metal oxide (e.g., gallium oxide (Ga2O3)), and the additive in the metal oxide is an oxide of an element other than the metal constituting the metal oxide (e.g., SnO2 or SiO2). Furthermore, even if the material is other than these materials, the concentration distribution of the additive in the finally grown ingot (single crystal) can be controlled by stacking a plurality of oxide plates.

[0040] From this point of view, as the material of the oxide plates G1 to G10, in addition to gallium oxide, for example, at least one selected from aluminum oxide (Al2O3), yttrium oxide (Y2O3), zirconium oxide (ZrO2), and lithium niobate (LiNbO3) can be used. As the material of the additive in the oxide plates G1 to G10, for example, at least one selected from SnO2 or SiO2 can be used. In addition, TiO2 and the like are also considered as additives.

[0041] Furthermore, Ga2O3 has crystal structures such as α, β, γ, δ, ε, and κ. Among these crystal structures, β-Ga2O3 has a crystal structure including a monoclinic β phase and has an energy band gap of about 4.8 eV. The melting point of β-Ga2O3 is about 1800°C. In this embodiment, β-Ga2O3 is exemplified as a preferred gallium oxide.

[0042] Furthermore, the additive (e.g., Sn) in the ingot is a specific element (e.g., Sn) contained in the additive (e.g., SnO2) in the oxide plate. The specific element (e.g., Sn) itself is also an additive in the oxide plate. Therefore, the relationship between the concentrations of the specific element (e.g., Sn) in multiple oxide plates is the same as the relationship between the concentrations of the above-mentioned additive (SnO2). If the relative relationship between the concentrations of the additives in each oxide plate is considered, the concentration of the additive can be any one of the molar concentration, mass percentage concentration, or atomic percentage concentration. Unless otherwise specified, the concentration of the additive represents the mass percentage concentration.

[0043] Figure 2 1 is an exploded perspective view of a crucible G. The crucible G is formed by laminating a plurality of oxide plates G1 to G10 and then sintering them at a high temperature to bond them together. This figure shows the oxide plates G1 to G10 before sintering.

[0044] The manufacturing method of the crucible G is as follows. As an example material, the main raw material S1 of the crucible G is gallium oxide (Ga2O3), and the additive S2 is SnO2. First, prepare the main raw material S1 composed of powder and the additive S2 composed of powder. Then, after adding the powder of the additive S2 to the powder of the main raw material S1, these are mixed by a mixing method such as a ball mill to obtain a mixed powder. The mixed powder is filled in rubber, shaped into a thinner disc, and then compacted by a method such as cold isostatic pressing (CIP). In this way, oxide plates G1 to G10 (disc-shaped pressed bodies) can be formed. The mixing ratio of the additive S2 is made different in each oxide plate G1 to G10. Each oxide plate G1 to G10 is obtained by compression molding gallium oxide powder and is a polycrystal of gallium oxide. The pressure during pressing is about 1000kg / cm 2 (98 MPa), and each oxide plate G1 to G10 is preferably sintered at about 1300° C. The thickness of each oxide plate G1 to G10 may be the same or different. In the present embodiment, the thickness of the oxide plates G1 to G10 is set to be the same.

[0045] Next, the oxide plates G1 to G10 with different additive concentrations are overlapped and stacked in the order of additive concentration, and heated by a heating device until the mixed powder undergoes a sintering reaction, and the oxide plates G1 to G10 are joined to form an integrated whole. As a heating device, an electric furnace or the like can be used. The sintering temperature is 1700°C. In order to control the additive concentration, the sintering temperature is set to be lower than the melting point (1800°C) of the main raw material S1.

[0046] The concave portion 4 of the crucible G can be formed by heating the center of the top surface by infrared rays or the like after the crucible G is placed in the crystal manufacturing apparatus. The concave portion 4 of the crucible G can also be formed by machining the center of the top surface. The concave portion 4 of the crucible G can also be formed by machining the upper surface of the first oxide plate G1 before sintering. When the concave portion 4 is formed, the crucible G can hold the molten liquid in the concave portion 4.

[0047] Figure 3 : is a graph showing the relationship between the position Z in the crucible G and the additive concentration C. The additive concentration C decreases in a step-like manner as it moves away from the top surface GT of the crucible G (position in the Z-axis direction: Z=0 (set to Z0)). In the state before the recess 4 is formed, the additive concentration in the first region from the top surface GT to the first position Z1 is the first concentration C1. The additive concentration in the second region from the first position Z1 to the second position Z2 is the second concentration C2. Similarly, let (N) be a natural number, and the additive concentration in the region from the position Z(N-1) to the position Z(N) is the concentration C(N).

[0048] When (N) regions corresponding to each oxide plate are set along the Z-axis direction of the crucible G, the upper end position of each region is set to Z(N-1) and the lower end position is set to Z(N). When N is an integer greater than 2, the additive concentration C(N) in each region satisfies C(N-1)>C(N).

[0049] According to the crucible G of this embodiment, the following effects can be obtained. In the crystal manufacturing, the crucible G is slowly melted and the melting position is continuously moved. Since the concentration of the additive varies depending on the position of the crucible G, the amount of the additive melted into the molten liquid also changes. Since the concentration distribution of the additive in the crucible G can be freely selected according to the shape of the stack when making the crucible G, the mixing ratio of the additive, etc., the amount of addition can be controlled in a manner to eliminate the uneven distribution in the ingot (single crystal) originally caused by the segregation of the additive, and the concentration of the additive in the ingot can be made uniform.

[0050] Figure 4 2 is a diagram showing a crystal manufacturing apparatus. The crystal manufacturing apparatus includes a support body 12 disposed at a lower portion within an external frame 20. A crucible table 2 is disposed and supported on the support body 12. A crucible G is disposed within the crucible table 2. The inner surface of the crucible table 2 is in contact with the outer peripheral surface of the crucible G. A high-frequency coil 3 is disposed around the crucible G. A recess 4 is provided on the top surface of the crucible G, and the lower end of the seed crystal 7 is in contact with the exposed surface of the molten liquid held in the recess 4. The recess 4 itself or the molten liquid in the recess 4 can be formed by heating with infrared rays IR emitted from an infrared heating source 13.

[0051] The seed crystal 7 is held by a seed crystal holder 10, and the seed crystal holder 10 is fixed to the lower end of a support rod 11. The upper end of the support rod 11 is engaged with a first drive mechanism D1, and the first drive mechanism D1 can move the support rod 11 up and down along the Z axis. The first drive mechanism D1 can also be a structure that rotates the support rod 11 around the Z axis. The first drive mechanism D1 can be driven by a first motor M1.

[0052] The lower end of the high frequency coil 3 is supported by a support mechanism, and the second drive mechanism D2 can engage with the support mechanism to move the support mechanism up and down along the Z axis. The second drive mechanism D2 is driven by a second motor M2.

[0053] Each element of the crystal manufacturing apparatus is controlled by a controller 14. The controller 14 is connected to a driving power supply 15 that supplies power to the first motor M1. The controller 14 is connected to the first motor M1 and outputs a rotation control signal to the first motor M1. The controller 14 is connected to the second motor M2 and outputs a rotation control signal to the second motor M2. The controller 14 is connected to an infrared heating power supply 16, and the power output from the infrared heating power supply 16 is supplied to the infrared heating source 13. The controller 14 is connected to a high frequency (RF) power supply 17, and the power output from the RF power supply 17 is supplied to the high frequency coil 3.

[0054] The crucible G is set in the crucible table 2. The solenoid type high frequency coil 3 is arranged around the crucible table 2. The concave portion 4 in the center of the top surface of the crucible G can hold the molten liquid 6 in the initial stage of heating. In order to generate the molten liquid 6 in the concave portion 4 of the crucible G, the infrared IR emitted from the infrared heating source 13 can be irradiated into the concave portion 4. When the magnetic flux density B (magnetic flux) generated by the high frequency coil 3 passes through the molten liquid and the inner surface of the concave portion 4, induction heating caused by eddy current is generated, and the crucible material is melted.

[0055] The crucible table 2 is a cooling device having the function of cooling the outer wall surface of the crucible G. The crucible table 2 has a flow path for a cooling medium 5 to flow. The cooling medium 5 is circulated by a cooling pump 18. The cooling medium 5 in this example is water. There are various materials as the cooling medium 5. Heavy water, carbon dioxide, helium, metallic sodium, sodium-potassium alloy, mercury, air and other cooling media are also known.

[0056] Figure 5 2 is a diagram showing the structure of the periphery of the crucible G. As described above, the crucible G is accommodated in the crucible table 2 (see Figure 4) inside. As the structure of the crucible table 2, multiple structures are conceivable. The exemplary crucible table shown in the figure is equipped with multiple cooling tubes 2A, 2B, and 2C. Each cooling tube 2A, 2B, and 2C is in the shape of a U-shape, and these cooling tubes 2A, 2B, and 2C are arranged to surround the crucible G. The cooling medium 5 flows in the cooling tubes 2A, 2B, and 2C. Each U-shaped cooling tube 2A, 2B, and 2C is provided with a cooling medium inlet at the lower part, extends upward from the cooling medium inlet, makes a U-shaped turn at the upper end, and bends, and extends downward to the cooling medium discharge port at the lower part. The material of the cooling tubes 2A, 2B, and 2C is preferably a metal with high thermal conductivity, and in this case, is made of copper (Cu). Since the figure shows a cross-sectional structure, although the number of cooling tubes shown in the figure is 3, it is actually more than 3 (for example, 8).

[0057] The cooling tubes 2A, 2B, and 2C are insulated so as not to generate eddy currents induced by the magnetic flux density B (magnetic flux) generated by the coil. The direction of the magnetic flux density B (magnetic flux) generated by the high-frequency coil 3 is set to be approximately perpendicular to the bottom surface of the deepest part in the recess 4 (for example, 80 to 100 degrees). In the case of generating a molten liquid, the direction of the magnetic flux density B (magnetic flux) can also be set to be approximately perpendicular to the exposed surface of the molten liquid (the interface with the seed crystal) (for example, 80 to 100 degrees).

[0058] The cooling tubes 2A, 2B, and 2C are in close contact with the outer peripheral surface of the crucible G. The bottom surface of the crucible G is supported by, for example, stoppers SA, SB, and SC that abut against the bottom surface. The stoppers SA, SB, and SC may be made of a conductor such as copper in addition to an insulator with high heat resistance in the case of cooling, and may be fixed to the cooling tubes 2A, 2B, and 2C.

[0059] In the initial stage of crystal production, infrared heat source 13 (refer to Figure 4 ) is irradiated with infrared rays IR emitted from the inner surface of the recess 4, and the surface of the recess 4 is melted to generate a molten liquid. Even when the crucible G is composed of only a cylindrical oxide body and does not have a recess 4, the initial recess 4 can be formed by irradiating infrared rays IR. By forming the recess 4, the crucible G has a structure that can hold the molten liquid inside the recess 4.

[0060] Figure 6 (A) Figure 6 (B) Figure 6 (C) Figure 6 (D) Figure 6 (E), and Figure 6 (F) is a diagram for explaining the method of producing a crystal. Figure 4 The crystal production apparatus shown is used for crystal production, and unless otherwise specified, the target elements are controlled by instructions from the controller 14 .

[0061] exist Figure 6 In the initial heating stage shown in (A), the infrared heating source 13 (see Figure 4 )(heating device), etc., to locally heat the upper surface of the crucible G to generate a molten liquid 6. A recess 4 may also be provided in advance in the center of the upper surface of the crucible G to stabilize the holding position of the molten liquid 6. The valence (ionic valence) of the metal element (e.g. Ga) constituting the oxide (e.g. Ga2O3) is different from that of the metal element (e.g. Sn) or semiconductor element (e.g. Si) constituting the additive. The mixture constituting the crucible G exhibits conductivity in the molten liquid state. When a high-frequency magnetic field (magnetic flux density B) is applied thereto by a high-frequency coil 3, the conductive melt is inductively heated to generate Joule heat. The melting of the crucible G is performed by increasing the amount of electricity applied to the high-frequency coil 3.

[0062] like Figure 6 As shown in (B), after the molten liquid 6 is generated in the recessed portion 4 on the upper surface of the crucible G, the seed crystal 7 is lowered from above so that the lower end of the seed crystal 7 contacts the liquid surface of the molten liquid 6, and the amount of electricity applied to the high-frequency coil 3 is adjusted in such a way that the molten liquid 6 and the seed crystal 7 coexist, and the temperature is waited to be stabilized.

[0063] like Figure 6 As shown in (C), after the temperature is stabilized, the seed crystal 7 is slowly moved upward, thereby precipitating a growth crystal 8 at the lower end of the seed crystal 7. The seed crystal 7 can be driven by the first motor M1. Figure 4 The first motor M1 is moved by the first driving mechanism D1 shown, and the moving speed and the moving amount can be controlled by a control signal output from the controller 14 to the first motor M1.

[0064] like Figure 6 (D)~ Figure 6 As shown in (F), when the high-frequency coil 3 is slowly moved downward while adjusting the amount of the molten liquid 6 required for crystal growth, the growing crystal 8 gradually becomes larger. The high-frequency coil 3 can be driven by the second motor M2. Figure 4 The high frequency coil 3 is moved by the second driving mechanism D2 shown in the figure, and the moving speed and the moving amount can be controlled by the control signal output from the controller 14 to the second motor M2. Furthermore, if the relative position of the high frequency coil 3 to the crucible G gradually moves downward, the position of the molten liquid 6 held in the crucible G is also lowered as shown in these figures.

[0065] When the concentration of the additive in the Z-axis direction in the crucible G is different, the amount of the additive supplied from the crucible G also changes according to the position of the melt 6. When the amount of the additive supplied from the crucible G to the melt 6 is constant, the amount of the additive entering the growing crystal 8 (single crystal of the ingot) changes. That is, if the effective segregation coefficient k of the additive relative to the material of the growing crystal 8 (in other words, the material of the main body of the crucible G) is eff If the effective segregation coefficient k is less than 1, the concentration of the additive in the growing crystal 8 is low at the beginning of growth due to segregation, and the concentration of the additive increases as the growth progresses. eff When the ratio is less than 1, only a part of the additive contained in the melt 6 enters the growing crystal 8, so the additive that has not entered remains in the melt 6, and the concentration of the additive in the melt 6 increases with the growth. If the concentration of the additive in the melt 6 increases, the concentration of the additive in the growing crystal 8 increases in the late stage of growth.

[0066] In contrast, if Figure 3 By predisposing the additive concentration in the crucible G to be higher at the top and lower at the bottom as shown in the additive concentration distribution, the amount of additive supplied from the crucible G decreases as crystal growth proceeds, thereby suppressing segregation of the additive.

[0067] (Example 1)

[0068] First, Example 1 is described. Using the above-mentioned crystal manufacturing method, a crystal ingot (single crystal) is manufactured. First, 4N purity gallium oxide (Ga2O3) powder is weighed and added to 4N purity tin oxide (SnO2) powder, and mixed using a ball mill. The mixed powder is filled into rubber and shaped into a disc. Then, a cold isostatic pressing (CIP) device is used to make an oxide plate (sample) with a diameter of about 100 mm and a thickness of about 10 mm. The pressure during pressurization is about 1000 kg / cm 2 (98MPa). The amount of tin oxide added to the 10 oxide plates is different. Each oxide plate is pre-sintered at about 1300°C. Regarding the 10 oxide plates G1 to G10, the ratio of the mass of the additive (tin oxide) to the mass of the main raw material gallium oxide is G1: 0.71%, G2: 0.66%, G3: 0.60%, G4: 0.54%, G5: 0.48%, G6: 0.42%, G7: 0.34%, G8: 0.27%, G9: 0.18%, G10: 0.08%.

[0069] The deposited oxide plates were heated at about 1700°C for 20 hours in an electric furnace at 1 atmosphere pressure, and sintered to integrate them. In this example, a crucible without a concave portion was produced. The gallium oxide constituting the crucible was polycrystalline.

[0070] During the growth of the single crystal, the pulling speed V of the seed crystal is UP is 5 (mm / h), the descending speed V of the high frequency coil 3 DOWN is 2 (mm / h). In addition, the rotation speed V of the seed crystal around the Z axis ROT As a preferred example, the manufacturing method of this example includes: arranging the high-frequency coil 3 around the crucible G composed of a fusible metal oxide by induction heating from the high-frequency coil 3, supplying high-frequency power to the high-frequency coil 3, melting the concave portion provided on the upper surface of the crucible G, making the seed crystal contact with the exposed surface of the molten liquid in the concave portion of the crucible G, and pulling at a pulling speed V UP Pull the seed crystal while descending at a speed V DOWN The process of lowering the high frequency coil 3 to grow the oxide single crystal is set to V UP >V DOWN , thereby making it possible to produce high-quality oxide single crystals, especially gallium oxide single crystals.

[0071] (Comparative Example 1)

[0072] In Comparative Example 1, the concentration of tin oxide (SnO2) in all oxide plates was made the same. For oxide plates G1 to G10, the ratio of the mass of the additive (tin oxide) to the mass of gallium oxide of the main raw material was 0.43%. The concentration of tin oxide in Comparative Example 1 was set to the average value of the concentration of tin oxide in Example 1. Comparative Example 1 was the same as Example 1 except for this aspect, and a crucible without a concave portion was manufactured. The gallium oxide constituting the crucible was polycrystalline.

[0073] Figure 7 It is a graph showing the relationship between the position Z in the crucible G and the concentration C (Sn) of Sn. The figure shows the distribution of additive concentrations in the integrated crucible G before sintering, and the additive distribution after sintering also has the same general shape of distribution. In addition, the concentration distribution of the additive (SnO2) is the same as the concentration distribution of the additive (Sn) as a specific element contained therein. For N (N=10) oxide plates, the numbers N=1, 2, 3...10 are marked from top to bottom, and the position of the lower surface of each oxide plate is ZN. Since the thickness of each oxide plate is 10 mm, Z1=10 mm, Z(N)-Z(N-1)=10 mm (N is an integer greater than 2). In this graph, the concentration C (Sn) is expressed in arbitrary units obtained by standardization with an average value.

[0074] The values ​​of the data of Example 1 in this graph are as follows.

[0075] (Z1, C1) = (10 mm, 1.676)

[0076] (Z2, C2) = (20 mm, 1.537)

[0077] (Z3, C3) = (30 mm, 1.397)

[0078] (Z4, C4) = (40 mm, 1.257)

[0079] (Z5, C5) = (50 mm, 1.117)

[0080] (Z6, C6) = (60 mm, 0.978)

[0081] (Z7, C7) = (70 mm, 0.791)

[0082] (Z8, C8) = (80 mm, 0.628)

[0083] (Z9, C9) = (90 mm, 0.428)

[0084] (Z10, C10) = (100 mm, 0.186)

[0085] In addition, the value of the concentration C(Sn) in Comparative Example 1 is constant regardless of the position Z, and the average concentration value CS=1.

[0086] Figure 8 This is a stereoscopic view of a growing crystal (single crystal) composed of an ingot. In the initial state of growth, the position of the initial interface 8T with the seed crystal is Z=0, and as the growth time passes, the crystal extends in the positive direction of the Z axis. Although the figure schematically shows that the diameter of the ingot is fixed in the Z-axis direction, in fact, the diameter of the upper part depends on the diameter of the seed crystal. The manufactured ingot is cut along a plane (XY plane) orthogonal to the Z-axis direction, divided into 12 equal parts, and a flat sample is manufactured, and the concentration C (Sn) of Sn on the upper surface of the flat sample is measured. A multi-wire saw can be used for cutting. The concentration of additives is measured by luminescence analysis using the Laser Ablation Inductively Coupled Plasma Mass Spectrometry (LA-ICP-MS) method. In the case of a mixed powder, about 1 g of powder sampled before press molding is measured. In the case of a single crystal, measurements are made at one position in the center of the above-mentioned flat sample and at four positions near the periphery, and the average value is set as a representative value.

[0087] (Evaluation of Additive Concentration Distribution)

[0088] Fig. 9It is a graph showing the relationship between the position Z in the grown single crystal and the concentration C (Sn) of Sn. In this graph, the concentration C (Sn) is expressed in an arbitrary unit obtained by normalizing with an average value. The concentration C (Sn) in Example 1 is approximately constant along the Z-axis direction. When the average value is set to 100%, the maximum value of the additive concentration is 104% and the minimum value is 97.5%. Even if an error of about 1% from the maximum value of 104% is allowed, the concentration of the additive along the growth axis (Z-axis) is within the range of ±5% of the average value of the concentration of the additive, and the deviation is small. The concentration C (Sn) in Comparative Example 1 increases along the positive direction of the Z-axis.

[0089] In this graph, the position Z is an arbitrary constant representing the position Z when the diameter of the ingot is assumed to be constant. In fact, the position Z represents the solidification rate (the ratio of the mass of all raw materials (or the mass of the entire crucible) to the mass of the resulting single crystal when growing a single crystal from a melt).

[0090] The data of position Z (curing rate) and concentration C in Example 1 are: (Z, C) = (0, 1), (0.045, 1.04), (0.093, 0.995), (0.15, 1.005), (0.2, 0.985), (0.25, 0.99), (0.3, 0.98), (0.35, 0.975), (0.4, 0.985), (0.44, 0.99), (0.48, 1.01), (0.52, 1.005).

[0091] The data of position Z (curing rate) and concentration C in Comparative Example 1 are: (Z, C) = (0, 0.27), (0.04, 0.278), (0.09, 0.289), (0.14, 0.301), (0.21, 0.320), (0.26, 0.336), (0.31, 0.354), (0.36, 0.373), (0.41, 0.396), (0.45, 0.417), (0.49, 0.441), (0.53, 0.468).

[0092] (Example 2)

[0093] Next, Example 2 is described. In Example 2, a powder of silicon dioxide (SiO2) (silicon oxide) with a purity of 4N is used as an additive instead of the powder of tin oxide (SnO2) in Example 1. For the 10 oxide plates G1 to G10, the ratio of the mass of the additive (silicon dioxide) to the mass of the main raw material gallium oxide is G1: 0.27%, G2: 0.25%, G3: 0.23%, G4: 0.21%, G5: 0.19%, G6: 0.17%, G7: 0.14%, G8: 0.11%, G9: 0.08%, G10: 0.03%. Example 2 is the same as Example 1 except for this aspect, and a crucible without a concave portion is manufactured. The gallium oxide constituting the crucible is polycrystalline.

[0094] (Comparative Example 2)

[0095] In Comparative Example 2, the concentration of silicon dioxide (SiO2) in all oxide plates is made the same. For oxide plates G1 to G10, the ratio of the mass of the additive (silicon dioxide) to the mass of the gallium oxide of the main raw material is 0.17%. The concentration of silicon dioxide in Comparative Example 2 is set to the average value of the concentration of silicon dioxide in Example 2. Comparative Example 2 is the same as Example 2 except for this aspect, and a crucible without a concave portion is manufactured. The additive concentration distribution can be measured by the same method as Example 1 and Comparative Example 1. The gallium oxide constituting the crucible is polycrystalline.

[0096] Fig.10 It is a graph showing the relationship between the position Z in the crucible G and the concentration C(Si) of Si. The figure shows the distribution of additive concentration in the integrated crucible G before sintering, and the distribution of additive concentration after sintering also has the same general shape of distribution. In addition, the concentration distribution of the additive (SiO2) is the same as the concentration distribution of the additive (Si) as the specific element contained therein. For N (N=10) oxide plates, the numbers N=1, 2, 3...10 are marked from top to bottom, and the position of the lower surface of each oxide plate is ZN. Since the thickness of each oxide plate is 10 mm, Z1=10 mm, Z(N)-Z(N-1)=10 mm (N is an integer greater than 2). In this graph, the concentration C(Sn) is expressed in an arbitrary unit obtained by standardization with an average value.

[0097] The values ​​of the data of Example 2 in this graph are as follows.

[0098] (Z1, C1) = (10 mm, 1.597)

[0099] (Z2, C2) = (20 mm, 1.487)

[0100] (Z3, C3) = (30 mm, 1.371)

[0101] (Z4, C4) = (40 mm, 1.250)

[0102] (Z5, C5) = (50 mm, 1.122)

[0103] (Z6, C6) = (60 mm, 0.983)

[0104] (Z7, C7) = (70 mm, 0.833)

[0105] (Z8, C8) = (80 mm, 0.671)

[0106] (Z9, C9) = (90 mm, 0.480)

[0107] (Z10, C10) = (100 mm, 0.202)

[0108] Furthermore, the value of the concentration C(Si) in Comparative Example 2 is constant regardless of the position Z, and the average concentration value CS=1.

[0109] In Example 2 and Comparative Example 2, as in Example 1 and Comparative Example 1, the manufactured ingot is cut along a plane (XY plane) orthogonal to the Z-axis direction into 12 equal parts to manufacture flat plate samples, and the Si concentration C(Si) on the upper surface of the flat plate sample is measured in the same manner as in Example 1.

[0110] (Evaluation of Additive Concentration Distribution)

[0111] Fig.11 It is a graph showing the relationship between the position Z in a single crystal and the concentration C(Si) of Si. In this graph, the concentration C(Si) is expressed in an arbitrary unit obtained by normalizing with an average value. The concentration C(Si) in Example 2 is approximately constant along the Z-axis direction. When the average value is set to 100%, the maximum value of the additive concentration is 101% and the minimum value is 97%. Even if an error of about 1% from the minimum value of 97% is allowed, the concentration of the additive along the growth axis (Z-axis) direction is within the range of ±4% of the average value of the concentration of the additive. The concentration of the additive along the growth axis (Z-axis) direction is at least within the range of ±5% of the average value of the concentration of the additive, so that the deviation is suppressed. The concentration C(Si) in Comparative Example 2 increases along the positive direction of the Z-axis.

[0112] In addition, in this graph, the position Z is an arbitrary constant indicating the position Z when the diameter of the ingot is assumed to be constant. In fact, the position Z indicates the solidification rate.

[0113] The data of position Z (curing rate) and concentration C in Example 2 are: (Z, C) = (0, 1), (0.03, 0.985), (0.07, 1.01), (0.12, 1.01), (0.18, 0.97), (0.23, 1.01), (0.28, 1.01), (0.33, 1), (0.38, 0.99), (0.42, 1.01), (0.46, 0.99), (0.5, 0.99).

[0114] The data of position Z (curing rate) and concentration C in Comparative Example 1 are: (Z, C) = (0, 0.35), (0.04, 0.359), (0.08, 0.369), (0.13, 0.38), (0.19, 0.401), (0.24, 0.418), (0.29, 0.43), (0.34, 0.458), (0.4, 0.487), (0.44, 0.510), (0.47, 0.528), (0.51, 0.556).

[0115] As described above, the crucible is a crucible for growing an oxide single crystal, and includes a main body, the main body includes an oxide containing an additive, and in the oxide of the main body, a plurality of regions arranged along a single axis are set, and among the plurality of regions, the concentration of the additive in the first region is higher than the concentration of the additive in the second region. When this crucible is used, an oxide single crystal having a uniform additive concentration distribution along a single axis (Z axis) direction can be manufactured.

[0116] The structure of the present invention can be varied in many ways. In addition, the elements disclosed in the embodiments can be omitted, replaced, and / or changed as needed. For example, the number of oxide plates used to make the crucible can be changed to two.

[0117] Fig.12: is a graph showing the relationship between the position Z in the crucible and the concentration C of the additive. In the crucible, two regions are set along the Z-axis direction, and the additive concentration of the first region on the surface side is set higher. The first concentration C1 of the additive in the first region from position 0 to the first position Z1 is higher than the second concentration C2 of the additive in the second region from the first position Z1 to the second position Z2. The number of regions set in the crucible can be 2 or more as described above. That is, in Example 1, Example 2, etc., the number of multiple regions set in the crucible is 3 or more, and the concentration of the additive in each region decreases as it moves away from the first region along a single axis (=Z axis). The more the number of multiple regions set in the crucible, the more precisely the additive concentration distribution can be controlled, and therefore, the number is preferably 3 or more, and more preferably N or more (N=4, 5, 6, 7, 8, 9, 10). From the perspective of manufacturing cost, the preferred upper limit of the number (N) can be set to 50 or less, for example.

[0118] In the case where the crucible is a crucible for growing a gallium oxide single crystal, the crucible includes a main body, the main body includes gallium oxide containing an additive, and in the gallium oxide of the main body, a plurality of regions arranged along a single axis are set, and the concentration of the additive in the first region among the plurality of regions is higher than the concentration of the additive in the second region. When the crucible is used, a gallium oxide single crystal having a uniform additive concentration distribution along a single axis (Z axis) direction can be manufactured. In the crucible, the additive includes at least one selected from SnO2 and SiO2. When these additives are incorporated into the single crystal as metal elements or semiconductor elements, they can act as N-type impurities in the ingot of the single crystal.

[0119] Regardless of the material of the oxide, in order to make the additive function as an N-type, in the above crucible, the valence (ionized: quadruple) of the metal element or semiconductor element (e.g., Sn or Si) constituting the additive is set to be greater than the valence (Ga: trivalent) of the metal element constituting the oxide (e.g., Ga2O3) contained in the main body of the crucible. Regarding the above crucible, in a preferred example, each oxide plate contains gallium oxide, and the additive contains at least one selected from SnO2 and SiO2. Consider the case of containing only SnO2, the case of containing only SiO2, and the case of containing both SnO2 and SiO2.

[0120] In addition, illustratively, Figure 1 to Figure 3 As shown, the crucible is a crucible for growing an oxide single crystal, and has a plurality of oxide plates G1 to G2 stacked and joined in the thickness direction (Z-axis direction), and the concentration of the additive in each oxide plate is different. Due to the different concentrations, it can be freely designed and a single crystal with high additive uniformity can be obtained.

[0121] Fig.13: This is a graph showing the relationship between the position Z in the crucible and the additive concentration C. In the crucible, two or more continuous regions are set along the Z-axis direction, and the additive concentration in the first region on the surface side is set higher. The first concentration C1 of the additive in the first region from position 0 to an appropriate position on the surface side is higher than the second concentration C2 of the additive in the second region from this position to a deeper position. The maximum concentration C on the top surface of the crucible is max As the position Z increases, it decreases. At the position Z of the bottom of the crucible, max The concentration C at which the minimum min Even in the case of such a concentration distribution, the above-mentioned effects can be exerted.

[0122] The above-mentioned crystal manufacturing method includes: using the above-mentioned crucible, while making the seed crystal contact with the exposed surface of the molten liquid in the crucible, while moving the position of the exposed surface in the vertical direction, thereby growing the oxide single crystal. When using the above-mentioned crucible, a single crystal having a uniform additive concentration distribution along the Z-axis direction can be manufactured.

[0123] The grown single crystal is produced by the above-mentioned crystal production method. It should be noted that even if the numerical values ​​of this embodiment include an error of at least ±20%, the same effect is achieved.

[0124] Such a single crystal is a single crystal of gallium oxide composed of an ingot to which Sn or Si is added as an additive, and the concentration of the additive along the growth axis direction (Z-axis direction) is within the range of ±5% of the average value of the concentration of the additive. The average value is the average value of the concentration of the additive distributed throughout the ingot. In the above, the ingot is cut in a direction perpendicular to the growth axis to form a plurality of flat samples, and the concentration of the additive is measured at one position in the center of the flat sample and at four positions near the periphery, and the average value of the data at these five points is set as the concentration of the additive in one flat sample. The average value of the concentration of the additive in the ingot can be obtained by adding the concentrations of the additives of N flat samples and dividing the added value by N.

[0125] Fig.14 It is the curing rate g and C g The graph shows the relationship between the normalized concentration C and the concentration C when a fixed amount of molten liquid is prepared and the molten liquid is gradually solidified. g / C0. Concentration C g represents the concentration of the additive in the crystal (ingot solid), and C0 represents the initial concentration in the melt. In the range of solidification rate g from 0 to 1, if the concentration of the additive C g Taking the definite integral, its value is C0. Furthermore, C g =C0×k eff ×(1-g) keff-1 .

[0126] As in Comparative Examples 1 and 2, when the concentration of the additive in the crucible is constant and the effective segregation coefficient k is eff = 0.3, there is not too much additive in the grown ingot crystal, and the additive concentration in the melt gradually increases with the consumption of the melt (the solidification rate g of the ingot is proportional to the position Z in the crucible). Similarly, the solid additive concentration C g When a limited amount of melt is prepared in advance, the additives not incorporated into the ingot solid are concentrated in the late growth stage. By setting the additive in the crucible before sintering to the effective segregation coefficient k eff A concentration distribution that is proportional to the inverse of the segregation distribution can offset the segregation as shown in this graph.

[0127] In the above crucible, when the oxide is gallium oxide, the effective segregation coefficient k of the additive relative to the oxide material contained in the main body is eff When it is less than 1, the first region is located on the side that is melted in the early stage of growth of the single crystal.

[0128] The following is the effective segregation coefficient k eff Supplementary explanation. When the valence or size (ionic radius) of the element constituting the crystal is different from that of the element of the additive, the ease of incorporation into the crystal when solidified from the melt is different. The ratio of the concentration of the additive in the crystal of the growing object to the concentration of the additive in the melt is set as the segregation coefficient k. The segregation coefficient k usually represents a value different from 1. Since the segregation coefficient k represents a value in the equilibrium state, the segregation coefficient k when the crystal growth is actually carried out dynamically is taken as the effective segregation coefficient k eff In single crystal growth, only a portion of the additives are often incorporated, so in this case the effective segregation coefficient k eff <1.

[0129] In k eff When the ratio is less than 1, the concentration of additives in the growing crystal is lower than that in the melt, and the additives not incorporated into the crystal remain in the melt. During the crystal growth process, the additives in the melt are concentrated, and the concentration of additives in the crystal gradually increases. The concentration of additives in the position where the crystal is precipitated is low in the early stage of crystallization, and the concentration of additives in the position where the crystal is precipitated is high in the later stage of crystallization, thus forming an uneven concentration distribution.

[0130] In 1<k eff In the case of , the opposite phenomenon occurs, forming a concentration distribution in which the concentration of the additive is higher at the location where the additive is precipitated in the early stage of crystallization, and the concentration of the additive is lower at the location where the additive is precipitated in the late stage of crystallization.

[0131] The crucible is used to produce oxide single crystals, is composed of raw materials for oxide single crystals, is a container for holding oxide melt, and contains additives to be added to the single crystals. By using this crucible, the amount of additives added during crystal growth can be controlled without setting up a complicated additive supply mechanism. In the crucible, the concentration of the additive varies depending on the location of the crucible, and the effective segregation coefficient k of the additive relative to the single crystal is controlled. eff When the effective segregation coefficient k is less than 1, the concentration of the additive in the crucible melted at the early growth stage is higher than that in the crucible melted at the late growth stage. eff When it exceeds 1, the concentration of the additive in the crucible portion melted in the early growth stage becomes lower than the concentration of the additive in the crucible portion melted in the late growth stage. The crucible for growing an oxide single crystal and the method for producing the crucible according to the present embodiment can produce a single crystal in which segregation of additives is suppressed.

[0132] Effective segregation coefficient k eff It depends on the material of the ingot (single crystal) and the material of the additive. Since the material of the ingot is the same as that of the crucible, the effective segregation coefficient k eff It depends on the relationship between the material of the crucible and the material of the additive. The crucible is made of oxide. In the above embodiment, the oxide is a metal oxide, specifically Ga2O3, and its sintered body is polycrystalline. When the additive is Sn or Si, the effective segregation coefficient k eff <1, for example 0.3.

[0133] As the effective segregation coefficient k eff >1 oxide and additive material combination, such as Y3Al5O 12 and Cr (or Cr2O3). In this case, the distribution of the additive in the crucible along the Z-axis direction is opposite to the above distribution. The crucible has a main body including an oxide containing an additive, and in the oxide of the main body, a plurality of regions arranged along a single axis are set, and in the plurality of regions, the concentration of the additive in the first region is higher than the concentration of the additive in the second region, and the second region is located above the first region. In other words, the effective segregation coefficient k of the material of the additive relative to the oxide contained in the main body is eff When it is larger than 1, the second region is located on the side that is melted in the early stage of growth of the single crystal.

[0134] As described above, according to the above-mentioned crucible and manufacturing method, a single crystal with a high uniformity of additive concentration along the growth axis direction can also be obtained. In particular, when Ga2O3 is used as the metal oxide constituting the ingot, it is more important to control the concentration of the additive that controls the electrical behavior from the perspective of application to electronic devices. That is, among oxides, some materials are thermodynamically unstable at high temperatures, and when heated at a temperature near the melting point in an atmosphere with an oxygen concentration of several percent or less, oxygen defects will be generated. The oxygen defects inside the crystal serve as color centers of optical materials, causing a decrease in transmittance, or affecting the activation of dopants in semiconductor materials.

[0135] When using a crucible made of indium, which is a precious metal, although it is a metal that is relatively difficult to oxidize, it will oxidize at more than 1100°C in an atmosphere with an oxygen concentration of about 20% to generate oxides (IrO2, etc.). When using an iridium crucible during crystal growth, in order to suppress the oxidation of iridium, the oxygen concentration needs to be suppressed to less than a few%. On the other hand, when β-Ga2O3, which has attracted much attention as a wide bandgap semiconductor, grows crystals at a low oxygen concentration, a high density of oxygen defects will be generated in the growing β-Ga2O3 crystals. Since oxygen defects act as N-type impurities and generate high concentrations of donors, it is difficult to precisely control the donor concentration. When using the crucible of the embodiment instead of the iridium crucible, the crucible has the advantage of not requiring oxidation suppression because it is composed of oxides. In addition, regardless of the size of the oxygen partial pressure, it is desirable to control additives other than oxygen.

[0136] In the case of using a metal or semiconductor additive such as Sn or Si, if the above crucible and manufacturing method are used, the uniformity of the additive concentration will be increased, which is useful. According to the above method, since the crucible material is an oxide, the additive concentration can be accurately controlled. Since the crucible material is the same as the single crystal material, it is also possible to suppress the mixing of unnecessary impurities into the single crystal.

[0137] In order to obtain material properties corresponding to the application, additives are added to the oxide single crystal. According to the above method, when the single crystal is divided into multiple parts to form components, the additives are evenly distributed in the crystal, so the characteristics of the components can be made consistent. Furthermore, the manufactured single crystal can be used for components that utilize physical properties in addition to electrical components.

[0138] Explanation of symbols

[0139] G…crucible, G1~G10…oxide plates, GT…top surface, 2…crucible table, 2A…cooling tube, 3…high-frequency coil, 4…recess, 5…cooling medium, 6…molten liquid, 7…seed, 8…growing crystal, 10…seed holder, 11…support rod, 12…support body, 13…infrared heating source, 14…controller, 15…driving power supply, 16…power supply for infrared heating, 17…RF power supply, 20…external frame, D1…first driving mechanism, D2…second driving mechanism, IR…infrared, M1…first motor, M2…second motor, SA, SB, SC…stoppers.

Claims

1. A crucible, It is characterized in that The crucible is used for growing oxide single crystals. A main body is provided, wherein the main body comprises an oxide containing an additive, In the oxide of the main body, a plurality of regions arranged along a single axis are set, and among the plurality of regions, a concentration of the additive in a first region is higher than a concentration of the additive in a second region.

2. A crucible, It is characterized in that The crucible is used for growing gallium oxide single crystals. A main body is provided, wherein the main body comprises gallium oxide containing an additive, In the gallium oxide of the main body, a plurality of regions arranged along a single axis are set, and among the plurality of regions, a concentration of the additive in a first region is higher than a concentration of the additive in a second region.

3. The crucible according to claim 1 or 2, It is characterized in that The effective segregation coefficient k of the additive relative to the oxide material contained in the main body eff Less than 1, The first region is located on the side that is melted in the early stage of growth of the single crystal.

4. The crucible according to claim 1 or 2, It is characterized in that The number of the plurality of regions is 3 or more, and the concentration of the additive in each region decreases as it moves away from the first region along the single axis.

5. The crucible according to claim 1 or 2, It is characterized in that The valence of the metal or semiconductor element constituting the additive is greater than the valence of the metal element constituting the oxide contained in the host.

6. The crucible according to claim 2, It is characterized in that The additive comprises a SnO 2 and SiO 2 At least one of .

7. A crucible, It is characterized in that The crucible is used for growing oxide single crystals. A plurality of oxide plates are stacked and bonded in a thickness direction, The concentration of the additive in each of the oxide plates is different.

8. The crucible according to claim 7, It is characterized in that Each of the oxide plates comprises gallium oxide, The additive comprises a SnO 2 and SiO 2 At least one of .

9. A method for producing a crystal, It is characterized in that The crucible according to claim 1, 2 or 7 is used, and the step of growing the oxide single crystal is included, by moving the position of the exposed surface in the vertical direction while bringing a seed crystal into contact with the exposed surface of the melt in the crucible.

10. A single crystal, It is characterized in that The crystal is obtained by the method for producing a crystal according to claim 9.

11. A single crystal, It is characterized in that The single crystal is a gallium oxide single crystal composed of an ingot to which Sn or Si is added as an additive, and the concentration of the additive along the growth axis direction is within the range of ±5% of the average value of the concentration of the additive.